A method for preparing anode material of solid-state battery

By using lithium iron phosphate, conductive carbon black, carbon nanotubes and other materials in the positive electrode material of solid-state battery, and combining with stable adjustment and effective adjustment reinforcement of doped bentonite, the poor performance stability of positive electrode materials in the prior art is solved. The problem is that higher circulation capacity retention rate and better high magnification and low temperature resistance are achieved.

CN118522896BActive Publication Date: 2024-11-29HUNAN JINYANG ALKENE CARBON NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410970251.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The circulation capacity retention performance of existing solid-state battery positive electrode materials is low, and the performance stability is poor under high magnification and low temperature conditions, which limits the efficiency of the product.

Method used

The high-performance solid-state battery positive electrode material is used to form a solid-state battery positive electrode material with doped bentonite-adjusted processes through ultrasonic mixing, ball milling and other processes.

Benefits of technology

It significantly improves the circulation capacity retention performance of the positive electrode material of solid-state battery and the performance stability under high magnification and low temperature resistance, and improves the efficiency of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of solid-state battery positive electrode materials, and specifically to a method for preparing a solid-state battery positive electrode material, comprising the following steps: coating a coating slurry on both sides of an aluminum foil, with a coating thickness of 10-15µm, drying at 55-65°C for 2h after coating, and obtaining a solid-state battery positive electrode material. In the preparation of the solid-state battery positive electrode material of the present invention, lithium iron phosphate, conductive carbon black, and carbon nanotubes are first mixed with a solvent to form a material matrix, and a stabilizer and an efficiency-adjusting reinforcing agent adjusted by adding bentonite are coordinated and coordinated to enhance the efficiency. The obtained positive electrode material product has excellent battery cycle capacity retention rate performance, and the product has a significant performance stability effect under high rate and low temperature resistance conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state battery positive electrode materials, and in particular to a method for preparing a solid-state battery positive electrode material. Background Art

[0002] All-solid-state lithium-ion batteries generally include three parts: positive electrode, negative electrode, and solid electrolyte. Among them, the positive electrode includes positive electrode active material, binder, and conductive agent; the negative electrode includes negative electrode active material, binder, conductive agent or lithium metal is used as the negative electrode; the solid electrolyte includes binder and electrolyte material, and the electrolyte material is selected from oxide or sulfide solid electrolyte.

[0003] Solid-state batteries made from existing positive electrode materials have low cycle capacity retention performance, and the product's performance stability is poor under high-rate and low-temperature conditions, further limiting the product's efficiency. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for preparing a positive electrode material for a solid-state battery to solve the problems raised in the above background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution:

[0006] The present invention provides a method for preparing a solid-state battery positive electrode material, comprising the following steps:

[0007] Step 1: Weigh the raw materials by weight:

[0008] 55-65 parts of lithium iron phosphate, 8-12 parts of stabilizer adjusted by doping bentonite, 10-15 parts of conductive carbon black, 3-5 parts of carbon nanotubes, 4-7 parts of effect-adjusting reinforcing agent, 2-4 parts of polyvinyl alcohol, 30-35 parts of ethanol solvent, 4-7 parts of gelatin;

[0009] Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 100-150 r / min for 1 hour, and then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent;

[0010] Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 500-700 r / min for 2 hours. Stir thoroughly, and finally add gelatin and keep the speed mixed for 1 hour to obtain a coating slurry;

[0011] Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 10-15 µm. After coating, dry at 55-65 ° C for 2 hours. After drying, obtain a solid-state battery positive electrode material. The preparation method of the stabilizer adjusted by doping bentonite is:

[0012] S01: The bentonite was heated to 170-180°C at a rate of 1-3°C / min, kept at that temperature for 5-10 minutes, then heated to 275°C at a rate of 2-4°C / min, kept at that temperature for 2-5 minutes, and finally air-cooled to room temperature;

[0013] S02: Preparation of modified yttrium oxide agent:

[0014] S021: treating the yttrium oxide with proton irradiation at a power of 350-400 W for 5 min to obtain irradiated yttrium oxide;

[0015] S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent;

[0016] The preparation method of the modified liquid is:

[0017] The graphene is first immersed in a sodium silicate solution with a volume of 2 to 5 times the total volume of the graphene, after which the immersion is completed, the solution is filtered and dried, and 3 to 5 parts of the dried graphene, 4 to 7 parts of the chitosan solution, 1 to 3 parts of the silane coupling agent KH560, and 0.4 to 0.7 parts of citric acid are mixed to obtain a modified solution;

[0018] S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained;

[0019] S04: The bentonite agent and stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:4. After the ball milling is completed, the mixture is washed with water and dried to obtain the stabilizer adjusted by doping bentonite.

