A mixed solution capable of improving the stability of metallic lithium negative electrode and its preparation method and application

By forming a composite protective film of lithiated naphthol and lithium carbonate on the surface of the metal lithium negative electrode, the problems of lithium dendrites are solved, the stability and cycle life of lithium metal batteries are improved, and more efficient energy density and Security.

CN114203976BActive Publication Date: 2024-11-08HARBIN NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111508058.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-10
Publication Date
2024-11-08
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

The metal lithium negative electrode is prone to growth of lithium dendrites and volume expansion during charging and discharge, resulting in poor circulation performance and low safety.

Method used

A mixed solution of lithiated naphthol and lithium carbonate is used as a protective film material. By forming an organic/inorganic composite artificial solid electrolyte interface (SEI) film on the surface of metal lithium, lithium ion conductivity is improved and lithium dendrites are inhibited.

Benefits of technology

It significantly improves the stability and cycle life of the metal lithium negative electrode, extends the service life, reduces volume expansion, and optimizes the rate performance and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114203976B_ABST
    Figure CN114203976B_ABST
Patent Text Reader

Abstract

A mixed solution capable of improving the stability of a metal lithium negative electrode, a preparation method and an application, and it relates to a mixed solution, a preparation method and an application. The purpose of the present invention is to solve the problem that the existing metal lithium negative electrode is prone to the growth of lithium dendrites and volume expansion. The solute of a mixed solution capable of improving the stability of a metal lithium negative electrode is lithiated naphthol and lithium carbonate, and the solvent is N-methylpyrrolidone. Method: 1. Prepare lithiated naphthol; 2. Prepare a mixed solution; A mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode. A mixed solution capable of improving the stability of a metal lithium negative electrode and a protective film for a metal lithium negative electrode obtained by the present invention have ingenious processes, low-cost processing equipment, simple procedures and methods, low costs, are conducive to large-scale industrial production, and can have broad application prospects in various metal lithium batteries and other energy storage fields. The present invention can obtain a mixed solution capable of improving the stability of a metal lithium negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a mixed solution and a preparation method and application thereof. Background Art

[0002] With the rapid development of economy and technology, people are in urgent need of clean energy. The development of renewable energy such as solar energy, wind energy, geothermal energy, tidal energy, etc. has gradually attracted people's attention. However, these new energy sources are intermittent and volatile, and cannot provide large-scale and stable energy for human daily life and production. The research on energy storage and conversion systems is the key to achieving a continuous supply of clean energy, and has attracted widespread attention for many years. Among them, rechargeable secondary batteries are a very important choice in energy storage systems, so they have become a hot topic of research. Chemical batteries have a history of more than 200 years, from nickel-cadmium batteries, lead-acid batteries, to environmentally friendly nickel-hydrogen batteries and lithium secondary batteries, and are gradually developing in the direction of high energy density, safety, and environmental protection.

[0003] The metallic lithium anode has an extremely high specific capacity (3860 mAh / g) and the lowest reduction potential (-3.040 V vs. standard hydrogen electrode), and is known as the "holy grail" of energy storage. Using metallic lithium as the negative electrode material and matching it with an ideal positive electrode material (such as ternary materials, sulfur or oxygen, etc.) can produce a high energy density lithium metal battery. However, during the charge and discharge process, the metallic lithium anode material will undergo uneven deposition, causing dendrite growth, resulting in lithium pulverization and volume expansion. At the same time, the fresh lithium exposed during the charge and discharge process will react with the electrolyte to form an unstable solid electrolyte interface (SEI) film, causing further decomposition of the electrolyte. In addition, the metallic lithium anode of the lithium-sulfur battery also has serious corrosion problems caused by the "shuttle effect" of lithium polysulfides. Therefore, lithium metal batteries generally have the disadvantages of poor cycle performance and low safety. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the existing metal lithium negative electrode is prone to lithium dendrite growth and volume expansion, and to provide a mixed solution and a preparation method and application that can improve the stability of the metal lithium negative electrode.

[0005] The solute of a mixed solution capable of improving the stability of a metal lithium negative electrode is lithiated naphthol and lithium carbonate, and the solvent is N-methylpyrrolidone; the mass ratio of the solute to the mixed solution capable of improving the stability of a metal lithium negative electrode is 1:(50-1000); and the mass ratio of the lithiated naphthol to the lithium carbonate is (10-1000):1.

[0006] A method for preparing a mixed solution that can improve the stability of a metallic lithium negative electrode is completed by the following steps:

[0007] 1. Preparation of lithiated naphthol:

[0008] adding lithium hydroxide monohydrate to a naphthol aqueous solution, and then stirring under heating conditions to obtain a lithium hydroxide / naphthol aqueous solution; drying the lithium hydroxide / naphthol aqueous solution to completely evaporate water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0009] 2. Preparation of mixed solution:

[0010] Dissolving lithiated naphthol in N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; adding lithium carbonate to the organic solution of lithiated naphthol and stirring to obtain a mixed solution capable of improving the stability of a metallic lithium negative electrode;

[0011] The mass ratio of lithiated naphthol to lithium carbonate in the mixed solution capable of improving the stability of the metallic lithium negative electrode is (10-1000):1;

[0012] The mass ratio of the total mass of the lithiated naphthol and lithium carbonate to the mixed solution for improving the stability of the metal lithium negative electrode is 1:(50-1000).

[0013] A mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode.

