Solid electrolyte, battery and preparation method thereof

By using a solid electrolyte that combines fluoropolymers and ion plastic crystals in lithium secondary batteries, the safety hazards and conductivity issues of traditional liquid electrolytes are solved, and the fast charging and long cycle performance of lithium secondary batteries are achieved.

CN118738541AActive Publication Date: 2024-10-01SHANGHAI JIAOTONG UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410915984.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Traditional organic liquid electrolytes in existing lithium secondary batteries have safety hazards such as being flammable, volatile, and easy to leak, and it is difficult to achieve high room temperature ionic conductivity and long cycle performance.

Method used

Using fluoropolymer as the matrix, introducing ion plastic crystals and lithium salts, and adjusting the component structure and proportions, a fluoropolymer/plastic crystal solid electrolyte with high room temperature ionic conductivity is prepared to achieve fast charging and charging of lithium secondary batteries. Long loop.

Benefits of technology

It achieves high room temperature ion conductivity and long cycle performance of lithium secondary batteries, improves the safety and energy density of the battery, and has fast charge and discharge capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738541A_ABST
    Figure CN118738541A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, in particular to a solid electrolyte, a battery and a preparation method thereof. The fluoropolymer (including a compound of various fluoropolymers) is used as a matrix, the ionic plastic crystal and the lithium salt are introduced, and the fluoropolymer / plastic crystal solid electrolyte is prepared by regulating and controlling the component structure and optimizing the component proportion. According to the invention, the solid electrolyte prepared by the method has high room-temperature ionic conductivity, and can realize fast charge and long cycle of the lithium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to a solid electrolyte, a battery and a preparation method thereof. Background Art

[0002] With the increase in the energy density of lithium secondary batteries, the safety hazards brought by traditional organic liquid electrolytes, such as flammability, volatility, and leakage, have become increasingly prominent. Compared with liquid electrolytes, solid electrolytes have high safety, wide electrochemical window, wide operating temperature range, and certain flexibility and high mechanical strength. They can effectively inhibit the piercing of lithium dendrites during battery cycling, making it possible to use metallic lithium with high theoretical specific capacity (3860mAh / g) and the lowest negative potential (-3.04V compared to the standard hydrogen electrode) as the negative electrode, which has attracted great attention from academia and industry.

[0003] Polymer electrolytes are mainly composed of polymer matrix and lithium salt. They have attracted wide attention due to their light weight, good mechanical flexibility, controllable size, excellent processing performance and other characteristics. Among them, polymer electrolytes with fluorinated polymers as the matrix have been developed. However, how to provide a solid electrolyte with high room temperature ionic conductivity and capable of fast charging and long cycle of lithium secondary batteries is still a constant exploration for those skilled in the art. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a solid electrolyte, a battery and a method for preparing the same. The present invention uses a fluoropolymer (including a composite of multiple fluoropolymers) as a matrix, introduces ionic plastic crystals and lithium salts, and prepares a fluoropolymer / plastic crystal solid electrolyte by regulating the component structure and optimizing the proportion of each component. The solid electrolyte has high room temperature ionic conductivity and first realizes fast charging and long cycle of lithium secondary batteries.

[0005] In the present invention, fluorine-containing polymers mainly refer to polymers formed by replacing all or part of the hydrogen atoms directly covalently bonded to carbon atoms in the main chain and side chain of organic polymer compounds with fluorine atoms, and have excellent properties such as outstanding chemical resistance, climate stability, low surface energy and low friction coefficient.

[0006] For polymer electrolytes, in order to take into account both mechanical properties and ion conductivity, technicians in this field are committed to exploring solid materials with high ion conductivity. Plastic crystals belong to the category of solid crystal materials. Due to the translational or rotational movement of their molecules / ions, the orientation is disordered and there are lattice vacancies. They exhibit solid-solid phase transition behavior before melting transition. The crystals show plastic characteristics between the solid-solid phase transition temperature and the melting point.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The first object of the present invention is to provide a solid electrolyte, which is obtained by using a fluoropolymer as a matrix and introducing ionic plastic crystals and lithium salts;

[0009] The mass ratio of the fluoropolymer, the ionic plastic crystal and the lithium salt is 20:4-100:1-40.