[0020] Preferably, the power of ultrasonic mixing in step 2 is 350-400 W, and the ultrasonic time is 1 h.

[0021] Preferably, the ultrasonic power of the SO22 ultrasonic modification treatment is 350-400 W, and the ultrasonic time is 20-30 min; the immersion power of the immersion treatment is 400-500 W, and the immersion time is 20-30 min.

[0022] Preferably, the mass fraction of the sodium silicate solution is 5-8%; the mass fraction of the chitosan solution is 3-5%;

[0023] The ball milling speed of the first-stage ball milling treatment in S03 is 450~550r / min, and the ball milling is 1~2h;

[0024] The ball milling speed of the secondary ball milling treatment in S04 is 750~850r / min, and the ball milling time is 35~50min.

[0025] Preferably, the stabilizer comprises the following raw materials in parts by weight:

[0026] The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 3 to 5 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid;

[0027] 5-8 parts of hydroxyapatite solution, 2-5 parts of lanthanum chloride solution, 1-3 parts of nano-silica sol and 1-2 parts of nano-magnesium oxide are mixed and milled thoroughly. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizing agent.

[0028] Preferably, the mass fraction of the sodium lignin sulfonate solution is 4-7%; the mass fraction of the lanthanum chloride solution is 2-5%.

[0029] Preferably, the blending is ball-milled at a speed of 1500 r / min for 1 to 2 h.

[0030] Preferably, the preparation method of the effect-adjusting reinforcing agent is:

[0031] S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying;

[0032] S102: 4-7 parts of dry silicon carbide whiskers, 1-3 parts of stearic acid, 2-4 parts of carboxymethyl cellulose, and 8-12 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1000-1500 r / min for 1-2 hours. After the stirring is completed, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

[0033] Preferably, the mass fraction of the potassium permanganate solution is 3-6%.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. In the preparation of the solid-state battery positive electrode material of the present invention, lithium iron phosphate, conductive carbon black, and carbon nanotubes are first mixed with a solvent to form a material matrix, and a stabilizer and an efficiency-adjusting reinforcing agent adjusted by doping bentonite are added to coordinate and enhance the efficiency together. The obtained positive electrode material product has excellent battery cycle capacity retention rate performance, and the product has significant performance stability under high rate and low temperature resistance conditions;

[0036] 2. The stabilizer adjusted by doping bentonite is first heated to 170~180℃ at a rate of 1~3℃ / min, and kept warm for 5~10min, and then heated to 275℃ at a rate of 2~4℃ / min, and kept warm for 2~5min. The interlaminar spacing of bentonite is optimized by step-by-step thermal improvement treatment, and the efficiency of active lamellae of bentonite is improved at the same time, so that bentonite can be interspersed in the system to enhance the performance stability of the system. The modified yttrium oxide agent uses yttrium oxide to be irradiated by protons to optimize its activity. The modified liquid is firstly treated by ultrasonic modification, and the graphene is first immersed in a sodium silicate solution to optimize the flake stability of the graphene. At the same time, the chitosan solution, the silane coupling agent KH560 and the citric acid are fully mixed to obtain the modified liquid. Through the coordination between the raw materials in the modified liquid, the flake graphene is interspersed with the bentonite to reinforce the bentonite, and the flake graphene is used to assemble the layered bentonite to optimize the system performance stability, thereby enhancing the product's performance stability effect under the conditions of high rate and low temperature resistance;

