In-situ preparation and application of high-temperature-resistant polymer solid electrolyte
The high-temperature-resistant polymer solid electrolyte prepared through in-situ polymerization method solves the problem of easy decomposition of polymer solid electrolyte at high temperature, improves the cycle stability and safety of solid-state batteries, and achieves good electrochemical performance under high temperature conditions. .
Patent Information
- Application Number
- CN202410924952.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-01
AI Technical Summary
Polymer solid electrolytes are easily decomposed under high temperature conditions, leading to failure and safety issues of solid-state batteries. Existing technologies still have room for improvement in high-temperature cycle performance.
A solid-state battery is assembled by an in-situ polymerization method, using a high-temperature-resistant polymer solid electrolyte composed of component A, component B, component C, component D, and component E, including polymer monomers and additives with specific functional groups , stir and stand at room temperature to prepare a solid electrolyte with high thermal stability and improve the interface contact between the electrolyte and the electrode.
The stable cycle performance of solid-state batteries at high temperatures is achieved, and the safety and energy density of the battery are improved. The method is simple and no side reactions occur.
Smart Images

Figure CN118738542A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid-state batteries and relates to the in-situ preparation and application of a high-temperature resistant polymer solid electrolyte. Background Art
[0002] At present, with the increasing prominence of environmental problems and the continuous advancement of science and technology, lithium-ion batteries are widely used in portable electronic products, energy storage, aerospace and electric vehicle fields. However, traditional lithium-ion batteries use organic liquids as electrolytes, resulting in low energy density and poor safety of the battery. Using solid electrolytes instead of liquid electrolytes can be compatible with positive and negative electrodes with high specific capacity, which can improve the energy density and safety of the battery cell. Therefore, solid-state lithium batteries have attracted widespread attention. However, the interface contact between the solid electrolyte and the electrode is solid-solid contact, resulting in poor interface contact. At the same time, polymer solid electrolytes are easy to decompose under high temperature conditions, resulting in failure and safety problems of solid-state batteries. Therefore, the stable operation of polymer solid electrolytes under high temperature conditions is the difficulty of polymer solid-state battery technology.
[0003] In the prior art, CN106532116A discloses a method for preparing a high temperature resistant solid polymer electrolyte and its application in a lithium battery, wherein the polymer monomers used contain different functional groups and cannot react with each other. CN117239227A discloses an in-situ polymerized all-solid polymer electrolyte and its preparation method and application, characterized in that the polyacrylate monomer is at least one of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, and poly(ethylene glycol) methacrylate. However, the in-situ solid-state battery prepared by the above prior art still has room for improvement in high temperature cycle performance. Summary of the invention
[0004] The present invention is to assemble solid-state batteries through an in-situ polymerization method. The core is to prepare a polymer solid electrolyte with high thermal stability, thereby realizing stable circulation of the solid-state battery at high temperature, and providing in-situ preparation and application of high-temperature resistant polymer solid electrolytes.
[0005] The in-situ preparation and application of the high temperature resistant polymer solid electrolyte of the present invention is characterized in that the high temperature resistant solid electrolyte is composed of component A, component B, component C, component D and component E.
[0006] The component A is at least one of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate and butyl acrylate;
[0007] The component B is at least one of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate and butyl acrylate;
[0008] The component C is at least one of benzophenone, potassium persulfate, ammonium persulfate, azobisisobutyronitrile, azodicarbonamide, dicumyl peroxide, benzoyl peroxide and cyclohexanone peroxide;
[0009] The component D is at least one of lithium tetrafluoroborate, lithium perchlorate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium bistrifluoromethanesulfonyl amide, lithium bisfluorosulfonyl amide and lithium hexafluorophosphate;
[0010] The component E is at least one of malononitrile, succinonitrile, adiponitrile, suberonitrile, acetonitrile, ethylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, dimethyl carbonate and dioxolane.
[0011] The in-situ preparation of the high temperature resistant polymer solid electrolyte and the assembly of the solid state battery of the present invention are carried out according to the following steps:
[0012] 1. Preparation of high temperature resistant polymer material: Component A, component B and component C are mixed, stirred at room temperature for 1 min to 600 min, and after being mixed evenly, allowed to stand at 40° C. to 100° C. for 0.5 h to 100 h to obtain a component A-component B polymer material;
[0013] 2. Preparation method of high temperature resistant polymer solid electrolyte: Mix component A, component B and component C, stir for 1 min to 600 min at room temperature, then add component D and component E, stir for 1 min to 600 min at room temperature, and obtain a precursor solution of polymer solid electrolyte after mixing evenly. The precursor solution is allowed to stand at 40°C to 100°C for 0.5h to 100h to obtain a high temperature resistant polymer solid electrolyte.
[0014] 3. Application of high temperature resistant polymer solid electrolyte in solid-state batteries: Assemble the battery with the positive electrode sheet, diaphragm and lithium sheet in a glove box, inject the solid electrolyte precursor prepared in step 2 into the battery, soak the diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~100℃ for 0.5h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor is 2g / Ah~15g / Ah.
