Electrolyte and lithium ion battery

By adding cyclic sulfate ester compounds and boron-containing lithium salt compounds to the lithium-ion battery electrolyte, a stable and dense CEI film is formed, which solves the problems of cycle life and storage performance of lithium-ion batteries at high temperatures and high voltages, and achieves for more efficient lithium-ion transmission and battery stability.

CN118738559APending Publication Date: 2024-10-01SHENZHEN HIGHPOWER TECH CO LTD

Patent Information

Application Number
CN202411053139.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the energy density and cycle life of existing lithium-ion batteries are increased, the increase in the cut-off voltage of transition metal oxides leads to cracking of the CEI membrane, electrolyte penetration and side reactions, deteriorating the cycle life and high-temperature storage performance of the battery.

Method used

Add cyclic sulfate compounds and boron-containing lithium salt compounds as additives to the electrolyte to form a dense and chemically stable CEI film, inhibit the thermodynamic corrosion reaction and co-intercalation reaction of solvent molecules, and reduce the number of positive and negative electrode materials and electrolyte. The loss of medium-active lithium improves high-temperature cycling and high-temperature storage performance.

Benefits of technology

It effectively improves the cycle capacity retention rate and high-temperature cycle performance of lithium-ion batteries, extends the cycle life of the battery, improves high-temperature storage and high-temperature cycle performance, while maintaining good low-temperature discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977052130000021
    Figure BDA0004977052130000021
  • Figure BDA0004977052130000022
    Figure BDA0004977052130000022
  • Figure BDA0004977052130000061
    Figure BDA0004977052130000061
Patent Text Reader

Abstract

The invention relates to an electrolyte and a lithium ion battery. The electrolyte comprises an additive I and an additive II, the additive I is a cyclic sulfate compound, and the additive II is a boron-containing lithium salt compound; wherein the mass percentage content of the additive I in the electrolyte is A%, the mass percentage content of the additive II in the electrolyte is B%, and A / B is larger than or equal to 0.2 and smaller than or equal to 10. According to the technical scheme, a CEI film with high density and good chemical stability can be formed on a positive electrode interface, thermodynamic corrosion reaction, co-intercalation reaction and the like of solvent molecules are inhibited, the loss of active lithium in positive and negative electrode materials and electrolyte in the cycle process is effectively reduced, and the high-temperature cycle and high-temperature storage performance of the lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to an electrolyte and a lithium-ion battery. Background Art

[0002] Lithium-ion battery refers to a secondary battery that relies on the movement of lithium ions between the positive and negative electrodes to achieve charging and discharging purposes. It has the advantages of high energy density, fast charging speed and high safety. It is widely used in energy storage devices for various electronic products, electric vehicles, etc.

[0003] The main components of lithium-ion batteries include positive electrode plates, negative electrode plates, separators and electrolytes. Among them, the electrolyte, as an important component of lithium-ion batteries, plays the role of transferring charge between the positive and negative electrodes in the lithium-ion battery system. During the first charge and discharge process of the battery, the electrolyte components and the electrodes undergo redox reactions at the liquid-solid interface, and the reaction products accumulate at the electrode interface to form a passivation layer, that is, a solid electrolyte interface SEI film can be formed on the negative electrode surface, and a positive electrode electrolyte interface CEI film can be formed on the positive electrode surface.

[0004] With the increasing demand for electronic products and the increasing requirements for the endurance of electric vehicles, the energy density requirements for lithium-ion batteries are also increasing. Currently, the discharge capacity and energy density can be increased by 15% to 35% by increasing the cutoff voltage of the transition metal oxide positive electrode, for example, to 4.5V or above. However, in these transition metal oxides, more Li insertion / extraction increases the electrode volume change, causing the CEI membrane to crack, and then the electrolyte will penetrate into the cracked transition metal oxide and react with it. The continuous side reaction of the transition metal oxide and the electrolyte will cause rapid capacity decay and deteriorate the cycle life of the battery. Summary of the invention

[0005] In order to solve or partially solve the problems existing in the related technology, the present application provides an electrolyte and a lithium-ion battery, which can form a CEI film with high density and good chemical stability at the positive electrode interface, inhibit the thermodynamic corrosion reaction and co-embedding reaction of solvent molecules, effectively reduce the loss of positive and negative electrode materials and active lithium in the electrolyte during the cycle process, and improve the high-temperature cycle and high-temperature storage performance of lithium-ion batteries.