[0037] 3. The stabilizer is further improved by treating the bentonite agent adjusted by yttrium oxide. The hydroxyapatite in the stabilizer is fully dispersed in the sodium lignin sulfonate solution to obtain a hydroxyapatite liquid, and then the stabilizer is obtained by ball milling with a lanthanum chloride solution, nano-silica sol and nano-magnesium oxide. The stabilizer uses hydroxyapatite as a point structure, and is matched with raw materials such as nano-magnesium dioxide and lanthanum chloride solution. Through the coordinated co-matching effect between the raw materials, the cycle capacity retention rate of the product and the performance stability effect of the product are further enhanced;

[0038] 4. The effect-adjusting reinforcing agent adopts silicon carbide whiskers treated with potassium permanganate solution to optimize its dispersion and activity. At the same time, it is fully blended and stirred with stearic acid, carboxymethyl cellulose and sodium dodecylbenzene sulfonate solution. Through the improvement of the co-matching between the raw materials, the whisker-shaped silicon carbide whiskers are distributed in the system to enhance the interface effect between the raw materials of the system. At the same time, the synergistic effect of the effect-adjusting reinforcing agent and the stabilizing agent adjusted by doping bentonite is enhanced, and the performance of the product is further improved. DETAILED DESCRIPTION

[0039] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] A method for preparing a positive electrode material for a solid-state battery in this embodiment comprises the following steps:

[0041] Step 1: Weigh the raw materials by weight:

[0042] 55-65 parts of lithium iron phosphate, 8-12 parts of stabilizer adjusted by doping bentonite, 10-15 parts of conductive carbon black, 3-5 parts of carbon nanotubes, 4-7 parts of effect-adjusting reinforcing agent, 2-4 parts of polyvinyl alcohol, 30-35 parts of ethanol solvent, 4-7 parts of gelatin;

[0043] Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 100-150 r / min for 1 hour, and then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent;

[0044] Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 500-700 r / min for 2 hours. Stir thoroughly, and finally add gelatin and keep the speed mixed for 1 hour to obtain a coating slurry;

[0045] Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 10-15µm. After coating, dry at 55-65°C for 2h to obtain a solid-state battery positive electrode material.

[0046] In step 2 of this embodiment, the power of ultrasonic mixing is 350-400 W, and the ultrasonic time is 1 h.

[0047] The preparation method of the stabilizer adjusted by doping bentonite in this embodiment is:

[0048] S01: The bentonite was heated to 170-180°C at a rate of 1-3°C / min, kept at that temperature for 5-10 minutes, then heated to 275°C at a rate of 2-4°C / min, kept at that temperature for 2-5 minutes, and finally air-cooled to room temperature;

[0049] S02: Preparation of modified yttrium oxide agent:

[0050] S021: treating the yttrium oxide with proton irradiation at a power of 350-400 W for 5 min to obtain irradiated yttrium oxide;

[0051] S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent;

[0052] The preparation method of the modified liquid is:

[0053] The graphene is first immersed in a sodium silicate solution with a volume of 2 to 5 times the total volume of the graphene, after which the immersion is completed, the solution is filtered and dried, and 3 to 5 parts of the dried graphene, 4 to 7 parts of the chitosan solution, 1 to 3 parts of the silane coupling agent KH560, and 0.4 to 0.7 parts of citric acid are mixed to obtain a modified solution;

[0054] S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained;

[0055] S04: The bentonite agent and stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:4. After the ball milling is completed, the agent is washed with water and dried to obtain the stabilizer adjusted by doping bentonite.

[0056] The ultrasonic power of the ultrasonic modification treatment of S022 in this embodiment is 350~400W, and the ultrasonic time is 20~30min; the immersion power of the immersion treatment is 400~500W, and the immersion time is 20~30min.

[0057] The mass fraction of the sodium silicate solution in this embodiment is 5-8%; the mass fraction of the chitosan solution is 3-5%;

[0058] The ball milling speed of the first-stage ball milling treatment in S03 is 450~550r / min, and the ball milling is 1~2h;

[0059] The ball milling speed of the secondary ball milling treatment in S04 is 750~850r / min, and the ball milling time is 35~50min.