[0010] In one embodiment of the present invention, the fluoropolymer is selected from one or more of the compounds represented by the following structural formulas:

[0011]

[0012] Wherein, in formula (1) to formula (6), the molecular weight of the polymer is 100,000 to 600,000; and x, y, n and m in each structural formula are independently positive integers.

[0013] In one embodiment of the present invention, the ionic plastic crystals are one or more selected from pyrrole ionic plastic crystals, piperidine ionic plastic crystals or morpholine ionic plastic crystals.

[0014] In one embodiment of the present invention, the structural formula of the pyrrole ionic plastic crystal is shown in formula (7), the structural formula of the piperidine ionic plastic crystal is shown in formula (8), and the structural formula of the morpholine ionic plastic crystal is shown in formula (9);

[0015]

[0016] Among them, in formula (7), formula (8) and formula (9), R1 is independently selected from -CH3 or -CH2CH3, and R2 is independently selected from -CH3, -CH2CH3 or -CH2CH2CH3.

[0017] In one embodiment of the present invention, the lithium salt is selected from one or more of lithium chloride, lithium sulfate, lithium carbonate, lithium acetate, lithium cobaltate, lithium nitrate or lithium phosphate.

[0018] A second object of the present invention is to provide a method for preparing a solid electrolyte, comprising the following steps:

[0019] The fluoropolymer, lithium salt and ionic plastic crystals are dissolved and mixed, then poured into a mold, and subjected to solvent removal and drying treatment to obtain a solid electrolyte.

[0020] In one embodiment of the present invention, during the mixing process, the temperature is 25 to 80°C;

[0021] The solvent removal process is carried out under an inert atmosphere and at room temperature;

[0022] The drying process specifically includes vacuum drying and argon drying;

[0023] During the vacuum drying process, the temperature is 25-80°C and the time is 8-48h;

[0024] During the argon drying process, the temperature is room temperature and the time is 8 to 48 hours.

[0025] A third object of the present invention is to provide a battery comprising the above-mentioned solid electrolyte.

[0026] The fourth object of the present invention is to provide a method for preparing a battery, wherein the positive electrode sheet, the electrolyte membrane prepared by the above-mentioned solid electrolyte, and the negative electrode sheet are stacked in order from bottom to top to form a laminate, and then a battery is obtained by stamping.

[0027] In one embodiment of the present invention, the positive electrode sheet is a positive electrode sheet using lithium iron phosphate / lithium cobalt oxide / lithium nickel cobalt manganese oxide as the positive electrode material;

[0028] Among them, the structural formula of lithium nickel cobalt manganese oxide is LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2 or LiNi 0.5 Co 0.3 Mn 0.2 One of O2;

[0029] The negative electrode sheet is a negative electrode sheet using lithium as the negative electrode material.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] In the present invention, there are "holes" in the lattice of the ionic plastic crystal that move with the rotation of molecules or ions, so that the plastic crystal has a higher lithium ion conductivity. In addition, the plastic crystal presents a molecularly ordered crystalline state at low temperatures, and there are one or more solid-solid phase transition temperatures before the melting point. The crystal exhibits plastic characteristics between the solid-solid phase transition temperature and the melting point, and the ions are rapidly transferred in the plastic crystal phase of the plastic crystal. Based on this, the most basic requirement for the plastic crystal is that it is in the plastic crystal phase within the operating temperature range of the battery, that is, the plastic crystal is required to have both a low solid-solid phase transition temperature and a high melting point. The solid electrolyte prepared using the above-mentioned ionic plastic crystal has the advantages of high room temperature ionic conductivity, and can achieve fast charging and long circulation of lithium secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Ion plastic crystal PP 12 DSC curve of FSI;

[0033] Figure 2 The cycle performance of the Li / LiFePO4 battery containing solid electrolyte prepared in Example 1 at 5C and 25°C;