[0006] In a first aspect, the present application provides an electrolyte, comprising an additive I and an additive II, wherein the additive I is a cyclic sulfate ester compound, and the additive II is a boron-containing lithium salt compound;

[0007] Wherein, the mass percentage of the additive I in the electrolyte is A%, the mass percentage of the additive II in the electrolyte is B%, and 0.2≤A / B≤10.

[0008] In some optional embodiments, the additive I is selected from at least one of the following compounds:

[0009]

[0010] In some optional embodiments, the additive II is selected from at least one of the following compounds:

[0011]

[0012] In some optional embodiments, the mass percentage A of the additive I in the electrolyte satisfies: 0.5%≤A%≤5%.

[0013] In some optional embodiments, the mass percentage content of the additive II in the electrolyte is B satisfying: 0.5%≤A%≤5%.

[0014] In some optional embodiments, the electrolyte further includes an additive III, and the additive III is selected from a mixture of one or more of carbonate additives, phosphate additives, and borate additives.

[0015] In some optional embodiments, the carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate.

[0016] In some optional embodiments, the phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, trispropargyl phosphate, and diethyl fluorophosphate.

[0017] In some optional embodiments, the borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

[0018] In some optional embodiments, the mass percentage of the additive III in the electrolyte is C%, 0.5%≤C%≤6%, and 1≤(B×C) / A.

[0019] In some optional embodiments, the electrolyte further includes a lithium salt; the lithium salt includes LiPF 6 、LiClO 4 、LiB(C 6 H 5 )、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF3 ) 2 、LiC(SO 2 CF 3 ) 3 and LiSiF 6 At least one of the following: the mass percentage of the lithium salt in the electrolyte is 8% to 15%.

[0020] A second aspect of the present application provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte as described in the first aspect of the present application.

[0021] In some optional embodiments, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, and the positive electrode material layer includes a positive electrode active material;

[0022] The chemical formula of the positive electrode active material is LiNi x Co y Mn (1-x-y) M z O 2 , 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti;

[0023] The specific surface area of ​​the positive electrode active material is Wm 2 / g; 5≤W≤20, 0.05≤(A×B) / W≤0.6.

[0024] A third aspect of the present application provides an electrical device, comprising the lithium-ion battery as described in the third aspect of the present application.

[0025] The technical solution provided by this application may have the following beneficial effects:

[0026] The present application scheme adds a cyclic sulfate ester compound and a boron-containing lithium salt compound as additives in the electrolyte, and utilizes the synergy of the two when used together to effectively make up for their respective defects, thereby improving the cycle capacity retention rate of the lithium-ion battery, especially the high-temperature storage and high-temperature cycle performance of lithium-ion batteries used in high-voltage and high-temperature environments.

[0027] Furthermore, the present application can further ensure that a thin, uniform, dense and stable interface film can be formed on the surface of the positive electrode plate by adjusting the relationship between the size of the positive electrode active material particles in the lithium-ion battery and the content of additive I and additive II in the electrolyte, thereby protecting the transition metal in the positive electrode plate, thereby ensuring that the battery has good kinetic performance while improving the high-temperature cycle performance and high-temperature storage performance of the battery, thereby improving the long cycle life of the battery.

[0028] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION

[0029] To make the present invention easy to understand, the present invention will be described in detail below. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terms used herein are only for describing specific embodiments and are not intended to be limiting.

[0030] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0031] Where a numerical range is provided, it is to be understood that each intermediate value between the upper and lower limits of the range and any other provisions or intermediate values ​​in the specified range is encompassed within the present invention. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges and are also encompassed within the present invention, subject to any explicitly excluded limits in the specified range. Where a specified range includes one or two limits, the scope excluding any or both of those included limits is also encompassed within the present invention. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically limited.

[0032] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any methods and materials or equivalent methods and materials described herein can also be used in the practice or testing of the present invention, preferred methods and materials are now described.

[0033] With the increasing demand for electronic products and the increasing requirements for the endurance of electric vehicles, the energy density requirements for lithium-ion batteries are also increasing. Currently, the discharge capacity and energy density can be increased by 15% to 35% by increasing the cutoff voltage of the transition metal oxide positive electrode, for example, to 4.5V or above. However, in these transition metal oxides, more Li insertion / extraction increases the electrode volume change, causing the CEI membrane to crack, and then the electrolyte will penetrate into the cracked transition metal oxide and react with it. The continuous side reactions of the transition metal oxide and the electrolyte will cause rapid capacity decay and deteriorate the cycle life of the battery.