[0060] The stabilizer of this embodiment includes the following raw materials in parts by weight:

[0061] The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 3 to 5 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid;

[0062] 5-8 parts of hydroxyapatite solution, 2-5 parts of lanthanum chloride solution, 1-3 parts of nano-silica sol and 1-2 parts of nano-magnesium oxide are mixed and milled thoroughly. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizing agent.

[0063] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 4-7%; the mass fraction of the lanthanum chloride solution is 2-5%.

[0064] The blending process of this embodiment is performed at a full milling speed of 1500 r / min for 1 to 2 hours.

[0065] The preparation method of the effect-adjusting reinforcing agent of this embodiment is:

[0066] S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying;

[0067] S102: 4-7 parts of dry silicon carbide whiskers, 1-3 parts of stearic acid, 2-4 parts of carboxymethyl cellulose, and 8-12 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1000-1500 r / min for 1-2 hours. After the stirring is completed, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

[0068] The mass fraction of the potassium permanganate solution in this embodiment is 3-6%.

[0069] Example 1

[0070] A method for preparing a positive electrode material for a solid-state battery in this embodiment comprises the following steps:

[0071] Step 1: Weigh the raw materials by weight:

[0072] 55 parts of lithium iron phosphate, 8 parts of stabilizer adjusted by doping bentonite, 10 parts of conductive carbon black, 3 parts of carbon nanotubes, 4 parts of effect-adjusting reinforcing agent, 2 parts of polyvinyl alcohol, 30 parts of ethanol solvent, and 4 parts of gelatin;

[0073] Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 100 r / min for 1 hour, and then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent;

[0074] Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 500 r / min for 2 hours. Stir thoroughly, and finally add gelatin and keep the speed mixed for 1 hour to obtain a coating slurry;

[0075] Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 10µm. After coating, dry at 55°C for 2h to obtain a solid-state battery positive electrode material.

[0076] In step 2 of this embodiment, the power of ultrasonic mixing is 350 W, and the ultrasonic time is 1 hour.

[0077] The preparation method of the stabilizer adjusted by doping bentonite in this embodiment is:

[0078] S01: The bentonite was heated to 170°C at a rate of 1°C / min, kept at that temperature for 5 min, then heated to 275°C at a rate of 2°C / min, kept at that temperature for 2 min, and finally cooled to room temperature in air;

[0079] S02: Preparation of modified yttrium oxide agent:

[0080] S021: treating the yttrium oxide with proton irradiation at a power of 350 W for 5 minutes to obtain irradiated yttrium oxide;

[0081] S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent;

[0082] The preparation method of the modified liquid is:

[0083] The graphene is first immersed in a sodium silicate solution twice the total amount of the graphene, after the immersion is completed, the solution is filtered and dried, and 3 parts of the dried graphene, 4 parts of the chitosan solution, 1 part of the silane coupling agent KH560 and 0.4 parts of citric acid are mixed to obtain a modified solution;

[0084] S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained;

[0085] S04: The bentonite agent and stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:4. After the ball milling is completed, the agent is washed with water and dried to obtain the stabilizer adjusted by doping bentonite.

[0086] The ultrasonic power of the ultrasonic modification treatment of S022 in this embodiment is 350W, and the ultrasonic time is 20min; the immersion power of the immersion treatment is 400W, and the immersion time is 20min.

[0087] The mass fraction of the sodium silicate solution in this embodiment is 5%; the mass fraction of the chitosan solution is 3%;

[0088] The ball milling speed of the first-stage ball milling treatment in S03 was 450 r / min, and the ball milling lasted for 1 h;

[0089] The ball milling speed of the secondary ball milling treatment in S04 is 750r / min, and the ball milling time is 35min.

[0090] The stabilizer of this embodiment includes the following raw materials in parts by weight:

[0091] The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 3 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid;

[0092] 5 parts of hydroxyapatite solution, 2 parts of lanthanum chloride solution, 1 part of nano-silica sol and 1 part of nano-magnesium oxide are mixed and milled thoroughly. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizer.

[0093] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 4%; the mass fraction of the lanthanum chloride solution is 2%.

[0094] The blending process of this embodiment is performed at a full milling speed of 1500 r / min for 1 hour.