[0014] Beneficial effects of the present invention:

[0015] 1. A mixed solution obtained by the present invention can improve the stability of the metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of the lithium sheet; the protective film is composed of lithiated naphthol and lithium carbonate, and has a thickness of 200nm to 5μm. Among them, the lithiated naphthol film is uniform and continuous, has good toughness, and is tightly adhered to the surface of the metal lithium sheet; the lithium carbonate is a granular prism, discretely embedded in the lithiated naphthol film; the long side of the lithium carbonate prism is 2 to 10μm, the short side is 0.5 to 5μm, and has a monoclinic crystal structure (JCPDS 9-0359);

[0016] 2. A mixed solution obtained by the present invention can improve the stability of the metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of the lithium sheet; the protective film has good lithium ion conductivity; its coating not only does not hinder the transfer of lithium ions, but the charge transfer resistance (20Ω) after activation is better than that of a new pure lithium sheet (37Ω);

[0017] 3. A mixed solution obtained by the present invention can improve the stability of metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of lithium sheet; the protective film can well inhibit the growth of lithium dendrites; the current density of the metal lithium sheet (450μm) protected by the film is 1mAcm -2 , 1mAhcm -2When the current density is 1mAcm -2 , 10mAhcm -2 When the current density is 5 mA cm -2 , 5mAhcm -2 When the film is used, it can stably cycle for 120 hours, and the cycle life is extended by more than 4 times; the service life of the ultra-thin metal lithium sheet (50μm) protected by the film is further extended, and can stably cycle for 200 hours;

[0018] 4. A mixed solution obtained by the present invention can improve the stability of the metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of the lithium sheet; the protective film can reduce the volume expansion of the metal lithium negative electrode during the cycle by 56.7%;

[0019] 5. A mixed solution obtained by the present invention can improve the stability of metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of lithium sheet; the metal lithium sheet protected by the film does not show obvious polarization at different current densities, showing good rate performance. The protective film is applied to the metal lithium negative electrode of lithium-sulfur battery, and the battery capacity can be 1164, 946.7, 807.2, 614.8, 425.4 mAh g at current densities of 0.1, 0.2, 0.5, 1 and 2C, respectively. -1 ;

[0020] 6. A mixed solution obtained by the present invention can improve the stability of metal lithium negative electrode, and form an organic / inorganic composite artificial SEI protective film on the surface of lithium sheet; the protective film is applied to the metal lithium negative electrode of lithium-sulfur battery, so that the cycle stability of the battery is significantly improved; when the current density is 0.1C, the initial discharge capacity of the lithium-sulfur battery with metal lithium coated with the protective film as the negative electrode is 1165.3mAh g -1 After 10 cycles, it is 978.8 mAh g -1 , after 100 cycles, 730mAh g -1 The capacity retention rates are 84% and 63%, respectively, which are significantly better than the metal lithium anode without protective film (74% and 47%). When the current density is 0.5C, the initial discharge capacity of the lithium-sulfur battery with the metal lithium coated with protective film as the anode is 970.7mAh g -1 , after 300 cycles, it is 622.3mAh g -1 , the capacity retention rate can be 64%, which is better than the metal lithium negative electrode without protective film (54%);

[0021] 7. The mixed solution and protective film of the metal lithium negative electrode obtained by the present invention can improve the stability of the metal lithium negative electrode, and the process is ingenious, the processing equipment is cheap, the procedure and method are simple, the cost is low, and it is conducive to large-scale industrial production;

[0022] 8. The mixed solution and protective film of the metal lithium negative electrode obtained by the present invention, which can improve the stability of the metal lithium negative electrode, can have broad application prospects in various metal lithium batteries and other energy storage fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is an X-ray diffraction spectrum, in which 1 is lithiated naphthol, 2 is a stainless steel substrate, 3 is Li2CO3, LN is a lithiated naphthol protective film prepared in Comparative Example 1 coated on a stainless steel substrate, and LNL is a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 coated on a stainless steel substrate;

[0024] Figure 2 This is a cross-sectional scanning electron microscope image of the composite protective film on the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1;

[0025] Figure 3 This is a scanning electron microscope image of the composite protective film on the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1;

[0026] Figure 4 1 is a lithium ion impedance spectrum curve of a symmetrical battery prepared in Example 2 using the high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as an electrode, and 2 is a lithium ion impedance spectrum curve of a symmetrical battery prepared in Comparative Example 2 using the metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode;

[0027] Figure 5 1 is a first cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, 2 is a cycle stability curve of a symmetrical battery prepared with a metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode in Comparative Example 2, and 3 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode in Example 2;

[0028] Figure 6 The cycle stability curve of a symmetrical battery prepared in Example 2 using the high-stability metal lithium electrode sheet coated with the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode;

[0029] Figure 71 is a second cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, 2 is a cycle stability curve of a symmetrical battery prepared with a metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode in Comparative Example 2, and 3 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode in Example 2;

[0030] Figure 8 1 is a third cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, and 2 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as an electrode in Example 2;

[0031] Fig. 9 are scanning electron microscope images, in which (a), (b), and (c) are scanning electron microscope images of a pure metal lithium sheet after deposition of an asymmetric battery assembled from a metal copper sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 3 and a pure metal lithium sheet, and (d), (e), and (f) are scanning electron microscope images of a pure metal lithium sheet after deposition of an asymmetric battery assembled from a metal copper sheet coated with lithiated naphthol and a pure metal lithium sheet prepared in Comparative Example 4 in Comparative Example 5;

[0032] Fig.10 The asymmetric battery assembled from the copper and pure lithium metal sheets coated with lithiated naphthol and lithium carbonate protective film prepared in Example 3 in Example 4 was 5 mAh cm -2 Cross-sectional SEM image of the copper electrode sheet after deposition at a deposition capacity of ;