[0034] Figure 3 The cycle performance of the Li / LiFePO4 battery containing solid electrolyte prepared in Example 2 at 5C and 25°C;

[0035] Figure 4 This is a schematic diagram of the solid electrolyte membrane prepared in Example 3;

[0036] Figure 5 The temperature dependence of the ionic conductivity of the solid electrolyte prepared in Example 3;

[0037] Figure 6 is the LSV curve of the solid electrolyte prepared in Example 3;

[0038] Figure 7 The cycle performance of the Li / LiFePO4 battery containing solid electrolyte prepared in Example 3 at 5C and 25°C;

[0039] Figure 8 The cycling performance of the Li / LiFePO4 battery containing solid electrolyte prepared in Example 3 at 6C and 25°C. DETAILED DESCRIPTION

[0040] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all monitoring means and methods used are conventional detection means and methods in the art.

[0042] Ionic plastic crystal NMR characterization method: AVANCE III HD 500 nuclear magnetic resonance spectrometer was used, deuterated dimethyl sulfoxide (DMSO-d6) was used as the deuterated reagent, a small amount of the sample to be tested was fully dissolved in the deuterated reagent, and then added dropwise to the analysis tube, which was sealed and placed in the nuclear magnetic resonance spectrometer for determination.

[0043] Ionic conductivity test method: CHI660E electrochemical workstation was used to test the AC impedance in the range of 0.1Hz to 100KHz, the AC amplitude was set to 5mV, and the test temperature was 30 to 70℃ to obtain the resistance of the solid electrolyte membrane, and then the electrolyte conductivity was obtained.

[0044] LSV test method: The linear sweep voltammetry (LSV) method was applied to the Li / SPE / SS battery using a CHI660E electrochemical workstation. The test temperature was 25°C, the voltage measurement range was 2 to 6 V, and the scan rate was 0.1 mV / s to obtain the current-potential curve.

[0045] Battery charge and discharge test method: Use the blue power test system to test the capacity of the battery at different charge and discharge currents under constant current conditions, and determine the battery's specific capacity and cycle performance.

[0046] In the following examples, N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP 12 FSI) was prepared by the following method:

[0047] (S1) under the protection of Ar gas, 9.92 g (0.1 mol) of the first compound (purity: 98%) and 40 mL of ethyl acetate solvent (purity: AR) were stirred and mixed in a flask to obtain a first mixed solution;

[0048] Then, 21.8 g (0.2 mol) of ethyl bromide (purity: 99%) was added dropwise to the first mixed solution, and the mixture was stirred at 50° C. for 24 hours to obtain a first solution, and the first solution was rotary evaporated to remove the solvent to obtain a crude product;

[0049] The crude product was then washed three times with anhydrous ether (purity: AR) and dried under vacuum at 70°C for 48 hours to obtain the second compound (PP 12 Br);

[0050] (S2) dissolving 16.11 g (0.0774 mol) of the second compound prepared in step (S1) in deionized water (25 mL), then adding dropwise a deionized solution of LiFSI (purity: battery grade) (wherein the ratio of LiFSI to deionized water is 17.37 g (0.093 mol): 20 mL), adding 100 mL of dichloromethane (purity: AR) until the mixture can no longer be stirred and stirring for 8 h to obtain a second mixed solution;

[0051] The second mixed solution was placed in a separatory funnel for extraction, and the lower dichloromethane phase was collected and washed three times with deionized water (25 mL each time), stirring for 15 min each time, until no Br was detected in the water layer with AgNO3. - The lower layer was taken, dichloromethane was removed by rotary evaporation, and vacuum dried at 80°C for 48 h to obtain the product N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP 12 FSI) Its DSC curve is as follows Figure 1 shown).

[0052] pass Figure 1It can be found that the synthesized ionic plastic crystal PP 12 FSI exhibits two solid-solid phase transitions at -40°C and -20°C, and a melting peak at 165°C, indicating that it can maintain the plastic phase in a wide temperature range close to room temperature. Therefore, after further compounding it with lithium salts and polymers, ions can be quickly transferred in the plastic phase of the plastic crystal, which is expected to develop new technologies for fast charging of high-safety lithium batteries.