[0095] The preparation method of the effect-adjusting reinforcing agent of this embodiment is:

[0096] S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying;

[0097] S102: 4 parts of dried silicon carbide whiskers, 1 part of stearic acid, 2 parts of carboxymethyl cellulose, and 8 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1000 r / min for 1 hour. After the stirring is completed, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

[0098] The mass fraction of the potassium permanganate solution in this embodiment is 3%.

[0099] Example 2

[0100] A method for preparing a positive electrode material for a solid-state battery in this embodiment comprises the following steps:

[0101] Step 1: Weigh the raw materials by weight:

[0102] 65 parts of lithium iron phosphate, 12 parts of stabilizer adjusted by doping bentonite, 15 parts of conductive carbon black, 5 parts of carbon nanotubes, 7 parts of effect-adjusting reinforcing agent, 4 parts of polyvinyl alcohol, 35 parts of ethanol solvent, and 7 parts of gelatin;

[0103] Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 150 r / min for 1 hour, and then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent;

[0104] Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 700 r / min for 2 hours. Stir thoroughly, and finally add gelatin and keep the speed mixed for 1 hour to obtain a coating slurry;

[0105] Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 15µm. After coating, dry at 65°C for 2h to obtain a solid-state battery positive electrode material.

[0106] In step 2 of this embodiment, the power of ultrasonic mixing is 400 W and the ultrasonic time is 1 h.

[0107] The preparation method of the stabilizer adjusted by doping bentonite in this embodiment is:

[0108] S01: The bentonite was heated to 180°C at a rate of 3°C / min, kept at this temperature for 10 min, then heated to 275°C at a rate of 4°C / min, kept at this temperature for 5 min, and finally cooled to room temperature in air;

[0109] S02: Preparation of modified yttrium oxide agent:

[0110] S021: treating the yttrium oxide with proton irradiation at a power of 400 W for 5 minutes to obtain irradiated yttrium oxide;

[0111] S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent;

[0112] The preparation method of the modified liquid is:

[0113] The graphene is first immersed in a sodium silicate solution with a volume of 5 times the total volume of the graphene, after which the immersion is completed, the graphene is filtered and dried, and 5 parts of the dried graphene, 7 parts of the chitosan solution, 3 parts of the silane coupling agent KH560 and 0.7 parts of citric acid are mixed to obtain a modified solution;

[0114] S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained;

[0115] S04: The bentonite agent and stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:4. After the ball milling is completed, the mixture is washed with water and dried to obtain the stabilizer adjusted by doping bentonite.

[0116] The ultrasonic power of the ultrasonic modification treatment of S022 in this embodiment is 400W, and the ultrasonic time is 30min; the immersion power of the immersion treatment is 500W, and the immersion time is 30min.

[0117] The mass fraction of the sodium silicate solution in this embodiment is 8%; the mass fraction of the chitosan solution is 5%;

[0118] The ball milling speed of the first-stage ball milling treatment in S03 was 550 r / min, and the ball milling lasted for 2 h;

[0119] The ball milling speed of the secondary ball milling treatment in S04 is 850r / min, and the ball milling time is 50min.

[0120] The stabilizer of this embodiment includes the following raw materials in parts by weight:

[0121] The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 5 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid;

[0122] 8 parts of hydroxyapatite solution, 5 parts of lanthanum chloride solution, 3 parts of nano-silica sol and 2 parts of nano-magnesium oxide are mixed and milled thoroughly. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizer.

[0123] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 7%; the mass fraction of the lanthanum chloride solution is 5%.

[0124] The blending process of this embodiment is performed at a full milling speed of 1500 r / min for 2 h.

[0125] The preparation method of the effect-adjusting reinforcing agent of this embodiment is:

[0126] S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying;

[0127] S102: 7 parts of dried silicon carbide whiskers, 3 parts of stearic acid, 4 parts of carboxymethyl cellulose, and 12 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1500 r / min for 2 hours. After the stirring is completed, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

[0128] The mass fraction of the potassium permanganate solution in this embodiment is 6%.