[0033] Fig.11 The asymmetric battery assembled from the metal copper coated with lithiated naphthol and the pure metal lithium sheet prepared in Comparative Example 4 in Comparative Example 5 has a power of 5 mAh cm -2 Cross-sectional SEM image of the copper electrode sheet after deposition at a deposition capacity of ;

[0034] Fig.12 The impedance spectrum of lithium-sulfur battery. The left figure is the impedance spectrum of uncycled lithium-sulfur battery, and the right figure is the impedance spectrum of lithium-sulfur battery under high current (5mA cm -2 ) Impedance spectrum of the lithium-sulfur battery after 5 cycles; wherein, in the figure, 1 is the impedance spectrum of the lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, 2 is the impedance spectrum of the lithium-sulfur battery prepared with a metal lithium electrode sheet coated with lithiated naphthol as the negative electrode in Comparative Example 7, and 3 is the impedance spectrum of the lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0035] Fig.13 1 is a charge-discharge curve diagram, in which 1 is a charge-discharge curve of the first cycle of a lithium-sulfur battery prepared with a pure metal lithium sheet as a negative electrode in Comparative Example 6, 2 is a charge-discharge curve of the tenth cycle of a lithium-sulfur battery prepared with a pure metal lithium sheet as a negative electrode in Comparative Example 6, 3 is a charge-discharge curve of the first cycle of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as a negative electrode in Example 5, 4 is a charge-discharge curve of the tenth cycle of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as a negative electrode in Example 5;

[0036] Fig.14 1 is a fourth cycle stability graph, in which 1 is a cycle stability curve of a lithium-sulfur battery prepared with the pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a cycle stability curve of a lithium-sulfur battery prepared with the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0037] Fig.15 1 is a fifth cycle stability graph, in which 1 is a cycle stability curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a cycle stability curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0038] Fig.16 : is a first rate characteristic graph, in which A is a rate characteristic curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and B is a rate characteristic curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0039] Fig.17 1 is a first rate characteristic graph, in which 1 is a rate characteristic curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a rate characteristic curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0040] Fig.18 Figures are SEM images, where (a) and (b) are SEM images of a lithium-sulfur battery prepared with a pure metallic lithium sheet as the negative electrode in Comparative Example 6 after 10 cycles at 0.1C, and (c) and (d) are SEM images of a lithium-sulfur battery prepared with a high-stability metallic lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode after 10 cycles at 0.1C in Example 5. DETAILED DESCRIPTION

[0041] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.

[0042] Specific implementation method 1: In this implementation method, the solutes of a mixed solution that can improve the stability of a metallic lithium negative electrode are lithiated naphthol and lithium carbonate, and the solvent is N-methylpyrrolidone; the mass ratio of the solute to the mixed solution that can improve the stability of a metallic lithium negative electrode is 1:(50-1000); the mass ratio of the lithiated naphthol to lithium carbonate is (10-1000):1.

[0043] Specific embodiment 2: This embodiment differs from the specific embodiment 1 in that the lithiated naphthol is prepared according to the following steps:

[0044] Add lithium hydroxide monohydrate to the naphthol aqueous solution, then stir under heating conditions to obtain a lithium hydroxide / naphthol aqueous solution; dry the lithium hydroxide / naphthol aqueous solution to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol. The other steps are the same as those in the first embodiment.

[0045] Specific implementation method three: The difference between this implementation method and specific implementation method two is that: the mass ratio of the lithium hydroxide monohydrate to the naphthol aqueous solution is (10mg-15mg): (3mL-8mL); the mass fraction of the naphthol aqueous solution is 4%-6%; the drying temperature is 25℃-80℃; the stirring temperature under the heating condition is 60℃, the stirring speed is 300r / min-1500r / min, and the stirring time is 1h-3h. The other steps are the same as those in specific implementation method two.

[0046] Specific embodiment 4: In this embodiment, a method for preparing a mixed solution that can improve the stability of a metallic lithium negative electrode is completed by the following steps:

[0047] 1. Preparation of lithiated naphthol:

[0048] adding lithium hydroxide monohydrate to a naphthol aqueous solution, and then stirring under heating conditions to obtain a lithium hydroxide / naphthol aqueous solution; drying the lithium hydroxide / naphthol aqueous solution to completely evaporate water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0049] 2. Preparation of mixed solution:

[0050] Dissolving lithiated naphthol in N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; adding lithium carbonate to the organic solution of lithiated naphthol and stirring to obtain a mixed solution capable of improving the stability of a metallic lithium negative electrode;

[0051] The mass ratio of lithiated naphthol to lithium carbonate in the mixed solution capable of improving the stability of the metallic lithium negative electrode is (10-1000):1;

[0052] The mass ratio of the total mass of the lithiated naphthol and lithium carbonate to the mixed solution for improving the stability of the metal lithium negative electrode is 1:(50-1000).

[0053] Specific embodiment 5: The difference between this embodiment and specific embodiment 4 is that the volume ratio of the mass of lithium hydroxide monohydrate and the naphthol aqueous solution described in step 1 is (10mg-15mg):(3mL-8mL); the mass fraction of the naphthol aqueous solution is 4%-6%. The other steps are the same as those of specific embodiment 4.

[0054] Specific embodiment 6: This embodiment differs from specific embodiments 4 to 5 in that the drying temperature in step 1 is 25° C. to 80° C. The other steps are the same as those in specific embodiments 4 to 5.

