Composite additive, electrolyte and lithium ion battery
By using composite additives to form a stable interfacial film in lithium-ion batteries, the problem of lithium salt thermal decomposition at high temperatures in lithium-ion batteries is solved, the lithium-ion migration rate and battery capacity are improved, the expansion rate is reduced, and the safety and high-temperature performance of the battery are enhanced.
Patent Information
- Application Number
- CN202410683771.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-30
AI Technical Summary
Under high-temperature conditions, lithium salts in the electrolyte of lithium-ion batteries undergo thermal decomposition due to the active hydrogen, resulting in side reactions that damage the electrode material structure, reduce the lithium-ion migration rate, decrease battery capacity, and generate a large amount of gas, affecting battery performance, lifespan, and safety.
Composite additives, including compounds shown in Structural Formula I and Structural Formula II, are used to form a thin and stable interfacial film, remove byproducts on the positive and negative electrode surfaces, improve the ionic conductivity of the interfacial film, and prevent the thermal decomposition of lithium salts at high temperatures. By generating CEI and SEI protective films on the NCM cathode and graphite anode surfaces, the battery impedance is reduced.
Under high temperature conditions, lithium-ion batteries exhibit high lithium-ion migration rate, high battery capacity retention, low expansion rate, and high safety, as well as excellent high-temperature cycling and storage performance.
Smart Images

Figure BDA0004866313270000021 
Figure BDA0004866313270000022 
Figure BDA0004866313270000031
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a composite additive, an electrolyte and a lithium ion battery. Background Art
[0002] In recent years, lithium-ion batteries have received extensive attention in hybrid vehicles and mobile device power supplies due to their high energy density, environmental friendliness and economy, and have become a new research hotspot.
[0003] However, when lithium-ion batteries are placed under high temperature conditions, the lithium salt in the electrolyte will undergo thermal decomposition due to the active hydrogen. The decomposition products will trigger side reactions, destroy the structure of the electrode material, lead to a decrease in the lithium ion migration rate, and reduce the battery capacity. In addition, the decomposition will produce a large amount of gas, causing the battery to swell, thus affecting the performance, life and safety of the lithium-ion battery. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a composite additive, an electrolyte and a lithium ion battery, which solve the technical problem that the electrolyte of the lithium ion battery will undergo thermal decomposition of active hydrogen to produce by-products and a large amount of gas under high temperature conditions.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] In one aspect, the present invention provides a composite additive, wherein the composite additive comprises compounds represented by structural formula I and structural formula II.
[0009]
[0010] The mass ratio of the compound represented by structural formula I to the compound represented by structural formula II is 1:5-5:1;
[0011] The compound represented by the structural formula I, R 1 is a halogenated hydrocarbon, the compound shown in structural formula II, R 2 One or two selected from methoxy and halogen elements.
[0012] As a preferred embodiment, the compound represented by the structural formula I is selected from compound 1,
[0013]
[0014] As a preferred embodiment, in order to further give full play to the synergistic effect of formula I and formula II, the compound represented by structural formula II is selected from one or both of compound 2 and compound 3.
[0015]
[0016] On the other hand, the present invention provides an electrolyte comprising a lithium salt, an organic solvent and the composite additive, wherein the addition amount of the composite additive is 0.1-3wt% of the total mass of the electrolyte.
[0017] As a preferred embodiment, the organic solvent includes any one or more of cyclic carbonate, chain carbonate and carboxylic acid ester.
[0018] As a preferred embodiment, the cyclic carbonate is selected from one or more of ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone;
[0019] The chain carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate;
[0020] The carboxylic acid ester is selected from one or more of methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate and ethyl butyrate.
[0021] As a preferred embodiment, the electrolyte further comprises conventional additives, the addition amount of the conventional additives is 0.5-3wt% of the total mass of the electrolyte, and the conventional additives are selected from lithium bis(fluorosulfonyl)imide salt, LiBF 4 , any one or more of lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(trifluoromethylsulfonyl)imide, phenyl sulfone, tris(trimethylsilyl)phosphite, vinyl sulfate, and methylene disulfonate.
[0022] On the other hand, the present invention provides a lithium ion battery, comprising a negative electrode sheet, a positive electrode sheet, a separator disposed between the negative electrode sheet and the positive electrode sheet, and the electrolyte.