[0034] In response to the above problems, the embodiments of the present application provide an electrolyte and a lithium-ion battery, which can form a CEI film with high density and good chemical stability at the positive electrode interface, inhibit the thermodynamic corrosion reaction and co-embedding reaction of solvent molecules, effectively reduce the loss of positive and negative electrode materials and active lithium in the electrolyte during the cycle process, and improve the high-temperature cycle and high-temperature storage performance of lithium-ion batteries.

[0035] The electrolyte of the embodiment of the present application includes additive I and additive II, additive I is a cyclic sulfate ester compound, and additive II is a boron-containing lithium salt compound; wherein the mass percentage of additive I in the electrolyte is A%, the mass percentage of additive II in the electrolyte is B%, and 0.2≤A / B≤10.

[0036] In the embodiments of the present application, a cyclic sulfate ester compound and a boron-containing lithium salt compound are added as additives to the electrolyte, and the synergy of the two when used together is utilized to effectively compensate for their respective defects, thereby improving the cycle capacity retention rate of the lithium-ion battery, especially the high-temperature storage and high-temperature cycle performance of the lithium-ion battery used in a high-voltage, high-temperature environment.

[0037] Specifically, the cyclic sulfate compound in additive I can participate in the film formation at the positive electrode, and make the formed interface film CEI film more chemically stable, not easy to decompose under high temperature and high voltage system, and can effectively improve the high temperature storage and high temperature cycle performance of the battery; however, the viscosity of additive I itself is relatively large, and when the content is high, it is easy to deteriorate the rate performance of the battery. The boron-containing functional group in additive II can also participate in the film formation at the positive electrode, and make the formed interface film CEI film denser and thinner, which is beneficial to improve the stability of the positive electrode material, and is more conducive to the transmission of lithium ions, and can alleviate the internal resistance growth rate of the battery in low temperature cycles; in addition, the Li contained in it + , there is no need to consume lithium salts in the electrolyte system when the positive and negative electrodes are formed into films, which effectively avoids the loss of active lithium in the positive and negative electrode materials and the electrolyte during the cycle process, so that the active lithium content in the battery system is maintained at a reasonable level for a long time, thereby improving the long cycle performance of lithium-ion batteries; however, Additive II is easy to decompose and produce gas during high-temperature storage and circulation, and high-temperature storage performance is easy to deteriorate when the content is high. In this application, by adding additive I cyclic sulfate compounds and boron-containing lithium salt compounds to the electrolyte, and further adjusting the relationship between the contents of additives I and additive II in the electrolyte, the two can better synergize and enhance the efficiency, thereby improving the cycle performance and storage performance of the battery under high temperature and high voltage systems while maintaining good low-temperature discharge performance.

[0038] In some embodiments, the cyclic sulfate compound of additive I is selected from sulfate compounds having three cyclic structures, and further is a sulfate compound containing 1-3 cyclic sulfates and 0-2 cyclic carbonate structures. When the amount of cyclic sulfates in additive I is too high, the viscosity of the electrolyte is easily increased, and the formed interface film is not conducive to the transmission of lithium ions, which deteriorates the rate performance of the battery; when additive I is a compound containing both cyclic sulfate and cyclic carbonate structures, or a compound containing three cyclic carbonate structures, it can form a film at the interface of the positive and negative electrodes at the same time during the battery charge and discharge process, improve the stability of the positive and negative electrodes, and the formed interface film has high density, good chemical stability, and good mechanical properties, thereby effectively improving the long cycle performance of the battery, especially the cycle performance under high voltage and high temperature systems.

[0039] In some embodiments, the additive I may be selected from at least one of the following compounds I-1 to I-8:

[0040]

[0041] The sulfur-based cyclic structure in the cyclic sulfate compound of additive I can be a sulfur-containing five-membered or six-membered heterocyclic structure. The interfacial film formed at the electrode interface has better chemical stability and better density. It can protect the positive and negative electrode interfaces with a thinner interfacial film, which is beneficial to the transmission of lithium ions and is also beneficial to improving the cycle performance and storage performance of the battery.