[0053] Wherein, the chemical structure of the first compound is shown below:

[0054] Wherein, R1 is -CH3;

[0055] The chemical structure of the second compound is shown below:

[0056] Wherein, R1 is -CH3, R2 is -CH2CH3, and X is Br.

[0057] In the following examples, N-methyl-N-ethylmorpholine bis(fluorosulfonyl)imide (PPO 12 FSI) was prepared by the following method:

[0058] (S1) under the protection of Ar gas, 10.1 g (0.1 mol) of the third compound (purity: 98%) and 40 mL of ethyl acetate solvent (purity: AR) were stirred and mixed in a flask to obtain a third mixed solution;

[0059] Then 21.8 g (0.2 mol) of ethyl bromide (purity: 99%) was added dropwise to the third mixed solution, and stirred at 50°C for 24 hours. The solution was rotary evaporated to remove the solvent to obtain a crude product; the crude product was then washed three times with anhydrous ether (purity: AR) and vacuum dried at 70°C for 48 hours to obtain the fourth compound (PPO 12 Br);

[0060] (S2) 15.3 g (0.0728 mol) of the fourth compound obtained in step (S1) was dissolved in deionized water (25 mL), and a deionized solution of LiFSI (purity: battery grade) was added dropwise (wherein the ratio of LiFSI to deionized water was 17.37 g (0.093 mol): 20 mL). When stirring was almost impossible, 100 mL of dichloromethane (purity: AR) was added and stirred for 8 h to obtain a fourth mixed solution; the fourth mixed solution was placed in a separatory funnel for extraction, the lower dichloromethane phase was collected, and deionized water was added for stirring and washing three times (25 mL each time), each time for 15 min, until no Br was detected in the water layer with AgNO3 -The lower layer was taken, dichloromethane was removed by rotary evaporation, and vacuum dried at 80°C for 48 h to obtain the product N-methyl-N-ethylmorpholine bis(fluorosulfonyl)imide (PPO 12 FSI).

[0061] Wherein, the chemical structural formula of the third compound is shown as follows:

[0062] Wherein, R1 is -CH3;

[0063] The chemical structural formula of the fourth compound is shown below:

[0064] Wherein, R1 is -CH3, R2 is -CH2CH3, and X is Br.

[0065] Example 1

[0066] In this embodiment, vinylidene fluoride-hexafluoropropylene (P(VDF-HFP))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0067] P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:55:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0068] Its ionic conductivity at 25°C is 8.5×10 -4 S / cm. The first discharge capacity of Li / LiFePO4 battery at 25℃ and 0.2C is 147.0mAh / g. After 800 cycles, the discharge capacity at 5C and 25℃ is 127.3mAh / g, and the capacity retention rate is above 99% ( Figure 2 ).

[0069] Example 2

[0070] In this embodiment, vinylidene fluoride-trifluoroethylene (P(VDF-TRFE))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0071] P(VDF-TRFE),PP 12FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:55:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0072] Its ionic conductivity at 25°C is 8.7×10 -4 S / cm. The first discharge capacity of Li / LiFePO4 battery at 25℃ and 0.2C is 153.7mAh / g. After 1000 cycles, the discharge capacity at 5C and 25℃ is 126mAh / g, and the capacity retention rate is above 99% ( Figure 3 ).

[0073] Example 3

[0074] In this embodiment, vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene (P(VDF-TRFE-CTFE))-vinylidene fluoride-trifluoroethylene (P(VDF-TRFE))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0075] Combine P(VDF-TRFE-CTFE), P(VDF-TRFE), PP 12 FSI and LiFSI were stirred at 45°C for 12 hours in a mass ratio of 10:10:55:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove the remaining solvent and water, thereby obtaining a solid electrolyte membrane, such as Figure 4 As shown, a uniform and transparent solid electrolyte membrane is obtained.