[0023] As a preferred embodiment, the positive electrode sheet includes a positive electrode material, and the positive electrode material is LiNi (1-x-y) Co x Mn y O 2 , wherein 0≤X≤1, 0≤Y≤1, the negative electrode sheet comprises a negative electrode material, and the negative electrode material is graphite.
[0024] As a preferred embodiment, the charging voltage of the lithium-ion battery is no higher than 4.8V.
[0025] (III) Beneficial effects
[0026] The present invention provides a composite additive, an electrolyte and a lithium ion battery. Compared with the prior art, the composite additive has the following beneficial effects:
[0027] The composite additive of the present invention can not only form a thin and stable interface film on the surface of the high-nickel NCM positive electrode and negative electrode graphite, but also remove by-products on the surface of the positive and negative electrode materials, greatly improving the ion conductivity of the interface film, and can prevent the lithium salt in the electrolyte from being thermally decomposed due to active hydrogen at high temperature. Therefore, the lithium ion battery prepared by the present invention has a high lithium ion migration rate under high temperature conditions, a high battery capacity, a low battery expansion rate, high safety, and excellent high-temperature cycle and high-temperature shelf storage performance. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The embodiments of the present application provide a composite additive, an electrolyte and a lithium-ion battery, thereby solving the technical problem that the electrolyte of a lithium-ion battery decomposes under high temperature conditions to produce by-products and a large amount of gas.
[0030] The technical solution in the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:
[0031] The present application provides an electrolyte, which includes a lithium salt, an organic solvent, a composite additive and a conventional additive.
[0032] The composite additive includes compounds shown in structural formula I and structural formula II. The compound shown in structural formula I contains a cyano group. Cyanide substances have a high dielectric constant and a low viscosity. The strongly electronegative cyanide group can form a CN-Co bond with the surface of the NCM metal oxide, inhibiting the direct contact of the electrolyte with the positive electrode, thereby improving the stability of the positive electrode interface. At the same time, the cyanide group has a strong electrophilic activity and can react with the water in the electrolyte and the active hydrogen in the positive and negative electrode materials to reduce the decomposition of lithium salts caused by active hydrogen under high temperature conditions.
[0033] The compound shown in the structural formula II contains a CF bond, which is easy to break, and is easy to generate LiF (the main component of the SEI film), and has good thermal stability. The compound shown in the structural formula II contains a silicon base, which is an electron-donating group, has a large electron cloud density, reduces the oxidation potential, and is easy to form a positive electrode film, thereby avoiding direct contact between the electrode and the electrolyte at high temperature, and can also delay the high-temperature oxidation decomposition reaction of the electrolyte. Therefore, the synergistic effect of the compounds shown in the structural formula I and the structural formula II in the composite additive is not only easy to generate a thinner and denser CEI and SEI protective film on the surface of the NCM cathode and the graphite anode, but also removes the residual lithium compounds on the surface of the positive and negative electrodes, improves the ion conductivity of the interface film, and can avoid the thermal decomposition of the lithium salt in the electrolyte due to active hydrogen at high temperature. Therefore, the lithium ion migration rate of the lithium ion battery of the present invention is high under high temperature conditions, the battery capacity retention rate is high, the battery expansion rate is low, the safety and recovery rate are high, and the high-temperature cycle and high-temperature storage performance are excellent.
[0034] The CEI and SEI protective films generated by the positive and negative electrodes are dynamic and will rupture and regenerate. The ruptured film components become the lithium compounds remaining on the surfaces of the positive and negative electrodes. The compounds shown in structural formula I and structural formula II in the composite additive of the present application work synergistically to remove the lithium compounds remaining on the surfaces of the positive and negative electrodes, thereby reducing the impedance of the battery.
[0035] Lithium ions and solvents are consumed in the process of rupture and regeneration of CEI and SEI protective films. The compounds represented by structural formula I and structural formula II in the composite additive of the present application cooperate with each other to form thinner and denser CEI and SEI protective films on the surfaces of NCM cathode and graphite anode, which are not easy to rupture, thereby reducing the consumption of active lithium.
[0036] In a further preferred embodiment, the conventional additives include lithium bis(fluorosulfonyl)imide salt, LiBF 4 , lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(trifluoromethylsulfonyl)imide, phenyl sulfone, tris(trimethylsilyl)phosphite, vinyl sulfate, methylene disulfonate, vinyl carbonate, methylene disulfonate, and fluoroethylene carbonate.
[0037] More preferably, the content of conventional additives in the electrolyte is 0.5-3wt%, for example, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%.