[0055] Specific embodiment 7: This embodiment differs from specific embodiments 4 to 6 in that: the stirring temperature under the heating conditions described in step 1 is 60°C, the stirring speed is 300r / min to 1500r / min, and the stirring time is 1h to 3h; the stirring speed described in step 2 is 300r / min to 1500r / min, and the stirring time is 10h to 12h. The other steps are the same as those of specific embodiments 4 to 6.

[0056] Specific implementation method eight: This implementation method is a mixed solution that can improve the stability of the metal lithium negative electrode and is used to improve the stability of the metal lithium negative electrode.

[0057] Specific embodiment 9: The difference between this embodiment and specific embodiment 8 is that a mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode in accordance with the following steps:

[0058] The mixed solution that can improve the stability of the metal lithium negative electrode is dripped onto the surface of the lithium sheet and then dried to obtain a high-stability metal lithium electrode sheet coated with a composite protective film. The other steps are the same as those in the eighth embodiment.

[0059] Specific embodiment 10: This embodiment is different from specific embodiment 8 or 9 in that the ratio of the volume of the mixed solution capable of improving the stability of the metal lithium negative electrode to the surface area of ​​the lithium sheet is (40 μL to 60 μL): (1 cm 2 ~1.5cm 2 ); the drying temperature is 60° C., and the drying time is 10 h to 12 h. The other steps are the same as those in the eighth or ninth embodiment.

[0060] The following examples are used to verify the beneficial effects of the present invention:

[0061] Embodiment 1: A method for preparing a high-stability lithium metal electrode sheet coated with a composite protective film is completed by the following steps:

[0062] 1. Preparation of lithiated naphthol:

[0063] 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0064] 2. Preparation of mixed solution:

[0065] 0.1 g of lithiated naphthol was dissolved in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; 5 mg of lithium carbonate was added to the organic solution of 10 g of lithiated naphthol, and stirred at a stirring speed of 500 r / min for 12 h to obtain a mixed solution that can improve the stability of the metal lithium negative electrode;

[0066] 3. Drip coating electrode sheet:

[0067] 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the lithium sheet was dried at 60°C for 12 hours to obtain a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate;

[0068] 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the stainless steel substrate is coated with a composite protective film of lithiated naphthol and lithium carbonate to obtain a stainless steel substrate.

[0069] Comparative Example 1: The preparation method of the metal lithium electrode sheet coated with lithiated naphthol is completed by the following steps:

[0070] 1. Preparation of lithiated naphthol:

[0071] 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0072] 2. Prepare the solution and drip-coat the electrode sheet:

[0073] Dissolve 0.1 g of lithiated naphthol in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol. Apply 50 μL of the organic solution of lithiated naphthol dropwise on a 1.91 cm 2 The surface of the lithium sheet was dried at 60°C for 12 hours to obtain a metal lithium electrode sheet coated with a lithiated naphthol protective film;

[0074] 50 μL of lithiated naphthol organic solution was dropped onto a 1.91 cm 2 The surface of the stainless steel substrate is coated with a lithiated naphthol protective film to obtain a stainless steel substrate.

[0075] Figure 1 is an X-ray diffraction spectrum, in which 1 is lithiated naphthol, 2 is a stainless steel substrate, 3 is Li2CO3, LN is a lithiated naphthol protective film prepared in Comparative Example 1 coated on a stainless steel substrate, and LNL is a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 coated on a stainless steel substrate;

[0076] from Figure 1 It can be seen that the diffraction peaks in the figure belong to lithiated naphthol and lithium carbonate, wherein lithium carbonate has a monoclinic crystal structure (JCPDS9-0359). It can be seen that the composite protective film synthesized in Example 1 is composed of lithiated naphthol and lithium carbonate.

[0077] Figure 2 This is a cross-sectional scanning electron microscope image of the composite protective film on the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1;

[0078] Figure 3 This is a scanning electron microscope image of the composite protective film on the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1;

[0079] from Figure 2 , Figure 3 It can be seen that the thickness of the synthesized lithiated naphthol and lithium carbonate composite protective film is 2.5 μm; among them, the lithiated naphthol film is uniform and continuous; the lithium carbonate is granular prisms with a long side of 4 μm and a short side of 2.5 μm, which is discretely embedded in the lithiated naphthol film.

[0080] Assembly of symmetrical battery:

[0081] Example 2: A mixed solution of DOL / DME is used as a solvent, wherein the volume ratio of DOL to DME is 1:1; LiTFSI and Li2S8 are used as solutes, and LiNO3 is used as an additive to obtain a polysulfide electrolyte; the concentration of LiTFSI in the polysulfide electrolyte is 1 mol / L, the concentration of Li2S8 is 2 mol / L, and the mass fraction of LiNO3 is 2%;

[0082] 40 μL of polysulfide electrolyte was taken, Celgard 2400 was used as a diaphragm, and the high-stability metal lithium electrode sheet coated with a composite protective film prepared in Example 1 was used as an electrode to prepare a symmetrical battery in an argon glove box.

[0083] Comparative Example 2: The difference between this embodiment and the second embodiment is that a metal lithium electrode sheet coated with a lithiated naphthol protective film is used as an electrode, and the other steps and parameters are the same as those of the second embodiment.

[0084] Comparative Example 3: The difference between this embodiment and the second embodiment is that pure metal lithium sheets are used as electrodes, and the other steps and parameters are the same as those of the second embodiment.