[0015] Beneficial effects of the present invention:
[0016] The present invention introduces the in-situ preparation of a high temperature resistant polymer solid electrolyte, thereby obtaining a polymer electrolyte with high thermal stability, and improving the cycle stability of a solid battery under high temperature conditions. The present invention involves mild chemical reaction conditions, simple methods, and no side reactions. The polymer solid electrolyte prepared by in-situ polymerization of the present invention has viscosity, which is beneficial to improving the interface contact between the solid electrolyte and the electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the cycle performance curve of the lithium iron phosphate solid-state battery at 120°C in Experiment 2; DETAILED DESCRIPTION
[0018] The present invention will be further described below with reference to embodiments and drawings, but the present invention is not limited to these embodiments.
[0019] Specific implementation method 1: A high temperature resistant in-situ polymerized solid electrolyte of the present invention is specifically composed of component A, component B, component C, component D and component E.
[0020] The component A is methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate or butyl acrylate;
[0021] The component B is methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate or butyl acrylate;
[0022] The component C is benzophenone, potassium persulfate, ammonium persulfate, azobisisobutyronitrile, azodicarbonamide, diisopropylbenzene peroxide, benzoyl peroxide and cyclohexanone peroxide;
[0023] The component D is lithium tetrafluoroborate, lithium perchlorate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium bistrifluoromethanesulfonamide, lithium bisfluorosulfonamide, lithium hexafluorophosphate or a mixture of two of them;
[0024] The component E is malononitrile, succinonitrile, adiponitrile, suberonitrile, acetonitrile, ethylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, dimethyl carbonate, dioxolane or a mixture of two of them.
[0025] Specific implementation method 2: This implementation method is the in-situ preparation of the high temperature resistant polymer solid electrolyte and the assembly of the solid state battery of specific implementation method 1, which is specifically carried out according to the following steps:
[0026] 1. Preparation of high temperature resistant polymer material: Component A, component B and component C are mixed, stirred at room temperature for 1 min to 600 min, and after being mixed evenly, allowed to stand at 40° C. to 100° C. for 0.5 h to 100 h to obtain a component A-component B polymer material;
[0027] 2. Preparation method of high temperature resistant polymer solid electrolyte: Mix component A, component B and component C, stir for 1 min to 600 min at room temperature, then add component D and component E, stir for 1 min to 600 min at room temperature, and obtain a precursor solution of polymer solid electrolyte after mixing evenly. The precursor solution is allowed to stand at 40°C to 100°C for 0.5h to 100h to obtain a high temperature resistant polymer solid electrolyte.
[0028] 3. Application of high temperature resistant polymer solid electrolyte in solid-state batteries: Assemble the positive electrode, diaphragm and negative electrode into a battery in a glove box, inject the solid electrolyte precursor prepared in step 2 into the battery, soak it on the PP diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~100℃ for 0.5h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor is 2g / Ah~15g / Ah.
[0029] Specific implementation method 3: This implementation method is different from specific implementation method 2 in that the mass ratio of component A to component B is 9:1 to 1:9. Other aspects are the same as those of specific implementation method 2.
[0030] Specific embodiment 4: This embodiment differs from specific embodiment 2 in that the mass ratio of the component C to the total mass of the components A and B is 1:1000 to 1:10. The rest is the same as specific embodiment 2.
[0031] Specific embodiment 5: This embodiment is different from specific embodiment 2 in that the molar concentration of component D in the precursor solution is (0.5 mol / L to 2 mol / L). Other aspects are the same as those of specific embodiment 2.
[0032] Specific embodiment 6: This embodiment is different from specific embodiment 2 in that the mass percentage of component E in the precursor solution is (5% to 50%). Other aspects are the same as specific embodiment 2.
[0033] Specific embodiment 7: This embodiment differs from specific embodiment 2 in that the separator used is a PE separator, a cellulose separator, a glass fiber separator, a polyimide separator, a polyacrylonitrile separator or a PE / PP / PE composite separator. The rest is the same as specific embodiment 2.
[0034] The present invention is verified by the following tests:
[0035] Experiment 1: This experiment is a method for preparing a precursor solution of a polymer solid electrolyte, which is specifically carried out in the following steps:
[0036] 1. Preparation of a precursor solution of a polymer solid electrolyte: Component A, component B and component C are mixed, the mass ratio of component A to component B is 9:1 to 1:9, the mass ratio of component C to the total mass of component A and component B is 1:1000 to 1:10, and stirred at room temperature for 1 min to 600 min, then component D and component E are added, the molar concentration of component D in the precursor solution is 2 mol / L, the mass percentage of component E in the precursor solution is 5%, stirred at room temperature for 1 min to 600 min, and mixed evenly to obtain a precursor solution of a polymer solid electrolyte.