[0038] In consideration of selecting a lithium salt that is more compatible with the above-mentioned additives, in a preferred embodiment, the lithium salt in the electrolyte is selected from one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalate borate), lithium difluorooxalate borate, lithium difluorooxalate phosphate, lithium bis(fluorosulfonyl)imide salt or lithium bis(trifluoromethylsulfonyl)imide. And the molar concentration of the lithium salt is 0.5-1.5M, for example, it can be 0.5M, 0.75M, 1M, 1.25M or 1.5M. The molar concentration of the lithium salt is limited to the above range, so that the battery can take into account both the better electrochemical performance and the room temperature cycle retention rate.
[0039] In a preferred embodiment, the organic solvent is one or more of a chain carbonate compound, a cyclic carbonate compound or a carboxylate compound. The cyclic carbonate compound is selected from one or more of ethylene carbonate, fluoroethylene carbonate or propylene carbonate; the chain carbonate compound is selected from one or more of dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; the carboxylate compound is selected from propyl acetate and / or ethyl acetate. The above additives are more compatible with this type of organic solvent, based on which the battery can have both better electrochemical performance and capacity retention.
[0040] In a preferred embodiment, the above-mentioned electrolyte can be prepared by the following preparation method: first add lithium salt to an organic solvent, and after the lithium salt is completely dissolved, add additives to the system to obtain the above-mentioned electrolyte, so the electrolyte obtained in this application has better performance uniformity.
[0041] The present invention also provides a lithium ion battery, which includes a negative electrode sheet, a positive electrode sheet and an electrolyte, wherein the material of the positive electrode sheet is LiNi (1-x-y) Co x Mn y O 2 , the negative electrode sheet is made of graphite, and the electrolyte is the aforementioned electrolyte. Based on the above reasons, the lithium-ion battery of the present application has excellent capacity retention and capacity recovery. In a preferred embodiment, the charging voltage of the lithium-ion battery is not higher than 4.8V, preferably 2.8-4.25V.
[0042] The composite additive and electrolyte of the present invention can form a thin and stable interface film on the surface of high-nickel positive electrode and negative electrode graphite, effectively isolating the electrolytes, and at the same time have the functions of dewatering, acid reduction or complexation, greatly improving the conductivity of the interface film.
[0043] The beneficial technical effects of the present application will be described below in combination with specific embodiments and comparative examples.
[0044] The compounds of structural formula I and structural formula II were purchased from the official website of Aladdin Reagents.
[0045] Example 1
[0046] This embodiment provides a method for preparing a lithium ion battery, comprising the following steps:
[0047] S1. Preparation of electrolyte:
[0048] Ethylene carbonate (EC), ethyl propionate (EP) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of EC:EP:EMC=1:1:2, and 0.7 mol of lithium hexafluorophosphate (LiPF 6 ), 0.3 mol of lithium bis(fluorosulfonyl)imide (LiFSI), after the lithium salt is completely dissolved, add compound 1 (CAS: 27328-86-5) and compound 2 (CAS: 866252-52-0), the mass ratio of compound 1 to compound 2 is 2:1, and the addition amount of compound 1 and compound 2 is 3%wt of the total mass of the electrolyte.
[0049] S2. Preparation of positive electrode: LiNi 0.7 C0 0.1 Mn 0.2 , conductive agent Super P, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 97.5:0.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector, and the coating amount is 360g / m 2 , dried at 85°C and then cold pressed; then striped and sliced, and then baked at 85°C in vacuum for 4 hours to make a lithium-ion battery positive electrode that meets the requirements.
[0050] S3. Preparation of negative electrode sheet: artificial graphite, conductive agent Super P, thickener CMC, and adhesive SBR (styrene-butadiene rubber latex) are prepared into slurry in a mass ratio of 95:1.5:1.0:2.5, and mixed evenly. The mixed slurry is applied on both sides of the copper foil, and then dried and rolled to obtain the negative electrode sheet, which is then baked at 85°C in vacuum for 4 hours to obtain a lithium-ion battery negative electrode sheet that meets the requirements.
[0051] S4. Preparation of lithium-ion batteries: The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are laminated to form a lithium-ion battery with a thickness of 0.5 mm, a width of 8 mm and a length of 10 mm, and a capacity of 3 Ah. The battery is vacuum-baked at 85°C for 48 hours, and the above electrolyte is injected to complete the battery production.