[0042] In some embodiments, the additive II may be selected from at least one of the following compounds II-1 to II-8:

[0043]

[0044] Additive II contains both boron-containing functional groups and lithium ions. On the one hand, the boron-containing functional groups can form films at the interfaces of the positive and negative electrodes at the same time. The conjugated system of the boron-containing functional groups helps to improve the stability and mechanical properties of the formed interface film, making the CEI film less likely to decompose and crack, thereby improving the stability of the positive and negative electrodes and the long cycle performance of the battery, especially the cycle performance under high voltage and high temperature systems; at the same time, the lithium ions therein can effectively avoid the consumption of the original lithium salt in the electrolyte system during the charge and discharge process, avoid the loss of active lithium in the positive and negative electrode materials and the electrolyte, and further improve the long cycle performance of the battery.

[0045] In some embodiments, the mass percentage A of the additive I in the electrolyte satisfies: 0.5%≤A%≤5%, for example, it can be 0.5%, 1%, 2%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of these values. By controlling the content of the sulfur-containing additive I in the electrolyte, the stability of the positive electrode CEI film can be effectively improved, and the high temperature cycle and high temperature storage performance of the battery can be improved while avoiding the deterioration of the low temperature performance of the battery.

[0046] In some embodiments, the mass percentage of additive II in the electrolyte satisfies B: 0.5%≤B%≤5%, for example, it can be 0.5%, 1%, 2%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two values ​​therein. By controlling the content of boron-containing lithium salt additive II in the electrolyte, on the one hand, the boron-containing functional group participates in the positive electrode film formation, which can improve the stability of the positive electrode material, and the formed CEI film is denser and thinner, which is conducive to the transmission of lithium ions; on the other hand, the additive itself contains Li + In the process of film formation, there is no need to consume the lithium salt in the system, which effectively avoids the loss of active lithium in the positive and negative electrode materials and the electrolyte. At the same time, it can avoid the decomposition and gas production of additives during high-temperature storage, and avoid the deterioration of the high-temperature storage performance of the battery.

[0047] In some embodiments, the electrolyte further includes an additive III, which may be selected from a mixture of one or more of carbonate additives, phosphate additives, and borate additives. Additive III may be used as an auxiliary additive in the electrolyte, and may cooperate with additives I and II to form a film at the positive and negative electrode interfaces, thereby further improving the compactness and stability of the CEI film, effectively avoiding the loss of active lithium, and improving the ion conductivity of the CEI film, thereby further improving the cycle performance.

[0048] In some specific embodiments, the carbonate additive may include at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate.

[0049] The phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tripropargyl phosphate, and diethyl fluorophosphate.

[0050] The borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

[0051] Among them, additive III helps to form films on the surfaces of positive and negative electrodes. When working together with additives I and II, it can effectively inhibit the decomposition of solvents in the electrolyte, slow down the consumption rate of the electrolyte, make the film thinner and more uniform, and reduce the mass transfer resistance of lithium ions in the CEI membrane. At the same time, additives such as phosphate esters have the ability to adsorb singlet oxygen on the surface of the positive electrode, reduce the damage to the positive electrode interface caused by side reactions, and protect the stability of the positive and negative electrode materials and the electrolyte.

[0052] In some embodiments, the mass percentage of additive III in the electrolyte is C%, 0.5%≤C%≤6%, for example, it can be 0.5%, 1%, 2%, 3%, 4%, 5%, 6% or a range consisting of any two of these values.

[0053] Furthermore, the total content of additives in the electrolyte is 0.1% to 16%, preferably 1% to 5.5%.

[0054] Furthermore, additive I, additive II, and additive III in the electrolyte satisfy: 1≤(B×C) / A.

[0055] In the embodiment of the present application, by adjusting the total amount of additives added in the electrolyte and the relationship between additives I, additives II, and additives III, when the above conditions are met, during the charge and discharge process of the battery, not only can the additives in the electrolyte form an interface film with high density and good stability at the interface of the positive and negative electrodes, but it is also not easy to cause the consumption of lithium salts in the electrolyte system, thereby effectively reducing the loss of active lithium and electrode active materials in the electrolyte; at the same time, it is not easy to deteriorate the viscosity of the electrolyte, and it is not easy to cause a surge in the amount of gas produced by the electrolyte during the charge and discharge process, so that the lithium-ion battery not only has good cycle performance, storage performance, and low-temperature discharge performance, but also has good safety performance.

