Preparation method and application of double-polymer composite quasi-solid electrolyte film

Through the preparation method of dual-polymer composite quasi-solid electrolyte films, the safety issues of pure liquid electrolytes in lithium-ion batteries and the problems of impurities on the surface of inorganic particles affecting interfacial compatibility are solved, achieving high stability and excellent ion transport performance. , improving the cycle life and conductivity of lithium-ion batteries.

CN118738543APending Publication Date: 2024-10-01HEFEI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411039380.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The pure liquid electrolyte of existing lithium-ion batteries is prone to leakage and internal short circuits, which poses safety problems. In addition, impurities on the surface of inorganic particles affect interfacial compatibility, resulting in poor electrochemical performance.

Method used

A method for preparing a dual-polymer composite quasi-solid electrolyte film is adopted, by ultrasonic treatment of inorganic nanoparticles LLZTO in an organic solvent, mixing polyvinylidene fluoride-chlorotrifluoroethylene copolymer and polyacrylonitrile, and adding bistrifluoromethanesulfonyl Lithium imide is used to form a uniform composite quasi-solid electrolyte slurry, and a thin film is obtained through vacuum drying to remove impurities on the surface of inorganic particles and form a highly stable interface.

Benefits of technology

It achieves high stability, high mechanical strength and excellent ion transmission performance, improves the cycle life and conductivity of lithium-ion batteries, and ensures the safety and performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738543A_ABST
    Figure CN118738543A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a double-polymer composite quasi-solid electrolyte film, and relates to the technical field of lithium ion battery preparation. The invention aims to solve the problems of poor chemical stability and poor electrochemical performance in the existing lithium battery. The method comprises the following steps: dispersing a certain amount of LLZTO powder in an organic solvent, and carrying out room-temperature ultrasonic treatment to obtain a uniform inorganic nanoparticle dispersion liquid; dispersing the PAN and the PVDF-CTFE in an organic solvent, and stirring until the PAN and the PVDF-CTFE are completely dissolved to form a uniform solution; pouring LITFSI and an LLZTO-containing dispersion liquid into the obtained double polymer solution, and fully stirring to obtain electrolyte slurry; and pouring the electrolyte slurry into a polytetrafluoroethylene mold, and carrying out vacuum drying to obtain the DP-L quasi-solid electrolyte. According to the invention, self-cleaning of the LLZTO surface and formation of a high-stability interface can be realized through a simple one-step compounding mode, and the cycling stability and safety of the lithium ion battery can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery preparation, and in particular to a preparation method and application of a double polymer composite quasi-solid electrolyte film. Background Art

[0002] With the rapid development of portable electronic devices and electric vehicle industries, higher demands are placed on advanced energy storage systems. In the field of secondary batteries, lithium-ion batteries with high energy density, long cycle life, high coulombic efficiency and high safety have become a hot research topic. Since pure liquid electrolytes are prone to leakage and internal short circuits, there are potential safety issues. Therefore, the research of solid electrolytes with advantages such as low flammability, high stability and inhibition of dendrite growth has become a top priority.

[0003] In order to improve the conductivity, mechanical strength and flexibility of the electrolyte, inorganic particles are introduced into the polymer electrolyte or flexible polymers are introduced into the inorganic electrolyte. The presence of inorganic fillers can promote the dissociation of lithium salts through surface Lewis acid sites, increase the concentration of free lithium ions, and further fix anions and increase the migration number of lithium ions. The presence of polymers can improve the flexibility of the electrolyte membrane to a certain extent. At the same time, the interface between the filler and the polymer can form a fast ion transport channel. However, the scattered distribution of inorganic particles makes it difficult to form a continuous structure, or the agglomeration of inorganic particles will destroy the conductive network. In addition, impurities are easily generated on the surface of LLZTO particles, which will affect the interface compatibility and lead to poor electrochemical performance.