[0129] Example 3

[0130] A method for preparing a positive electrode material for a solid-state battery in this embodiment comprises the following steps:

[0131] Step 1: Weigh the raw materials by weight:

[0132] 60 parts of lithium iron phosphate, 10 parts of stabilizer adjusted by doping bentonite, 12.5 parts of conductive carbon black, 4 parts of carbon nanotubes, 5.5 parts of effect-adjusting reinforcing agent, 3 parts of polyvinyl alcohol, 32.5 parts of ethanol solvent, and 5.5 parts of gelatin;

[0133] Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 125 r / min for 1 hour, then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent;

[0134] Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 600 r / min for 2 hours. Stir thoroughly, and finally add gelatin and mix at the same speed for 1 hour to obtain a coating slurry;

[0135] Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 12.5µm. After coating, dry at 60°C for 2h to obtain a solid-state battery positive electrode material.

[0136] In step 2 of this embodiment, the power of ultrasonic mixing is 370 W, and the ultrasonic time is 1 h.

[0137] The preparation method of the stabilizer adjusted by doping bentonite in this embodiment is:

[0138] S01: The bentonite was heated to 175°C at a rate of 2°C / min, kept at this temperature for 7.5 min, then heated to 275°C at a rate of 3°C / min, kept at this temperature for 3.5 min, and finally cooled to room temperature in air;

[0139] S02: Preparation of modified yttrium oxide agent:

[0140] S021: treating the yttrium oxide with protons at a power of 375 W for 5 minutes to obtain irradiated yttrium oxide;

[0141] S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent;

[0142] The preparation method of the modified liquid is:

[0143] The graphene is first immersed in a sodium silicate solution with a volume of 3.5 times the total volume of the graphene, and after the immersion is completed, the graphene is filtered and dried, and 4 parts of the dried graphene, 5.5 parts of the chitosan solution, 2 parts of the silane coupling agent KH560 and 0.55 parts of citric acid are mixed to obtain a modified solution;

[0144] S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained;

[0145] S04: The bentonite agent and stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:4. After the ball milling is completed, the mixture is washed with water and dried to obtain the stabilizer adjusted by doping bentonite.

[0146] The ultrasonic power of the ultrasonic modification treatment of S022 in this embodiment is 370W, and the ultrasonic time is 25min; the immersion power of the immersion treatment is 450W, and the immersion time is 25min.

[0147] The mass fraction of the sodium silicate solution in this embodiment is 6.5%; the mass fraction of the chitosan solution is 4%;

[0148] The ball milling speed of the first-stage ball milling treatment in S03 was 500 r / min, and the ball milling lasted for 1.5 h;

[0149] The ball milling speed of the secondary ball milling treatment in S04 is 800r / min, and the ball milling time is 45min.

[0150] The stabilizer of this embodiment includes the following raw materials in parts by weight:

[0151] The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 4 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid;

[0152] 6.5 parts of hydroxyapatite solution, 3.5 parts of lanthanum chloride solution, 2 parts of nano-silica sol and 1.5 parts of nano-magnesium oxide are mixed and milled thoroughly. After the ball milling is completed, the mixture is washed with water and dried to obtain a stabilizer.

[0153] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 5.5%; the mass fraction of the lanthanum chloride solution is 3.5%.

[0154] The blending process of this embodiment is performed at a full milling speed of 1500 r / min for 1.5 h.

[0155] The preparation method of the effect-adjusting reinforcing agent of this embodiment is:

[0156] S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying;

[0157] S102: 5.5 parts of dried silicon carbide whiskers, 2 parts of stearic acid, 3 parts of carboxymethyl cellulose, and 10 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1250 r / min for 1.5 hours. After stirring, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

[0158] The mass fraction of the potassium permanganate solution in this embodiment is 4.5%.

[0159] Comparative Example 1

[0160] The difference from Example 3 is that no stabilizer for adjusting by doping bentonite is added.

[0161] Comparative Example 2

[0162] The difference from Example 3 is that the S01 step is not used in the stabilizer adjusted by doping bentonite.

[0163] Comparative Example 3

[0164] The difference from Example 3 is that the stabilizer adjusted by doping bentonite is not treated with modified yttrium oxide.