[0056] In some embodiments, the electrolyte further comprises a lithium salt. The lithium salt may comprise LiPF 6 、LiClO 4 、LiB(C 6 H 5 )、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiC(SO 2 CF 3 ) 3 and LiSiF 6 At least one of the following: the mass percentage of lithium salt in the electrolyte is 8% to 15%.

[0057] The inventors of the present application have discovered in their research that by simultaneously adjusting the contents of lithium salt and boron-containing lithium salt additives in the electrolyte system, the concentration of lithium ions in the electrolyte can be maintained within a reasonable range, thereby ensuring sufficient charge carriers while avoiding ion aggregation and the like, thereby ensuring good ion mobility; and improving the stability of electrodes and electrolytes under high voltages, thereby ensuring efficient, stable and safe operation of the battery.

[0058] In some embodiments, the electrolyte further includes an organic solvent, and the organic solvent may include at least one of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, diphenyl carbonate, methyl acetate, methyl propionate, methyl butyrate, methyl acetate, ethyl acetate, propyl acetate, ethyl butyrate, propyl propionate, γ-butyrolactone, 1,3-dioxolane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0059] It should be noted that the present application does not specifically limit the method for preparing the electrolyte, and those skilled in the art can prepare it into an electrolyte according to conventional technical means, for example, by uniformly mixing the raw materials according to a proportion.

[0060] The lithium-ion battery provided in the embodiment of the present application comprises a positive electrode sheet, a negative electrode sheet, a separator and the above-mentioned electrolyte.

[0061] In the embodiment of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector. The positive electrode current collector mentioned in the present application is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. In one embodiment, the positive electrode current collector can be a metal material such as aluminum, stainless steel, nickel plating, titanium, tantalum, and a carbon material such as carbon cloth and carbon paper.

[0062] In some embodiments, the positive electrode material layer includes a positive electrode active material, the chemical formula of the positive electrode active material is LiNi x Co y Mn (1-x-y) M z O 2 , 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti; specifically, for example, it can be at least one of lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, lithium nickel oxide, nickel cobalt manganese oxide or lithium-rich manganese-based materials.

[0063] In some embodiments, the specific surface area of ​​the positive electrode active material is Wm 2 / g, 5≤W≤20, for example, it can be 5m 2 / g, 8m 2 / g, 10m2 / g, 12.5m 2 / g, 15m 2 / g, 20m 2 / g, and the range of any two values ​​between the above values. By controlling the specific surface area of ​​the positive electrode active material, the efficiency of electron conduction and ion mass transfer can be guaranteed, the side reactions of the electrolyte can be reduced, and the consumption of electrolyte in the cycle of the lithium-ion battery can be controlled, thereby ensuring that the active lithium content in the battery system is at a reasonable level and improving the cycle performance of the secondary battery. If the specific surface area of ​​the lithium-ion active material is too small (less than 5m 2 / g), the particles of lithium-ion positive electrode active materials are large, and both electronic conduction and ion mass transfer are limited, resulting in a decrease in kinetic performance, an increase in DCR, and a corresponding increase in voltage polarization, which further increases the degree of electrolyte side reactions and leads to a decrease in cycle performance; if the specific surface area of ​​the lithium-ion active material is too large (greater than 20m 2 / g), the contact area between the electrolyte and the positive electrode active material increases, the degree of side reactions intensifies, the electrolyte consumption accelerates, and the active lithium content cannot be maintained at a reasonable level, which leads to a decrease in cycle performance.

[0064] Furthermore, the lithium-ion battery satisfies: 0.05≤(A×B) / W≤0.6, and more preferably 0.1-0.3. By adjusting the size of the positive electrode active material particles in the lithium-ion battery and the content relationship of the additive I and the additive II in the electrolyte, it can be further ensured that a thin and uniform interface film with good density and stability can be formed on the surface of the positive electrode plate to protect the transition metal in the positive electrode plate, thereby ensuring that the battery has good kinetic performance while improving the high-temperature cycle performance and high-temperature storage performance of the battery, and improving the long cycle life of the battery.

[0065] In some embodiments, the positive electrode material layer further includes a conductive agent and a binder. Specifically, the positive electrode material layer is formed by mixing the positive electrode active material, the conductive agent and the binder into a positive electrode slurry, and then coating the positive electrode slurry on the surface of the positive electrode current collector.

[0066] The conductive agent may be at least one of superconducting carbon black, conductive carbon black, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0067] The adhesive may be at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin.