[0076] Its ionic conductivity at 25°C is 9.15×10 -4 S / cm; the first discharge capacity of Li / LiFePO4 battery at 0.2C at 25℃ is 156.1mAh / g, the first cycle coulomb efficiency is 93.3%, the discharge capacity at 5C and 25℃ after 2800 cycles is 125mAh / g, and the capacity retention rate is above 98%; the discharge capacity at 6C and 25℃ after 1400 cycles is 123mAh / g, and the capacity retention rate is above 99% ( Figures 5 to 8 ).

[0077] Example 4

[0078] In this embodiment, vinylidene fluoride-trifluoroethylene (P(VDF-TRFE))-vinylidene fluoride-hexafluoropropylene (P(VDF-HFP))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0079] P(VDF-TRFE), P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 45°C for 12 hours in a mass ratio of 10:10:55:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0080] Its ionic conductivity at 25°C is 8.9×10 -4 The first discharge capacity of Li / LiFePO4 battery at 0.2C at 25°C is 156mAh / g, and the discharge capacity at 5C and 25°C after 800 cycles is 125mAh / g, with a capacity retention rate of about 99%.

[0081] Example 5

[0082] In this embodiment, vinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene (P(VDF-TRFE-CTFE))-vinylidene fluoride-trifluoroethylene (P(VDF-TRFE))-N-methyl-N-ethylmorpholinebis(fluorosulfonyl)imide (PPO) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0083] Combine P(VDF-TRFE-CTFE), P(VDF-TRFE), PPO 12 FSI and LiFSI were stirred at 45°C for 12 hours in a mass ratio of 10:10:60:20 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0084] Its ionic conductivity at 25°C is 9.07×10 -4 S / cm. Li / LiFePO4, the battery has a first discharge capacity of 153mAh / g at 0.2C at 25°C, and a discharge capacity of 122mAh / g at 5C and 25°C after 900 cycles, with a capacity retention rate of about 99%.

[0085] Comparative Example 1

[0086] In this comparative example, vinylidene fluoride-hexafluoropropylene (P(VDF-HFP))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0087] P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:20:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0088] At 25℃, its ionic conductivity is 1×10 -4 S / cm. The first discharge capacity of Li / LiFePO4 battery at 0.2C at 25℃ is 90.0mAh / g.

[0089] Comparative Example 2

[0090] In this comparative example, vinylidene fluoride-hexafluoropropylene (P(VDF-HFP))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0091] P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:40:25 to form a uniform solution; the solution was then cast onto a polytetrafluoroethylene template, most of the acetone was removed at room temperature under an Ar atmosphere, and the electrolyte membrane was then vacuum dried at 60°C for 48 hours, and then moved into an argon-filled glove box for drying for 24 hours to remove residual solvent and water to obtain a solid electrolyte membrane.

[0092] Its ionic conductivity at 25°C is 4×10 -4 S / cm. The first discharge specific capacity of Li / LiFePO4 battery at 0.2C at 25℃ is 110.0mAh / g.

[0093] Comparative Example 3

[0094] In this comparative example, vinylidene fluoride-hexafluoropropylene (P(VDF-HFP))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0095] P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:80:25 to form a uniform solution. The solution was then cast onto a polytetrafluoroethylene template, and most of the acetone was removed at room temperature under an Ar atmosphere. The electrolyte membrane was then vacuum dried at 60°C for 48 hours and then moved into an argon-filled glove box for 24 hours to remove residual solvent and water. The resulting solid electrolyte membrane was very sticky and had poor mechanical properties.

[0096] Comparative Example 4

[0097] In this comparative example, vinylidene fluoride (P(VDF))-N-methyl-N-ethylpiperidinium bis(fluorosulfonyl)imide (PP) was prepared by solution casting. 12 FSI)—Lithium bis(fluorosulfonyl)imide (LiFSI) solid electrolyte.

[0098] P(VDF-HFP), PP 12 FSI and LiFSI were stirred at 50°C for 12 hours in a mass ratio of 20:80:25 to form a uniform solution. The solution was then cast onto a polytetrafluoroethylene template, and most of the acetone was removed at room temperature under an Ar atmosphere. The electrolyte membrane was then vacuum dried at 60°C for 48 hours and then moved into an argon-filled glove box for 24 hours to remove residual solvent and water. The resulting solid electrolyte membrane was very sticky and had poor mechanical properties.