[0085] Figure 4 1 is a lithium ion impedance spectrum curve of a symmetrical battery prepared in Example 2 using the high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as an electrode, and 2 is a lithium ion impedance spectrum curve of a symmetrical battery prepared in Comparative Example 2 using the metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode;

[0086] from Figure 4 It can be seen that the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 has good lithium ion conductivity; compared with the lithiated naphthol protective film, the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 exhibits very small lithium ion impedance, which represents a higher lithium ion conductivity; the higher the lithium ion conductivity exhibited by the protective film on the surface of the lithium sheet, the more uniform the deposition of lithium ions on the surface of the lithium sheet, thus indicating that the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 can achieve more uniform lithium ion deposition, thereby promoting stable circulation of the electrode.

[0087] Figure 5 1 is a first cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, 2 is a cycle stability curve of a symmetrical battery prepared with a metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode in Comparative Example 2, and 3 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode in Example 2;

[0088] Figure 6 The cycle stability curve of a symmetrical battery prepared in Example 2 using the high-stability metal lithium electrode sheet coated with the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode;

[0089] Figure 71 is a second cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, 2 is a cycle stability curve of a symmetrical battery prepared with a metal lithium electrode sheet coated with a lithiated naphthol protective film as an electrode in Comparative Example 2, and 3 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as an electrode in Example 2;

[0090] Figure 8 1 is a third cycle stability curve diagram, in which 1 is a cycle stability curve of a symmetrical battery prepared with a pure metal lithium sheet as an electrode in Comparative Example 3, and 2 is a cycle stability curve of a symmetrical battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as an electrode in Example 2;

[0091] from Figures 5 to 8 It can be seen that the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 can well improve the cycle stability of the metal lithium negative electrode; the metal lithium sheet (450 μm) protected by the film has a cycle stability of 1 mA cm -2 , 1mAh cm -2 Under the conditions, it can stably cycle for 800 hours; at 1mA cm -2 , 10mAh cm -2 Under the same conditions, it can stably cycle for 480 hours; at 5 mA cm -2 , 5mAhcm -2 Under the same conditions, the battery can be stably cycled for 120 hours, and the cycle life is extended by more than 4 times. The service life of the ultra-thin lithium metal sheet (50μm) protected by the membrane is further extended, and the battery can be stably cycled for 200 hours.

[0092] Assembly of asymmetric cells:

[0093] Embodiment 3: The preparation method of the metal copper sheet coated with the protective film is completed by the following steps:

[0094] 1. Preparation of lithiated naphthol:

[0095] 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0096] 2. Preparation of mixed solution:

[0097] 0.1 g of lithiated naphthol was dissolved in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; 5 mg of lithium carbonate was added to the organic solution of 10 g of lithiated naphthol, and stirred at a stirring speed of 500 r / min for 12 h to obtain a mixed solution that can improve the stability of the metal lithium negative electrode;

[0098] 3. Drip coating electrode sheet:

[0099] 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the metal copper sheet was then dried at 60°C for 12 hours to obtain a metal copper sheet coated with lithiated naphthol and lithium carbonate protective film.

[0100] Example 4: An asymmetric battery assembled with a metal copper sheet coated with a protective film prepared in Example 3 and a pure metal lithium sheet is completed by the following steps:

[0101] A DOL / DME mixed solution is used as a solvent, wherein the volume ratio of DOL to DME is 1:1; LiTFSI and Li2S8 are used as solutes, and LiNO3 is used as an additive to obtain a polysulfide electrolyte; the concentration of LiTFSI in the polysulfide electrolyte is 1 mol / L, the concentration of Li2S8 is 2 mol / L, and the mass fraction of LiNO3 is 2%;

[0102] Take 40 μL of polysulfide electrolyte, use Celgard 2400 as a diaphragm, use pure metal lithium sheets and metal copper sheets coated with lithiated naphthol and lithium carbonate protective film prepared in Example 3 as electrodes, and assemble an asymmetric battery in an argon glove box.

[0103] Comparative Example 4: The preparation method of the metal copper sheet coated with lithiated naphthol is completed according to the following steps:

[0104] 1. Preparation of lithiated naphthol:

[0105] 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol;

[0106] 2. Prepare the solution and drip-coat the electrode sheet:

[0107] Dissolve 0.1 g of lithiated naphthol in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol. Apply 50 μL of the organic solution of lithiated naphthol dropwise on a 1.91 cm 2 The surface of the metal copper sheet was coated with lithiated naphthol, and then dried at 60°C for 12 hours to obtain a metal copper sheet coated with lithiated naphthol.

[0108] Comparative Example 5: The asymmetric battery assembled from the metal copper sheet coated with lithiated naphthol prepared in Comparative Example 4 and the pure metal lithium sheet is completed according to the following steps:

[0109] A DOL / DME mixed solution is used as a solvent, wherein the volume ratio of DOL to DME is 1:1; LiTFSI and Li2S8 are used as solutes, and LiNO3 is used as an additive to obtain a polysulfide electrolyte; the concentration of LiTFSI in the polysulfide electrolyte is 1 mol / L, the concentration of Li2S8 is 2 mol / L, and the mass fraction of LiNO3 is 2%;

[0110] Take 40 μL of polysulfide electrolyte, use Celgard 2400 as a diaphragm, use pure metal lithium sheets and the metal copper sheets coated with lithiated naphthol prepared in Comparative Example 4 as electrodes, and assemble an asymmetric battery in an argon glove box.