[0037] Experiment 2: Using the precursor solution of the polymer solid electrolyte obtained in Experiment 1, an in-situ solid-state lithium iron phosphate battery was assembled and tested:
[0038] 1. Solid-state lithium iron phosphate battery assembly:
[0039] Lithium iron phosphate, conductive carbon material and adhesive were mixed in a mass ratio of 8:1:1, and added to N-methylpyrrolidone to form a uniform slurry. The slurry was applied to the current collector aluminum foil and dried in a vacuum oven at 100°C for 12 hours. The dried aluminum foil was then cut into discs and assembled with the diaphragm and lithium sheet. The polymer solid electrolyte precursor was then injected and packaged using a battery packaging machine. After standing at 40°C for 24 hours, a solid-state lithium iron phosphate battery was obtained for testing.
[0040] 2. Electrochemical performance test:
[0041] The constant current charge and discharge tester produced by Xinwei Company was used to carry out charge and discharge tests to measure the cycle performance curve of the solid-state lithium iron phosphate battery. The charge and discharge voltage range was 2.5V to 3.8V.
[0042] Figure 1 This is the cycle performance curve of the phosphoric acid battery in Experiment 2. As shown in the figure, the assembled lithium iron phosphate battery can be charged and discharged 100 times at 120°C.
[0043] The above data fully demonstrate that the solid electrolyte prepared in the present invention can be applied to high-temperature solid-state batteries, and the obtained solid-state batteries have good cycle performance.
[0044] It should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An in-situ preparation and application of a high temperature resistant polymer solid electrolyte, characterized in that The high temperature resistant solid electrolyte is composed of component A, component B, component C, component D and component E; The component A is at least one of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate and butyl acrylate; The component B is at least one of acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, 2-methoxyethyl methacrylate, 2-methoxyethyl acrylate, vinylene carbonate, vinylethylene carbonate, butyl methacrylate and butyl acrylate; The component C is at least one of benzophenone, potassium persulfate, ammonium persulfate, azobisisobutyronitrile, azodicarbonamide, dicumyl peroxide, benzoyl peroxide and cyclohexanone peroxide; The component D is at least one of lithium tetrafluoroborate, lithium perchlorate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium bistrifluoromethanesulfonyl amide, lithium bisfluorosulfonyl amide and lithium hexafluorophosphate; The component E is at least one of malononitrile, succinonitrile, adiponitrile, suberonitrile, acetonitrile, ethylene carbonate, fluoroethylene carbonate, ethylene glycol dimethyl ether, dimethyl carbonate and dioxolane.
2. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 1, characterized in that The in-situ preparation and application of a high temperature resistant polymer solid electrolyte is carried out according to the following steps:
1. Preparation of high temperature resistant polymer material: Component A, component B and component C are mixed, stirred at room temperature for 1 min to 600 min, and after being mixed evenly, allowed to stand at 40° C. to 100° C. for 0.5 h to 100 h to obtain a component A-component B polymer material; 2. Preparation method of high temperature resistant polymer solid electrolyte: Mix component A, component B and component C, stir for 1 min to 600 min at room temperature, then add component D and component E, stir for 1 min to 600 min at room temperature, and obtain a precursor solution of polymer solid electrolyte after mixing evenly. The precursor solution is allowed to stand at 40°C to 100°C for 0.5h to 100h to obtain a high temperature resistant polymer solid electrolyte.
3. Application of high temperature resistant polymer solid electrolyte in solid-state batteries: Assemble the positive electrode, diaphragm and negative electrode into a battery in a glove box, inject the solid electrolyte precursor prepared in step 2 into the battery, soak it on the diaphragm, and then use a battery packaging machine to package it. Let it stand at 40℃~100℃ for 0.5h~100h, and obtain a solid-state battery by in-situ polymerization, wherein the amount of solid electrolyte precursor is 2g / Ah~15g / Ah.
3. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 2, characterized in that The mass ratio of the component A to the component B is 9:1 to 1:
9.
4. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 2, characterized in that The mass ratio of the component C to the total mass of the components A and B is 1:1000 to 1:
10.
5. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 2, characterized in that The molar concentration of the component D in the precursor solution is (0.5 mol / L to 2 mol / L).
6. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 2, characterized in that The mass percentage of the component E in the precursor solution is (5% to 50%).
7. The in-situ preparation and application of a high temperature resistant polymer solid electrolyte according to claim 2, characterized in that The diaphragm used is a PE diaphragm, a PP diaphragm, a cellulose diaphragm, a glass fiber diaphragm, a polyimide diaphragm, a polyacrylonitrile diaphragm or a PE / PP / PE composite diaphragm.
8. Application of a high temperature resistant polymer solid electrolyte according to claim 2 in the field of solid state batteries.
9. The solid-state battery using a high-temperature resistant polymer solid electrolyte according to claim 2 can stably cycle at 30°C-120°C.