[0165] Comparative Example 4

[0166] The difference from Example 3 is that no irradiated yttrium oxide is added in the preparation of the modified yttrium oxide agent.

[0167] Comparative Example 5

[0168] The difference from Example 3 is that no modification liquid treatment is used in the preparation of the modified yttrium oxide agent.

[0169] Comparative Example 6

[0170] The difference from Example 3 is that no dry graphene is added in the preparation of the modified solution.

[0171] Comparative Example 7

[0172] The difference from Example 3 is that no stabilizer treatment is added during the preparation of the stabilizer adjusted by doping bentonite.

[0173] Comparative Example 8

[0174] The difference from Example 3 is that no effect-adjusting reinforcing agent is added.

[0175] Comparative Example 9

[0176] The difference from Example 3 is that the effect-adjusting reinforcing agent is not treated with step S102.

[0177] Comparative Example 10

[0178] The difference from Example 3 is that no hydroxyapatite liquid is added to the stabilizer.

[0179] Comparative Example 11

[0180] The difference from Example 3 is that no nano magnesium oxide is added to the stabilizer.

[0181] Comparative Example 12

[0182] The difference from Example 3 is that no lanthanum chloride solution or nano-silica sol is added to the stabilizer.

[0183] The positive electrode materials of Examples 1 to 3 and Comparative Examples 1 to 12 were assembled into solid-state batteries, and the performance test results were as follows:

[0184]

[0185] It is found from Examples 1 to 3 and Comparative Examples 1 to 12 that

[0186] The product of Example 3 of the present invention has excellent cycle capacity retention performance under the conditions of 100 cycles and 300 cycles, and the product still has excellent cycle stability under 1C conditions and 2C conditions;

[0187] It can be seen from Comparative Example 1, Comparative Example 8 and Example 3 that the product does not add a stabilizer adjusted by bentonite and does not add one of the effect-adjusting and reinforcing agents. The cycle retention rate performance of the product after 100 cycles and 300 cycles is significantly deteriorated. At the same time, the performance of the product is significantly deteriorated after 300 cycles under 2C conditions. Only when the stabilizer adjusted by bentonite and the effect-adjusting and reinforcing agent are coordinated and coordinated, the performance effect of the product is the most significant.

[0188] It can be seen from Comparative Examples 1 to 7 and Example 3 that the S01 step is not used in the stabilizer adjusted by bentonite, the modified yttrium oxide agent is not used in the stabilizer adjusted by bentonite, the irradiated yttrium oxide is not added in the preparation of the modified yttrium oxide agent, the modified yttrium oxide agent is not treated with a modifying liquid, the modified liquid is not added with dried graphene, and the stabilizer is not added in the preparation of the stabilizer adjusted by bentonite. The performance of the product has a tendency to deteriorate;

[0189] From Comparative Examples 10 to 12 and Example 3, it can be seen that when no hydroxyapatite solution, no nano magnesium oxide, no lanthanum chloride solution or nano silica sol is added to the stabilizer, the performance of the product also shows a trend of deterioration. Only when the stabilizer is obtained by the method of the present invention, the performance effect of the product is the most obvious.

[0190] The modified liquid obtained by the specific method of the present invention and the stabilizer obtained by the method of the present invention are combined with the stabilizer adjusted by doping bentonite prepared by the method of the present invention. The performance effect of the product is the most significant. The effect of other methods is not as obvious as that of the present invention.

[0191] In addition, the performance of the product also showed a trend of deterioration when the S102 step was not used in the performance-adjusting and reinforcing agent. Only the performance-adjusting and reinforcing agent prepared by the method of the present invention had the most significant performance effect.

[0192] Based on the above test, the present invention found that the product has a significant performance effect in capacity retention rate after 300 cycles at 2C, and comparative examples 1 to 12 have obvious deterioration trends to varying degrees. Based on this, the present invention conducts a low temperature resistance test on the product to test the temperature resistance stability of the product;

[0193] The test product was placed at -30°C to test the capacity retention rate of the product. The test results are as follows:

[0194]

[0195] It can be seen from Examples 1 to 3 and Comparative Examples 1 to 12 that the product still has an excellent cycle capacity retention rate at a temperature of -30°C, and the capacity retention rate is higher than 96%, and the performance stability effect of the product is remarkable. The products using Comparative Examples 1 to 12 all have a tendency to deteriorate to varying degrees, and the product does not contain any of the stabilizer or the effect-adjusting reinforcing agent doped with bentonite, and the low-temperature stability of the product deteriorates significantly. The synergistic effect of the two is used to achieve the most significant performance effect of the product.