[0111] Fig. 9 are scanning electron microscope images, in which (a), (b), and (c) are scanning electron microscope images of a pure metal lithium sheet after deposition of an asymmetric battery assembled from a metal copper sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 3 and a pure metal lithium sheet, and (d), (e), and (f) are scanning electron microscope images of a pure metal lithium sheet after deposition of an asymmetric battery assembled from a metal copper sheet coated with lithiated naphthol and a pure metal lithium sheet prepared in Comparative Example 4 in Comparative Example 5;

[0112] from Fig. 9 It can be seen that the composite protective film of lithiated naphthol and lithium carbonate can effectively inhibit the growth of lithium dendrites. The asymmetric battery assembled using uncoated metal lithium sheets and metal copper sheets coated with the composite protective film of lithiated naphthol and lithium carbonate as electrodes increased the deposition capacity density from 0.5 to 1 and then to 3 mAh cm -2 The morphology of lithium deposition is flat and uniform. This is mainly because the high lithium ion conductivity of the protective film makes the lithium ion concentration on the upper layer of the lithium sheet and the lithium ion concentration on the protective film not much different, so that the lithium ions on the surface of the lithium sheet can be replenished in time after deposition, thereby promoting the uniform deposition of lithium ions on the surface of the lithium sheet. In contrast, the asymmetric battery assembled with uncoated metal lithium sheets and lithiated naphthol-coated metal copper as electrodes has a lower deposition capacity density of 0.5 mAh cm -2 Under this condition, many lithium dendrites are deposited after lithium ions pass through the lithiated naphthol membrane. The existence of these lithium dendrites will further cause the uneven deposition of lithium ions, resulting in the serious growth of lithium dendrites. When the deposition density reaches 1 mAh cm -2 and 3mAhcm -2 When the electrode is heated, a large number of lithium dendrites appear on the surface of the electrode.

[0113] Fig.10The asymmetric battery assembled from the copper and pure lithium metal sheets coated with lithiated naphthol and lithium carbonate protective film prepared in Example 3 in Example 4 was 5 mAh cm -2 Cross-sectional SEM image of the copper electrode sheet after deposition at a deposition capacity of ;

[0114] Fig.11 The asymmetric battery assembled from the metal copper coated with lithiated naphthol and the pure metal lithium sheet prepared in Comparative Example 4 in Comparative Example 5 has a power of 5 mAh cm -2 Cross-sectional SEM image of the copper electrode sheet after deposition at a deposition capacity of ;

[0115] from Fig.10 , Fig.11 It can be seen that at 5 mAhcm -2 At the deposition capacity of , the cross-sectional thickness of lithium ions deposited when passing through the lithiated naphthol layer of the comparison sample is about 42.3μm, and the deposition thickness through the lithiated naphthol and lithium carbonate composite film (protective film) is about 27μm, and the volume expansion is reduced by 56.7%; the smaller deposition thickness and more compact deposition structure indicate that the composite protective film can promote the uniform deposition of lithium ions and effectively alleviate the volume expansion of the lithium negative electrode.

[0116] Assembly of lithium-sulfur batteries:

[0117] Example 5: A lithium-sulfur battery prepared by using the high-stability metal lithium electrode sheet coated with the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 as the negative electrode is completed by the following steps:

[0118] First, the mixed powder of activated carbon and sulfur powder was continuously heated at 155°C for 12 hours (the mass ratio of activated carbon to sulfur powder was 3:7). The mixed powder obtained after heating was mixed again with acetylene black and PVDF in a mass ratio of 8:1:1, and then an appropriate amount of NMP organic solvent was added and stirred for 2 hours at room temperature to obtain a positive electrode slurry. The mixed positive electrode slurry was coated on an aluminum foil current collector using a coater and dried at 60°C for 12 hours. The dried sample was punched into a 13 mm diameter disc using a puncher to obtain a positive electrode of a lithium-sulfur battery. The positive electrode surface loading was 1.3 mg cm -2 ; The solute of the electrolyte used is lithium bis(trifluoromethane)sulfonyl imide (LiTFSI), the solvent is a mixture of LiNO3, DOL and DME, the mass fraction of LiNO3 in the solvent is 2%, and the volume ratio of DOL and DME is 1:1; the concentration of lithium bis(trifluoromethane)sulfonyl imide (LiTFSI) in the electrolyte is 1 mol / L;

[0119] Then, 40 μl of electrolyte was taken, Celgard 2400 was used as a diaphragm, and the high-stability metal lithium electrode sheet coated with a composite protective film prepared in Example 1 was used as an electrode, and a lithium-sulfur battery was assembled in an argon glove box.

[0120] Comparative Example 6: The difference between this example and Example 5 is that a pure metal lithium sheet is used as the negative electrode, and a lithium-sulfur battery is assembled in an argon glove box. The other steps and parameters are the same as those in Example 5.

[0121] Comparative Example 7: The difference between this example and Example 5 is that the metal lithium electrode sheet coated with lithiated naphthol is used as the negative electrode, and the lithium-sulfur battery is assembled in an argon glove box. The other steps and parameters are the same as those in Example 5.

[0122] Fig.12 The impedance spectrum of lithium-sulfur battery. The left figure is the impedance spectrum of uncycled lithium-sulfur battery, and the right figure is the impedance spectrum of lithium-sulfur battery under high current (5mA cm -2 ) Impedance spectrum of the lithium-sulfur battery after 5 cycles; wherein, in the figure, 1 is the impedance spectrum of the lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, 2 is the impedance spectrum of the lithium-sulfur battery prepared with a metal lithium electrode sheet coated with lithiated naphthol as the negative electrode in Comparative Example 7, and 3 is the impedance spectrum of the lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0123] from Fig.12 It can be seen that although the charge transfer resistance of the pure metal lithium sheet is the smallest before the cycle, its electrochemical impedance increases significantly as the charge and discharge process proceeds. This is because the uneven deposition of lithium ions makes the electrode structure loose and more dead lithium appears, which hinders the transfer of lithium ions. In contrast, the coating of the lithiated naphthol and lithium carbonate composite protective film prepared in Example 1 not only does not hinder the transfer of lithium ions, but also has a good effect at high current (5mA cm -2 ) After 5 cycles, the charge transfer resistance (20Ω) is better than that of a new pure lithium sheet (37Ω).