[0099] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A solid electrolyte, It is characterized in that It is obtained by using fluoropolymer as the matrix and introducing ionic plastic crystals and lithium salts; The mass ratio of the fluoropolymer, the ionic plastic crystal and the lithium salt is 20:4-100:1-40.

2. A solid electrolyte according to claim 1, It is characterized in that The fluoropolymer is selected from one or more of the compounds represented by the following structural formulas; Wherein, in formula (1) to formula (6), the molecular weight of the polymer is 100,000 to 600,000; x, y, n and m in each structural formula are independently positive integers; The ionic plastic crystal is selected from one or more of pyrrole ionic plastic crystals, piperidine ionic plastic crystals or morpholine ionic plastic crystals; The lithium salt is selected from one or more of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide or lithium difluorooxalatoborate.

3. A solid electrolyte according to claim 2, It is characterized in that The fluoropolymer is selected from one of P(VDF-HFP), PVDF, P(VDF-CTFE), P(VDF-TrFE), P(VDF-TrFE-CTFE) and PTFE.

4. A solid electrolyte according to claim 2, It is characterized in that The structural formula of the pyrrole ionic plastic crystal is shown in formula (7), the structural formula of the piperidine ionic plastic crystal is shown in formula (8), and the structural formula of the morpholine ionic plastic crystal is shown in formula (9); Among them, in formula (7), formula (8) and formula (9), R 1 Independently selected from -CH 3 or -CH 2 CH 3 , R 2 Independently selected from -CH 3 、-CH 2 CH 3 or -CH 2 CH 2 CH 3 .

5. A solid electrolyte according to claim 4, It is characterized in that The ionic plastic crystal is selected from PP 12 FSI or PPO 12 One of the FSIs.

6. A method for preparing a solid electrolyte as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: The fluoropolymer, lithium salt and ionic plastic crystals are dissolved and mixed, then poured into a mold, and subjected to solvent removal and drying treatment to obtain a solid electrolyte.

7. A method for preparing a solid electrolyte according to claim 6, It is characterized in that During the mixing process, the temperature is 25-80°C; The solvent removal process is carried out under an inert atmosphere and at room temperature; The drying process specifically includes vacuum drying and argon drying; During the vacuum drying process, the temperature is 25-80°C and the time is 8-48h; During the argon drying process, the temperature is room temperature and the time is 8 to 48 hours.

8. A battery, It is characterized in that The battery contains the solid electrolyte according to any one of claims 1 to 5.

9. A method for preparing a battery, It is characterized in that The positive electrode sheet, the electrolyte membrane prepared by the solid electrolyte according to any one of claims 1 to 5, and the negative electrode sheet are stacked in order from bottom to top to form a laminate, and then punched to obtain a battery.

10. A method for preparing a battery according to claim 9, It is characterized in that The positive electrode sheet is a positive electrode sheet using lithium iron phosphate / lithium cobalt oxide / lithium nickel cobalt manganese oxide as the positive electrode material; Among them, the structural formula of lithium nickel cobalt manganese oxide is LiNi 0.8 Co 0.1 Mn 0.1 O 2 、LiNi 0.6 Co 0.2 Mn 0.2 O 2 or LiNi 0.5 Co 0.3 Mn 0.2 O 2 One of; The negative electrode sheet is a negative electrode sheet using lithium as the negative electrode material.

Citation Information

Patent Citations

  • Compound polymer electrolytic material and preparation method thereof

    CN101045806A

  • Polymer electrolyte composition, polymer electrolyte sheet, manufacturing method thereof, electrode for electrochemical device and polymer secondary battery

    CN110661034A

  • Solid electrolyte containing organic ion plastic crystal, and application thereof

    CN111370757A

  • Organic ion plastic crystal doped composite electrolyte membrane and preparation method and application thereof

    CN115224357A

  • Phase change solid electrolyte and preparation method thereof

    CN118173879A