[0004] Therefore, in order to construct a high-performance composite quasi-solid-state electrolyte, it is necessary to optimize the selected high-conductivity inorganic materials and rationally design a composite system with high-performance properties. Summary of the invention

[0005] The purpose of the present invention is to remove impurities on the surface of inorganic particles and form a highly stable interface phase on the surface of inorganic particles, thereby proposing a preparation method and application of a dual polymer composite quasi-solid electrolyte film.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a dual polymer composite quasi-solid electrolyte film comprises the following steps:

[0008] Step S1: adding inorganic nanoparticles (LLZTO) into an organic solvent and subjecting it to ultrasonic treatment at room temperature to obtain a uniform inorganic nanoparticle dispersion;

[0009] Step S2: dispersing polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE) and polyacrylonitrile (PAN) in an organic solvent, stirring until completely dissolved, to obtain a dual polymer solution;

[0010] Step S3: mixing the inorganic particle dispersion obtained in step S1 with the dual polymer solution obtained in step S2, adding lithium bis(trifluoromethanesulfonyl)imide (LITFSI), and stirring evenly to obtain a composite quasi-solid electrolyte slurry;

[0011] Step S4: pour the composite quasi-solid electrolyte slurry obtained in step S3 into a polytetrafluoroethylene mold, and vacuum dry it to finally obtain a dual-polymer composite quasi-solid electrolyte film.

[0012] As a further preferred technical solution of the present invention, in the preparation method:

[0013] The preparation method of the inorganic nanoparticles (LLZTO) in step S1 is:

[0014] First, La 2 O 3 Calcinated at 900 °C for 12 h, LiOH calcined at 200 °C for 12 h;

[0015] Then, weigh 0.55 g LiOH, 0.90 g La 2 O 3 , 0.34g ZrO 2 , 0.21g Ta 2 O 5 , mixed in a grinding jar, then added 4 g of isopropanol, and ball-milled at 400 rpm for 12 h to obtain a mixed slurry;

[0016] Next, the mixed slurry was placed on aluminum foil and dried in an oven at 55-60°C for 2-3 hours to obtain a powder;

[0017] Finally, the powder was calcined in a muffle furnace at 950°C for 6 h to obtain inorganic nanoparticles (LLZTO).

[0018] The organic solvent used in steps S1 and S2 is at least one of acetone, cyclohexanone, tetrahydrofuran, methanol, ethanol, butanone, N,N-dimethylformamide, chloroform, toluene, acetonitrile, and N-methylpyrrolidone (NMP).

[0019] In the composite quasi-solid electrolyte slurry prepared in step S3, the mass ratio of the inorganic nanoparticles (LLZTO), polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE), polyacrylonitrile (PAN), and lithium bis(trifluoromethanesulfonyl)imide (LITFSI) is 0.5-1.5:0.5-1.2:0.5-1.5:0.1-1, and the mass concentration of the inorganic nanoparticles (LLZTO) is 0.01-0.1 g / mL.

[0020] The vacuum drying temperature in step S4 is 50-90° C. and the drying time is 12-24 hours. The thickness of the prepared dual polymer composite quasi-solid electrolyte film is 20-100 μm.

[0021] The present invention also proposes a quasi-solid-state battery, comprising a positive electrode, a negative electrode and a prepared double polymer composite quasi-solid-state electrolyte film.

[0022] The advantages of the present invention over the prior art are:

[0023] The self-cleaning of the surface of lithium lanthanum zirconium oxide and the formation of a highly stable structure can be achieved through a simple one-time compound. The polymer polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE) is used to remove impurities Li on the surface of inorganic particles of lithium lanthanum zirconium oxide. 2 CO 3 At the same time, another polymer introduced, polyacrylonitrile (PAN), can interact strongly with the surface of lithium lanthanum zirconium oxide (LLZTO). While ensuring the presence of pure inorganic particles, an electrolyte with a highly stable structure is formed. In addition, the crystallinity of the dual polymer is reduced, the creep of the polymer chain is promoted, and ion transport is further promoted. The combination of high-conductivity LLZTO and polymers with high mechanical strength and high flexibility can not only solve the problem of low ionic conductivity of pure organic polymer electrolytes, but also greatly improve the mechanical properties of the composite electrolyte. In addition, the dual-polymer composite electrolyte prepared by the present invention can be stably cycled for more than 2000 hours by assembling a lithium metal symmetrical battery, and the ionic conductivity at room temperature can reach 0.221 to 0.443 mS cm -1 .

[0024] The beneficial effects of the present invention are specifically shown as follows:

[0025] (1) The dual polymer composite quasi-solid electrolyte film provided by the present invention has a flat surface, which can increase the interfacial compatibility with the electrode.