[0068] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector. The negative electrode current collector mentioned in the present application is not particularly limited, as long as it can achieve the purpose of the present application, for example, it can be copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector.

[0069] The negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. Specifically, the negative electrode material layer is formed by mixing the negative electrode active material, the conductive agent and the binder into a negative electrode slurry, and then coating the negative electrode slurry on the surface of the negative electrode current collector.

[0070] In some embodiments, the negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon beads, hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO 2 , spinel-structured lithiated TiO 2 -Li 4 Ti 5 O 12 , Li-Al alloy.

[0071] The carbon material conductive agent may include at least one of carbon nanotubes, carbon nanofibers, graphene, artificial graphite, natural graphite and mesophase carbon microspheres.

[0072] The binder may include one or more of lithium carboxymethyl cellulose (CMC-Li), sodium carboxymethyl cellulose (CMC-Na), potassium carboxymethyl cellulose (CMC-K), styrene-butadiene rubber (SBR), styrene acrylic emulsion, lithium polyacrylate (PAA-Li), sodium polyacrylate (PAA-Na), potassium polyacrylate (PAA-K), lithium alginate (ALG-Li), sodium alginate (ALG-Na) and potassium alginate (ALG-K).

[0073] In the lithium-ion battery mentioned in the present application, the diaphragm is arranged between the positive electrode and the negative electrode to prevent short circuit. The embodiment of the present application has no particular restrictions on the material and shape of the diaphragm, as long as it does not significantly damage the effect of the present application. In some embodiments, the diaphragm includes a porous sheet or non-woven fabric-like material with excellent liquid retention. The materials of the resin or glass fiber diaphragm include but are not limited to polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc.

[0074] The preparation process of the battery is well known to those skilled in the art and is not particularly limited in this application. For example, the electrochemical device can be manufactured by the following process: the positive electrode sheet and the negative electrode sheet are overlapped via a diaphragm, and after winding, folding, etc. as required, they are placed in a housing, and the electrolyte is injected into the housing and sealed, wherein the diaphragm used is the diaphragm provided in this application. In addition, overcurrent protection elements, guide plates, etc. can also be placed in the housing as required to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0075] The present application also provides an electrical device or various energy storage systems using batteries as energy storage elements. Electrical devices include but are not limited to mobile phones, tablets, computers, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc.

[0076] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0077] Example 1

[0078] (1) Preparation of electrolyte

[0079] Ethylene carbonate (EC), propylene carbonate (PC), and propyl propionate (PP) were mixed in a mass ratio of 1:1:1 to obtain a solvent; then, based on the total mass of the electrolyte, additives in the mass percentages shown in Table 1 were added respectively, and after mixing evenly, lithium salt LiPF 6 , and mix evenly to obtain an electrolyte.

[0080] (2) Preparation of positive electrode sheet

[0081] The positive electrode active material is lithium cobalt oxide (LiCoO 2 ), conductive agent CNT (Carbon Nanotube), and adhesive polyvinylidene fluoride PVDF are mixed in a mass ratio of 95:2.5:2.5, and then N-methylpyrrolidone (NMP) is added as a solvent, and the mixture is stirred and mixed to form a uniform positive electrode slurry. The slurry is coated on the positive electrode current collector aluminum foil, dried, and cold pressed to obtain a positive electrode sheet.

[0082] (3) Preparation of negative electrode sheet

[0083] The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber, and the thickener sodium carboxymethyl cellulose are fully stirred and mixed in a deionized water solvent at a mass ratio of 96:1.2:1.5:1.3 to form a uniform negative electrode slurry. The slurry is coated on the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.

[0084] (4) Preparation of lithium-ion batteries

[0085] PE porous polymer film is used as the separator.

[0086] The positive electrode sheet, the separator and the negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play a role of isolation, and then the stacked electrode sheet and the separator are wound to obtain a roll core. The roll core is placed in the aluminum-plastic film bag formed by punching the shell, and the non-aqueous electrolyte prepared above is injected into the baked and dried battery cells respectively. After vacuum packaging, standing, formation and other processes, a lithium-ion battery is obtained.

[0087] Examples 2-37 and Comparative Examples 1-5 adopt the same method as Example 1, the difference being the type and content of the additives, as shown in Table 1 for details.