[0124] Fig.13 1 is a charge-discharge curve diagram, in which 1 is a charge-discharge curve of the first cycle of a lithium-sulfur battery prepared with a pure metal lithium sheet as a negative electrode in Comparative Example 6, 2 is a charge-discharge curve of the tenth cycle of a lithium-sulfur battery prepared with a pure metal lithium sheet as a negative electrode in Comparative Example 6, 3 is a charge-discharge curve of the first cycle of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as a negative electrode in Example 5, 4 is a charge-discharge curve of the tenth cycle of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as a negative electrode in Example 5;

[0125] Fig.141 is a fourth cycle stability graph, in which 1 is a cycle stability curve of a lithium-sulfur battery prepared with the pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a cycle stability curve of a lithium-sulfur battery prepared with the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0126] Fig.15 1 is a fifth cycle stability graph, in which 1 is a cycle stability curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a cycle stability curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0127] from Figures 13-15 It can be seen that the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 is applied to the metal lithium negative electrode of the lithium-sulfur battery, which significantly improves the cycle stability of the battery. When the current density is 0.1C, the initial discharge capacity of the lithium-sulfur battery with the metal lithium coated with the protective film as the negative electrode is 1165.3mAhg -1 , after 10 cycles, it is 978.8mAhg -1 , after 100 cycles, it is 730mAhg -1 The capacity retention rates are 84% and 63%, respectively, which are significantly better than the metal lithium negative electrode without protective film (74% and 47%). When the current density is 0.5C, the initial discharge capacity of the lithium-sulfur battery with the metal lithium coated with protective film as the negative electrode is 970.7mAhg -1 , after 300 cycles, it is 622.3mAhg -1 The capacity retention rate is 64%, which is better than the metal lithium negative electrode without protective film (54%).

[0128] Fig.16 : is a first rate characteristic graph, in which A is a rate characteristic curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and B is a rate characteristic curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0129] Fig.17 1 is a first rate characteristic graph, in which 1 is a rate characteristic curve of a lithium-sulfur battery prepared with a pure metal lithium sheet as the negative electrode in Comparative Example 6, and 2 is a rate characteristic curve of a lithium-sulfur battery prepared with a high-stability metal lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode in Example 5;

[0130] from Fig.16 , Fig.17It can be seen that the high-stability metal lithium electrode sheet coated with the composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 showed no obvious polarization at different current densities, showing good rate performance. The protective film was applied to the metal lithium negative electrode of the lithium-sulfur battery and also showed good rate performance. The battery had a capacity of 1164, 946.7, 807.2, 614.8, 425.4 mAh g at current densities of 0.1, 0.2, 0.5, 1, and 2C, respectively. -1 .

[0131] Fig.18 Figures are SEM images, where (a) and (b) are SEM images of a lithium-sulfur battery prepared with a pure metallic lithium sheet as the negative electrode in Comparative Example 6 after 10 cycles at 0.1C, and (c) and (d) are SEM images of a lithium-sulfur battery prepared with a high-stability metallic lithium electrode sheet coated with a composite protective film of lithiated naphthol and lithium carbonate prepared in Example 1 as the negative electrode after 10 cycles at 0.1C in Example 5.

[0132] from Fig.18 It can be seen that the composite protective film coated with lithiated naphthol and lithium carbonate prepared in Example 1 can effectively inhibit the growth of lithium dendrites and improve the cycle stability of the metal lithium negative electrode.

[0133] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An application of a mixed solution that can improve the stability of a metallic lithium negative electrode, characterized in that A mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode, and is specifically completed in the following steps: The mixed solution that can improve the stability of the metal lithium negative electrode is dripped on the surface of the lithium sheet and then dried to obtain a high-stability metal lithium electrode sheet coated with a composite protective film. The high-stability metal lithium electrode sheet coated with the composite protective film is used to assemble a symmetrical battery. The symmetrical battery has a current of 1 mA cm -2 , 1mAhcm -2 Under the following conditions, it can stably cycle for 800 hours; The assembly method of the symmetrical battery is as follows: A DOL / DME mixed solution is used as a solvent, wherein the volume ratio of DOL to DME is 1:1; LiTFSI and Li2S8 are used as solutes, and LiNO3 is used as an additive to obtain a polysulfide electrolyte; the concentration of LiTFSI in the polysulfide electrolyte is 1 mol / L, the concentration of Li2S8 is 2 mol / L, and the mass fraction of LiNO3 is 2%; Take 40 μL of polysulfide electrolyte, Celgard2400 as the separator, and high-stability metal lithium electrode sheets coated with composite protective film as electrodes, and assemble a symmetrical battery in an argon glove box; The method for preparing the high-stability metal lithium electrode sheet coated with the composite protective film is completed by the following steps:

1. Preparation of lithiated naphthol: 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol; 2. Preparation of mixed solution: 0.1 g of lithiated naphthol was dissolved in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; 5 mg of lithium carbonate was added to the organic solution of 10 g of lithiated naphthol, and stirred at a stirring speed of 500 r / min for 12 h to obtain a mixed solution that can improve the stability of the metal lithium negative electrode; 3. Drip coating electrode sheet: 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the lithium sheet was then dried at 60°C for 12 hours to obtain a high-stability metal lithium electrode sheet coated with a composite protective film.