[0026] (2) The dual polymer composite quasi-solid electrolyte film provided by the present invention can be confirmed to function as a dual polymer through Fourier infrared testing and analysis.

[0027] (3) The dual polymer composite quasi-solid electrolyte film provided by the present invention has excellent flexibility, high mechanical strength, excellent thermal stability and high lithium ion migration number.

[0028] (4) The dual polymer composite quasi-solid electrolyte film provided by the present invention is used in a lithium iron phosphate (LiFePO 4 ) as the positive electrode and metallic lithium as the negative electrode, it has excellent cycle performance at room temperature and high capacity retention rate.

[0029] (5) The method for preparing the dual-polymer composite quasi-solid-state electrolyte film provided by the present invention has the advantages of simple process, short process cycle, low cost, etc., and can be widely used in lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of lithium lanthanum zirconium oxide particles prepared by a solid phase method in Example 1 of the present invention.

[0031] Figure 2 The SEM image (a) of the dual polymer composite quasi-solid electrolyte corresponding to Example 1 provided by the present invention, at 800-950cm -1 Fourier infrared test image (b), at 2200-2300cm -1 Fourier infrared test image (c).

[0032] Figure 3 The stress-strain curve (a), thermogravimetric test TGA graph (b), and rate test graph (c) at different current densities of the dual-polymer composite quasi-solid electrolyte film in Example 1 provided by the present invention are shown.

[0033] Figure 4 This is a cycle performance diagram of a lithium iron phosphate solid-state lithium battery prepared using the dual polymer composite quasi-solid electrolyte film in Example 1 provided by the present invention.

[0034] Figure 5 This is a cycle performance diagram of a lithium-lithium symmetrical battery prepared using the dual-polymer composite quasi-solid electrolyte film in Example 1 provided by the present invention.

[0035] Figure 6 The SEM image (a) of the corresponding single polymer composite quasi-solid electrolyte in Comparative Example 1 provided by the present invention, at 2200-2300cm -1 Fourier infrared test image (b).

[0036] Figure 7 The stress-strain curve (a), thermogravimetric test TGA graph (b), and rate test graph (c) at different current densities of the corresponding single polymer composite quasi-solid electrolyte in Comparative Example 1 provided by the present invention.

[0037] Figure 8 This is a cycle performance diagram of a lithium iron phosphate solid-state lithium battery prepared using the single polymer composite quasi-solid electrolyte film in Comparative Example 1 provided by the present invention.

[0038] Fig. 9 The SEM image (a) of the single polymer composite quasi-solid electrolyte corresponding to Comparative Example 2 provided by the present invention, 800-950cm -1 Fourier infrared test image (b).

[0039] Fig.10 The stress-strain curve (a), thermogravimetric test TGA graph (b), and rate test graph (c) at different current densities of the single polymer composite quasi-solid electrolyte corresponding to Comparative Example 2 provided by the present invention.

[0040] Fig.11 This is a cycle performance diagram of the corresponding single polymer composite quasi-solid electrolyte in Comparative Example 2 provided by the present invention.

[0041] Fig.12 The conductivity bar graph of the stainless steel symmetrical battery prepared by using Example 1, Comparative Example 1 and Comparative Example 2 provided by the present invention. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below in conjunction with embodiments and drawings.

[0043] Example 1

[0044] The preparation method of DP-L (dual polymer) composite quasi-solid electrolyte film is carried out according to the following steps:

[0045] 1. Preparation of inorganic Li particles 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO):

[0046] La before preparation 2 O 3 Calcinate at 900℃ for 12h, and calcine LiOH at 200℃ for 12h. 2 O 3 、ZrO 2 and Ta 2 O 5(Weigh 0.55g, 0.90g, 0.34g, 0.21g respectively) and mix in a grinding jar, add 4g isopropanol, and ball mill at 400rpm for 12h. Then put the mixed slurry on aluminum foil, put the obtained powder into an oven to dry (60℃, 3h), and then calcine in a muffle furnace at 950℃ for 6h. LLZTO nanoparticles are obtained.

[0047] 2. Preparation of DP-L (dual polymer) composite quasi-solid electrolyte film:

[0048] 0.3 g of LLZTO powder was weighed and dissolved in 2 mL of N,N-dimethylformamide and ultrasonically treated for 1 h to obtain an LLZTO dispersion; then 0.35 g of PAN and 0.32 g of PVDF-CTFE powder were weighed and dissolved in 6 mL of N,N-dimethylformamide and stirred to obtain a uniformly mixed polymer solution; then the ultrasonically dispersed LLZTO dispersion and 0.2 g of LITFSI were added to the mixed polymer solution and stirred at room temperature until uniform.