[0088] Table 1 Examples and Comparative Examples Types and Contents

[0089]

[0090]

[0091] Lithium-ion battery performance test:

[0092] 1) 45℃ cycle performance test

[0093] In a (45±2)℃ constant temperature box, the lithium-ion battery was charged to 4.5V at 1C constant current and constant voltage, the cut-off current was 0.05C, and then discharged to 3V at 1C. Multiple charge and discharge cycles were performed under the above conditions, and the capacity retention rate of the battery after 600 cycles was calculated. There were 5 batteries in each group, and the average capacity retention rate after the cycle was calculated and recorded in Table 2.

[0094] Capacity retention rate (%) = discharge capacity corresponding to the number of cycles (mAh) / discharge capacity of the third cycle (mAh) * 100%

[0095] 2) 0℃ cycle test

[0096] In a (0±2)℃ constant temperature box, the lithium-ion battery was charged to 4.5V at 1C constant current and constant voltage, the cut-off current was 0.05C, and then discharged to 3V at 1C. Multiple charge and discharge cycles were performed under the above conditions, and the capacity retention rate of the battery after 600 cycles was calculated. There were 5 batteries in each group, and the average capacity retention rate after the cycle was calculated and recorded in Table 2.

[0097] Capacity retention rate (%) = discharge capacity corresponding to the number of cycles (mAh) / discharge capacity of the third cycle (mAh) * 100%

[0098] 3) High temperature storage test

[0099] In a (25±2)℃ constant temperature box, charge the lithium-ion battery to 4.5V at 1C constant current and constant voltage, with a cut-off current of 0.05C. Test the cell thickness H 1 ; Then place the battery cell in a constant temperature box at (85±2)℃ for 36 hours, take out the battery cell from the high temperature oven and test the thickness of H 2 There are 5 batteries in each group. The thickness expansion rate is calculated and the average value is recorded in Table 2.

[0100] High temperature storage thickness expansion rate (%) = (H 2 -H 1 ) / H 1 *100%

[0101] Table 2 Test data

[0102]

[0103]

[0104] The data of Comparative Examples 1-3 show that the addition of additive I alone or additive II alone is difficult to effectively improve the 0°C and 45°C cycle performance of the lithium-ion battery, and may deteriorate the 85°C storage performance. The data of Comparative Examples 1 and Comparative Examples 4-5 show that when additives I and II are added to the electrolyte at the same time, the relative ratio between additives I and additives II is too high or too low, and it is still difficult to effectively improve the cycle performance and storage performance of the lithium-ion battery at the same time, and may even deteriorate the performance of the lithium-ion battery.

[0105] The data of Examples 1-9 and Comparative Examples 4-5 show that when the ratio of Additive I to Additive II is in the range of 0.2-10, the high temperature cycle performance, low temperature cycle performance and high temperature storage performance of the battery can be synergistically improved. On the one hand, the boron-containing functional group participates in the positive electrode film formation, improves the stability of the positive electrode material, and the formed CEI film is denser and thinner, which is conducive to the transmission of lithium ions; on the other hand, the additive itself contains Li + During the film formation process, there is no need to consume the lithium salt in the system, which effectively avoids the loss of active lithium in the positive and negative electrode materials and the electrolyte.

[0106] At the same time, according to the data of Examples 1-4, when the content of additive I increases, the high temperature cycle performance and high temperature storage performance of the battery are improved, but the 0°C cycle will be slightly deteriorated. This is because excessive additive I will cause the interface impedance to rise sharply, and excessive additive I will cause the viscosity of the electrolyte to rise sharply, which is not conducive to the low temperature performance of the battery. According to the data of Examples 5-9, when the content of additive II increases, the low temperature cycle performance and high temperature cycle performance of the battery are improved, but the high temperature storage performance will be slightly deteriorated; especially when the content of additive II gradually decreases relative to additive I and tends to 0.2 or even lower, the cycle performance of the battery will also deteriorate. This is because excessive boron-containing lithium salt additives II will decompose and produce gas in large quantities during high temperature storage, which is not conducive to the storage of the battery in a high temperature environment and the cycle life of the battery.

[0107] According to the data of Examples 2 and 10-26, the combination of Additive I and Additive II of the present application, that is, the combination of a cyclic sulfate compound containing three ring structures and a boron-containing lithium salt compound, can significantly improve the low-temperature cycle performance, high-temperature cycle performance and high-temperature storage performance of the battery.