2. An application of a mixed solution that can improve the stability of a metallic lithium negative electrode, characterized in that A mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode, and is specifically completed in the following steps: The mixed solution that can improve the stability of the metal lithium negative electrode is dripped on the surface of the lithium sheet and then dried to obtain a high-stability metal lithium electrode sheet coated with a composite protective film. The high-stability metal lithium electrode sheet coated with a composite protective film is used to assemble an asymmetric battery. The deposition capacity density of the asymmetric battery increases from 0.5 to 1 and then to 3 mAh cm -2 When , the morphology of lithium deposition is flat and uniform; The assembly method of the asymmetric battery is as follows: A DOL / DME mixed solution is used as a solvent, wherein the volume ratio of DOL to DME is 1:1; LiTFSI and Li2S8 are used as solutes, and LiNO3 is used as an additive to obtain a polysulfide electrolyte; the concentration of LiTFSI in the polysulfide electrolyte is 1 mol / L, the concentration of Li2S8 is 2 mol / L, and the mass fraction of LiNO3 is 2%; Take 40 μL of polysulfide electrolyte, use Celgard2400 as the separator, use pure metal lithium sheets and high-stability metal lithium electrode sheets coated with composite protective films as electrodes, and assemble an asymmetric battery in an argon glove box; The method for preparing the high-stability metal lithium electrode sheet coated with the composite protective film is completed by the following steps:

1. Preparation of lithiated naphthol: 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol; 2. Preparation of mixed solution: 0.1 g of lithiated naphthol was dissolved in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; 5 mg of lithium carbonate was added to the organic solution of 10 g of lithiated naphthol, and stirred at a stirring speed of 500 r / min for 12 h to obtain a mixed solution that can improve the stability of the metal lithium negative electrode; 3. Drip coating electrode sheet: 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the lithium sheet was then dried at 60°C for 12 hours to obtain a high-stability metal lithium electrode sheet coated with a composite protective film.

3. An application of a mixed solution for improving the stability of a metallic lithium negative electrode, characterized in that A mixed solution capable of improving the stability of a metal lithium negative electrode is used to improve the stability of a metal lithium negative electrode, and is specifically completed in the following steps: The mixed solution that can improve the stability of the metal lithium negative electrode is dripped onto the surface of the lithium sheet and then dried to obtain a high-stability metal lithium electrode sheet coated with a composite protective film. The high-stability metal lithium electrode sheet coated with the composite protective film is used as a negative electrode to assemble a lithium-sulfur battery. The capacity of the lithium-sulfur battery is 1164, 946.7, 807.2, 614.8, and 425.4 mAh g at current densities of 0.1, 0.2, 0.5, 1, and 2C, respectively. -1 ; The assembly method of the lithium-sulfur battery is: First, the mixed powder of activated carbon and sulfur powder was continuously heated at 155°C for 12 hours, and the mass ratio of activated carbon to sulfur powder was 3:

7. The mixed powder obtained after heating was mixed again with acetylene black and PVDF in a mass ratio of 8:1:1, and then NMP organic solvent was added, and stirred for 2 hours at room temperature to obtain a positive electrode slurry; the mixed positive electrode slurry was coated on the aluminum foil current collector using a coater and dried at 60°C for 12 hours; the dried sample was punched into a 13mm diameter disc using a puncher to obtain a positive electrode of a lithium-sulfur battery, and the obtained positive electrode surface loading was 1.3mgcm -2 ; The solute of the electrolyte used is bis(trifluoromethane)sulfonyl imide lithium salt, the solvent is a mixture of LiNO3, DOL and DME, the mass fraction of LiNO3 in the solvent is 2%, and the volume ratio of DOL and DME is 1:1; the concentration of bis(trifluoromethane)sulfonyl imide lithium salt in the electrolyte is 1 mol / L; Take 40 microliters of electrolyte, Celgard2400 as the separator, and a high-stability metal lithium electrode sheet coated with a composite protective film as the negative electrode, and assemble it with the positive electrode of the lithium-sulfur battery in an argon glove box to form a lithium-sulfur battery; The method for preparing the high-stability metal lithium electrode sheet coated with the composite protective film is completed by the following steps:

1. Preparation of lithiated naphthol: 12.75 mg of lithium hydroxide monohydrate is added to 5 mL of a 5% by mass naphthol aqueous solution, and then stirred at 60° C. for 2 hours to obtain a lithium hydroxide / naphthol aqueous solution; the lithium hydroxide / naphthol aqueous solution is dried at 80° C. for 12 hours to completely evaporate the water in the lithium hydroxide / naphthol aqueous solution to obtain lithiated naphthol; 2. Preparation of mixed solution: 0.1 g of lithiated naphthol was dissolved in 9.9 g of N-methylpyrrolidone to obtain an organic solution of lithiated naphthol; 5 mg of lithium carbonate was added to the organic solution of 10 g of lithiated naphthol, and stirred at a stirring speed of 500 r / min for 12 h to obtain a mixed solution that can improve the stability of the metal lithium negative electrode; 3. Drip coating electrode sheet: 50 μL of the mixed solution that can improve the stability of the metal lithium negative electrode was dropped on a 1.91 cm 2 The surface of the lithium sheet was then dried at 60°C for 12 hours to obtain a high-stability metal lithium electrode sheet coated with a composite protective film.