[0049] The uniform solution obtained in step 2 was cast on a polytetrafluoroethylene mold and vacuum dried at 65° C. for 12 h to obtain a DP-L composite quasi-solid electrolyte film.

[0050] The positive electrode (lithium iron phosphate), DP-L composite quasi-solid electrolyte film and lithium metal negative electrode are placed in the battery shell. After the battery is packaged, it is left to stand for 8 hours to obtain a DP-L composite quasi-solid-state battery.

[0051] Figure 1 is a scanning electron microscope (SEM) image of the inorganic particles prepared in Example 1; Figure 1 It can be seen that the particle size is small and uniform.

[0052] Figure 2 (a) is a surface SEM image of the DP-L electrolyte membrane prepared in Example 1, from which it can be seen that the inorganic particles are evenly dispersed in the dual polymer; Figure 2 (b) is the LLZTO and DP-L composite quasi-solid electrolyte in Example 1 at 800-950cm -1 Fourier infrared test shows that LLZTO is at 865cm -1 Existence 2 CO 3 When PAN and PVDF-CTFE act together, the impurity disappears, indicating that the impurity has a complex reaction with the polymer. Figure 2 (c) is the quasi-solid electrolyte of PAN and DP-L in Example 1 at 2200-2300 cm -1 Fourier infrared test, from the test results we can see that PAN is at 2243.3cm -1The -CN groups present at the DP-L electrolyte membrane were shifted, indicating that a strong interaction occurred between PAN and LLZTO or PVDF-CTFE.

[0053] Figure 3 (a) is the stress-strain performance of the DP-L electrolyte membrane tested in Example 1. It can be seen from the figure that the strain of the DP-L electrolyte can reach 160% and the stress can reach 16MPa. The excellent stress-strain capacity can cope with the volume expansion phenomenon of the battery; Figure 3 (b) is the thermogravimetric performance of the DP-L electrolyte membrane in Example 1. It can be seen from the figure that at a high temperature of 500°C, the DP-L electrolyte still has about 60% of the material remaining, and the thermal stability is very good; Figure 3 (c) is the rate performance tested on the DP-L electrolyte membrane in Example 1. It can be seen from the figure that the rate performance of the DP-L electrolyte is excellent.

[0054] Figure 4 This is the cycle performance of the DP-L electrolyte membrane in Example 1. It can be seen from the figure that after the DP-L electrolyte membrane is cycled 120 times at 0.5C and room temperature, the capacity still remains at 90.68%, and the long cycle performance is stable.

[0055] Figure 5 The DP-L electrolyte membrane in Example 1 is used to test the cycle performance of the lithium-lithium symmetric battery. From the figure, it can be seen that the cycle performance of the lithium-lithium symmetric battery assembled with the DP-L electrolyte is very stable.

[0056] Comparative Example 1

[0057] The preparation method of PAN-L (single polymer) composite quasi-solid electrolyte film is carried out according to the following steps:

[0058] 1. Preparation of inorganic Li particles 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO)

[0059] The preparation process of the inorganic particles is the same as that in Example 1.

[0060] 2. Preparation of PAN-L (single polymer) composite quasi-solid electrolyte film:

[0061] 0.3 g of LLZTO powder was weighed and dissolved in 2 mL of N,N-dimethylformamide and ultrasonically treated for 1 h to obtain a LLZTO dispersion; then 0.45 g of PAN was weighed and dissolved in 6 mL of N,N-dimethylformamide and stirred to obtain a uniformly mixed polymer solution; then the ultrasonically dispersed LLZTO dispersion and 0.2 g of LITFSI were added to the mixed polymer solution and stirred at room temperature until uniform.

[0062] The uniform solution obtained in step 2 was cast on a polytetrafluoroethylene mold and vacuum dried at 65° C. for 12 h to obtain a PAN-L composite quasi-solid electrolyte film.

[0063] The positive electrode (lithium iron phosphate), PAN-L composite quasi-solid-state electrolyte film and lithium metal negative electrode are placed in the battery shell. After the battery is packaged, it is left to stand for 8 hours to obtain a PAN-L composite quasi-solid-state battery.