[0052] In Examples 2 to 11 and Comparative Examples 1 to 6, the ratio and type of specific substances in the electrolyte were changed, and the other aspects were the same as in Example 1, to prepare lithium-ion batteries, and the electrolyte formulas were as shown in Table 1.
[0053] Table 1 Electrolyte composition and battery performance of the embodiments and comparative examples
[0054]
[0055]
[0056] The composite additive of the present invention can improve the high-temperature comprehensive performance of the battery, and the high-temperature comprehensive performance is mainly manifested in two major electrical properties: high-temperature cycling and high-temperature storage performance. From Table 1, by comparing the 60°C storage 28D retention rate and 45°C cycle 800 cycle retention rate of the battery prepared in Example 1-11 with that in Comparative Example 1-6, it can be seen that the 60°C storage 28D retention rate and 45°C cycle 800 cycle retention rate of the battery prepared in Example 1-11 are greater. This is because the introduction of the composite additive makes the positive and negative electrode film formation more dense and stable, reduces the interface impedance of the positive and negative electrodes, and can remove byproducts on the surface of the positive and negative electrodes, improve the ionic conductivity of the interface film, and greatly improve the high-temperature performance of the battery.
[0057] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0058] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention is described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. Anything not described in detail in the present invention is a well-known technology to those skilled in the art.
Claims
1. A composite additive, characterized in that: The composite additive comprises compounds shown in structural formula I and structural formula II, The mass ratio of the compound represented by structural formula I to the compound represented by structural formula II is 1:5-5:1; In the compound represented by structural formula I, R1 is a halogenated hydrocarbon, and in the compound represented by structural formula II, R2 is selected from one or two of methoxy and halogen.
2. The composite additive according to claim 1, characterized in that The compound represented by the structural formula I is selected from compound 1, 3. The composite additive according to claim 1, characterized in that The compound represented by structural formula II is selected from one or both of compound 2 and compound 3, 4. An electrolyte, characterized in that: The invention comprises a lithium salt, an organic solvent and the composite additive according to any one of claims 1 to 3, wherein the addition amount of the composite additive is 0.1-3wt% of the total mass of the electrolyte.
5. The electrolyte according to claim 4, characterized in that The organic solvent includes any one or more of cyclic carbonate, chain carbonate and carboxylic acid ester.
6. The electrolyte according to claim 5, characterized in that The cyclic carbonate is selected from one or more of ethylene carbonate, propylene carbonate, butylene carbonate, and γ-butyrolactone; The chain carbonate is selected from one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, and ethyl propyl carbonate; The carboxylic acid ester is selected from one or more of methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate and ethyl butyrate.
7. The electrolyte according to claim 4, characterized in that The electrolyte also includes conventional additives, the addition amount of the conventional additives is 0.5-3wt% of the total mass of the electrolyte, and the conventional additives are selected from any one or more of bis(trifluoromethylsulfonyl)imide lithium salt, LiBF4, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorooxalatophosphate, lithium bis(trifluoromethylsulfonyl)imide, phenyl sulfone, tris(trimethylsilyl)phosphite, vinyl sulfate, and methylene disulfonate.
8. A lithium ion battery, characterized in that: The invention comprises a negative electrode sheet, a positive electrode sheet, a separator arranged between the negative electrode sheet and the positive electrode sheet, and the electrolyte according to any one of claims 4 to 7.
9. The lithium ion battery according to claim 8, characterized in that The positive electrode sheet includes a positive electrode material, and the positive electrode material is LiNi (1-x-y) Co x Mn y O2, wherein 0≤X≤1, 0≤Y≤1, the negative electrode sheet comprises a negative electrode material, and the negative electrode material is graphite.
10. The lithium ion battery according to claim 8, characterized in that The charging voltage of the lithium-ion battery is no higher than 4.8V.
Citation Information
Patent Citations
Nonaqueous electrolyte solution, electricity storage device using same, and trifluoromethylbenzene compound
CN103493277A
Electrolyte solution for nonaqueous electrolyte batteries, and nonaqueous electrolyte battery using same
CN108140891A
Additive for lithium ion battery electrolyte, lithium ion battery electrolyte and lithium ion battery containing electrolyte
CN114400378A
Lithium ion secondary battery
JP2015125949A
Electrolyte and lithium ion battery
WO2024104049A1
Cited By
Electrolyte combined additive, electrolyte and lithium ion battery
CN119481276A