[0108] The data of Examples 27-33 show that, on the basis of the addition of Additives I and II described in the present application, the addition of Additive III can further improve the cycle performance. Among them, the phosphate additive can form a film on the positive electrode surface, inhibit the decomposition of the electrolyte solvent, slow down the consumption rate of the electrolyte, make the film thinner and more uniform, reduce the mass transfer resistance of lithium ions in the CEI membrane, and at the same time have the ability to adsorb singlet oxygen on the positive electrode surface, and have a good effect on improving battery performance.

[0109] Moreover, additives II and additives III, such as phosphate additives, synergistically improve the low-temperature cycle performance more effectively. That is, when the content of additives II and additives III is too low relative to additive I, it is not conducive to improving the deterioration of the low-temperature performance of the battery. When the condition 1≤(B×C) / A is met, the synergistic effect of the three types of additives in the electrolyte is the best.

[0110] The data in Tables 1 and 2 show that by controlling the specific surface area of ​​the positive electrode active material, the content of the electrolyte additive I and the boron-containing lithium salt additive II in the electrolyte so as to satisfy the following relationship: 0.2≤A / B≤10, 0.05≤(A×B) / W≤0.6, 5≤W≤20, the improvement effect on the cycle performance and storage performance of the lithium-ion battery is significant.

[0111] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present application may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.

Claims

1. An electrolyte, It is characterized in that It comprises an additive I and an additive II, wherein the additive I is a cyclic sulfate ester compound, and the additive II is a boron-containing lithium salt compound; Wherein, the mass percentage of the additive I in the electrolyte is A%, the mass percentage of the additive II in the electrolyte is B%, and 0.2≤A / B≤10.

2. The electrolyte according to claim 1, It is characterized in that The additive I is selected from at least one of the following compounds:

3. The electrolyte according to claim 1, It is characterized in that The additive II is selected from at least one of the following compounds:

4. The electrolyte according to claim 1, It is characterized in that The mass percentage A of the additive I in the electrolyte satisfies: 0.5%≤A%≤5%; And / or, the mass percentage content of the additive II in the electrolyte is B satisfying: 0.5%≤B%≤5%.

5. The electrolyte according to claim 1, It is characterized in that The electrolyte further includes an additive III, and the additive III is selected from a mixture of one or more of carbonate additives, phosphate additives, and borate additives.

6. The electrolyte according to claim 5, It is characterized in that The carbonate additive includes at least one of fluoroethylene carbonate, vinylene carbonate, 3,3,3-trifluoropropylene carbonate, tetrafluoroethylene carbonate, and vinyl ethylene carbonate; And / or, the phosphate additive includes at least one of tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tripropargyl phosphate, and diethyl fluorophosphate; And / or, the borate ester additive includes at least one of tris(trimethylsilyl)borate, triallyl borate, and tris(triethylsilyl)borate.

7. The electrolyte according to claim 5, It is characterized in that The mass percentage of the additive III in the electrolyte is C%, 0.5%≤C%≤6%, and 1≤(B×C) / A.

8. The electrolyte according to claim 1, It is characterized in that The electrolyte also includes a lithium salt; The lithium salt includes LiPF 6 、LiClO 4 、LiB(C 6 H 5 )、LiCH 3 SO 3 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiC(SO 2 CF 3 ) 3 and LiSiF 6 At least one of; The mass percentage of the lithium salt in the electrolyte is 8% to 15%.

9. A lithium ion battery, It is characterized in that The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte as claimed in any one of claims 1 to 8.

10. The lithium ion battery according to claim 9, It is characterized in that The positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer coated on the surface of the positive electrode current collector, wherein the positive electrode material layer comprises a positive electrode active material; The chemical formula of the positive electrode active material is LiNi x Co y Mn (1-x-y) M z O 2 , 0.5≤x≤0.9, x+y<1, 0≤z<0.08, M is one of Al, Mg, Zr and Ti; The specific surface area of ​​the positive electrode active material is Wm 2 / g; 5≤W≤20, 0.05≤(A×B) / W≤0.6.

Citation Information

Patent Citations

  • Electrolyte and lithium ion battery containing electrolyte

    CN104916867A

  • Electrolytic solution, electrochemical device, lithium-ion secondary cell, and module

    CN110062976A

  • Lithium ion battery

    CN114864922A

  • Lithium ion battery

    CN117728026A

  • Electrochemical device and electronic device

    CN117832637A

Cited By

  • Lithium ion battery

    CN119208736A

  • Lithium ion battery

    CN119400963A

  • Lithium ion battery

    CN119627230A