[0064] Figure 6 (a) is a surface SEM image of the PAN-L electrolyte membrane prepared in Comparative Example 1, from which it can be seen that the inorganic particles are dispersed more evenly in the polymer; Figure 6 (b) is the quasi-solid electrolyte of PAN and PAN-L in Comparative Example 1 at 2200-2300 cm -1 Fourier infrared test shows that PAN is at 2243.3cm -1 The -CN group existing at the PAN-L electrolyte membrane was shifted, indicating that PAN and LLZTO had a strong interaction.

[0065] Figure 7 (a) is the stress-strain performance of the PAN-L electrolyte membrane prepared in Example 1. It can be seen from the figure that the strain of the PAN-L electrolyte can only reach 40% and the stress can reach 18MPa. The excellent stress capacity is not enough to cope with the volume expansion phenomenon of the battery; Figure 7 (b) is the thermogravimetric performance of the PAN-L electrolyte membrane in Example 1. It can be seen from the figure that the PAN-L electrolyte has about 60% of the material remaining at a high temperature of 400°C. Figure 7 (c) is the rate performance of the PAN-L electrolyte membrane tested in Example 1. It can be seen from the figure that the rate performance of PAN-L electrolyte is excellent before the current density of 1C, and the capacity decays rapidly at 2C.

[0066] Figure 8 This is the cycle performance of the PAN-L electrolyte membrane tested in Example 1. It can be seen that the capacity of the electrolyte membrane decays quickly. After 120 cycles at 0.5C and room temperature, the capacity remains only 23.22%, and the long cycle performance is poor.

[0067] Comparative Example 2

[0068] The preparation method of PC-L (single polymer) composite quasi-solid electrolyte film is carried out according to the following steps:

[0069] 1. Preparation of inorganic Li particles 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO):

[0070] The preparation process of the inorganic particles is the same as that in Example 1.

[0071] 2. Preparation of PC-L (single polymer) composite quasi-solid electrolyte film:

[0072] 0.3 g of LLZTO powder was weighed and dissolved in 2 mL of N,N-dimethylformamide and ultrasonically treated for 1 h to obtain a LLZTO dispersion; then 0.45 g of PVDF-CTFE was weighed and dissolved in 6 mL of N,N-dimethylformamide and stirred to obtain a uniformly mixed polymer solution; then the ultrasonically dispersed LLZTO dispersion and 0.2 g of LITFSI were added to the mixed polymer solution and stirred at room temperature until uniform.

[0073] The uniform solution obtained in step 2 was cast on a polytetrafluoroethylene mold and vacuum dried at 65° C. for 12 h to obtain a PC-L composite quasi-solid electrolyte film.

[0074] The positive electrode (lithium iron phosphate), PC-L composite quasi-solid electrolyte film and lithium metal negative electrode are placed in the battery shell. After the battery is packaged, it is left to stand for 8 hours to obtain a PC-L composite quasi-solid-state battery.

[0075] Fig. 9 (a) is a surface SEM image of the PC-L electrolyte membrane prepared in Comparative Example 2. It can be seen from the image that the inorganic particles are agglomerated in the polymer and the surface of the composite electrolyte membrane is uneven; Fig. 9 (b) is the quasi-solid electrolyte of LLZTO and PC-L in Comparative Example 2 at 800-950 cm -1 Fourier infrared test shows that LLZTO is at 865cm -1 Existence 2 CO 3 When PVDF-CTFE and LLZTO work together, Li 2 CO 3 The impurity disappeared, indicating that the impurity reacted with PVDF-CTFE.

[0076] Fig.10(a) is the stress-strain performance of the PC-L electrolyte membrane prepared in Example 2. It can be seen from the figure that the strain of the PC-L electrolyte can reach 170% and the stress can reach 16MPa. The excellent stress capacity is sufficient to cope with the volume expansion phenomenon of the battery; Fig.10 (b) is the thermogravimetric performance of the PC-L electrolyte membrane in Example 2. It can be seen from the figure that the PC-L electrolyte has about 60% of the material remaining at a high temperature of 300°C, and the thermal stability is poor; Fig.10 (c) is the rate performance of the PC-L electrolyte membrane tested in Example 2. It can be seen from the figure that the rate performance of the PC-L electrolyte is poor and the capacity decay is fast.

[0077] Fig.11 This is the cycle performance of the PC-L electrolyte membrane in Example 2. It can be seen that the capacity of the electrolyte membrane is relatively stable. After 120 cycles at 0.5C and room temperature, the remaining capacity is 84.9%.

[0078] Fig.12 The conductivity bar graph of the stainless steel symmetrical batteries prepared by using Example 1, Comparative Example 1 and Comparative Example 2 provided by the present invention is shown. It can be seen from the graph that compared with Comparative Example 1 and Comparative Example 2, the conductivity of Example 1 is the highest.

[0079] By comparing Example 1 with Comparative Examples 1 and 2, it can be found that compared with the use of a single polymer, the present invention uses a polymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE), to remove impurities Li on the surface of inorganic particles of lithium lanthanum zirconium oxide. 2 CO 3 At the same time, another polymer introduced, polyacrylonitrile (PAN), can interact strongly with the surface of lithium lanthanum zirconium oxide (LLZTO), thereby ensuring the formation of an electrolyte with a highly stable structure and strong electrochemical properties while having pure inorganic particles.

[0080] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a dual polymer composite quasi-solid electrolyte film, characterized in that: The following steps are involved: Step S1: adding inorganic nanoparticles (LLZTO) into an organic solvent and subjecting it to ultrasonic treatment at room temperature to obtain a uniform inorganic nanoparticle dispersion; Step S2: dispersing polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE) and polyacrylonitrile (PAN) in an organic solvent, stirring until completely dissolved, to obtain a dual polymer solution; Step S3: mixing the inorganic particle dispersion obtained in step S1 with the dual polymer solution obtained in step S2, adding lithium bis(trifluoromethanesulfonyl)imide (LITFSI), and stirring evenly to obtain a composite quasi-solid electrolyte slurry; Step S4: pour the composite quasi-solid electrolyte slurry obtained in step S3 into a polytetrafluoroethylene mold, and vacuum dry it to finally obtain a dual-polymer composite quasi-solid electrolyte film.

2. The preparation method according to claim 1, characterized in that The preparation method of the inorganic nanoparticles (LLZTO) in step S1 is: First, La2O3 was calcined at 900℃ for 12h, and LiOH was calcined at 200℃ for 12h; Then, 0.55 g LiOH, 0.90 g La2O3, 0.34 g ZrO2, and 0.21 g Ta2O5 were weighed and mixed in a grinding jar, and 4 g isopropanol was added, and the mixture was ball-milled at 400 rpm for 12 h to obtain a mixed slurry; Next, the mixed slurry was placed on aluminum foil and dried in an oven at 55-60°C for 2-3 hours to obtain a powder; Finally, the powder was calcined in a muffle furnace at 950°C for 6 h to obtain inorganic nanoparticles (LLZTO).

3. The preparation method according to claim 1, characterized in that: The organic solvent used in steps S1 and S2 is at least one of acetone, cyclohexanone, tetrahydrofuran, methanol, ethanol, butanone, N,N-dimethylformamide, chloroform, toluene, acetonitrile, and N-methylpyrrolidone (NMP).

4. The preparation method according to claim 1, characterized in that: In the composite quasi-solid electrolyte slurry prepared in step S3, the mass ratio of the inorganic nanoparticles (LLZTO), polyvinylidene fluoride-chlorotrifluoroethylene copolymer (PVDF-CTFE), polyacrylonitrile (PAN), and lithium bis(trifluoromethanesulfonyl)imide (LITFSI) is 0.5-1.5:0.5-1.2:0.5-1.5:0.1-1, and the mass concentration of the inorganic nanoparticles (LLZTO) is 0.01-0.1 g / mL.

5. The preparation method according to claim 1, characterized in that: In step S4, the vacuum drying temperature is 50-90° C., and the drying time is 12-24 hours.

6. The preparation method according to claim 1, characterized in that: The thickness of the dual polymer composite quasi-solid electrolyte film prepared in step S4 is 20 to 100 μm.

7. A quasi-solid-state battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a double polymer composite quasi-solid electrolyte film prepared by the method according to any one of claims 1 to 6.

Citation Information

Cited By

  • Inorganic-organic composite solid electrolyte and preparation method thereof

    CN119400935A