[0196] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0197] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a solid-state battery positive electrode material, characterized in that: The following steps are involved: Step 1: Weigh the raw materials by weight: 55-65 parts of lithium iron phosphate, 8-12 parts of stabilizer adjusted by doping bentonite, 10-15 parts of conductive carbon black, 3-5 parts of carbon nanotubes, 4-7 parts of effect-adjusting reinforcing agent, 2-4 parts of polyvinyl alcohol, 30-35 parts of ethanol solvent, 4-7 parts of gelatin; Step 2: Stir polyvinyl alcohol and ethanol solvent at a speed of 100-150 r / min for 1 hour, and then add lithium iron phosphate, conductive carbon black and carbon nanotubes and mix them by ultrasonic mixing to obtain a matrix agent; Step 3: Add the stabilizer and the effect-adjusting reinforcing agent doped with bentonite to the base agent and stir at a speed of 500-700 r / min for 2 hours. Stir thoroughly, and finally add gelatin and keep the speed mixed for 1 hour to obtain a coating slurry; Step 4: Apply the coating slurry to both sides of the aluminum foil with a coating thickness of 10-15 µm. After coating, dry at 55-65 °C for 2 h to obtain a solid-state battery positive electrode material. The preparation method of the stabilizer adjusted by doping bentonite is: S01: The bentonite was heated to 170-180°C at a rate of 1-3°C / min, kept at that temperature for 5-10 minutes, then heated to 275°C at a rate of 2-4°C / min, kept at that temperature for 2-5 minutes, and finally air-cooled to room temperature; S02: Preparation of modified yttrium oxide agent: S021: irradiating the yttrium oxide with protons at a power of 350-400 W for 5 min to obtain irradiated yttrium oxide; S022: subjecting the irradiated yttrium oxide and the modified liquid to ultrasonic modification in a weight ratio of 2:5, and completing the modification to obtain a modified yttrium oxide agent; The preparation method of the modified liquid is: The graphene is first immersed in a sodium silicate solution with a volume of 2 to 5 times the total volume of the graphene, after which the immersion is completed, the solution is filtered and dried, and 3 to 5 parts of the dried graphene, 4 to 7 parts of the chitosan solution, 1 to 3 parts of the silane coupling agent KH560, and 0.4 to 0.7 parts of citric acid are mixed to obtain a modified solution; S03: The bentonite product S01 and the modified yttrium oxide agent are subjected to primary ball milling at a weight ratio of 5:3, and after the ball milling is completed, a bentonite agent adjusted with yttrium oxide is obtained; S04: The bentonite agent and the stabilizer adjusted by yttrium oxide are subjected to secondary ball milling at a weight ratio of 7:

4. After the ball milling is completed, the stabilizer is washed with water and dried to obtain a stabilizer adjusted by doping bentonite; The stabilizer comprises the following raw materials in parts by weight: The hydroxyapatite is first dispersed fully in a sodium lignin sulfonate solution which is 3 to 5 times the total amount of the hydroxyapatite to obtain a hydroxyapatite liquid; 5-8 parts of hydroxyapatite solution, 2-5 parts of lanthanum chloride solution, 1-3 parts of nano-silica sol and 1-2 parts of nano-magnesium oxide are mixed and ball-milled thoroughly, and after the ball-milling is completed, the mixture is washed with water and dried to obtain a stabilizing agent; The preparation method of the effect-adjusting reinforcing agent is as follows: S101: mixing the silicon carbide whiskers with a sufficient amount of potassium permanganate solution, and then washing and drying; S102: 4-7 parts of dry silicon carbide whiskers, 1-3 parts of stearic acid, 2-4 parts of carboxymethyl cellulose, and 8-12 parts of 5% by mass sodium dodecylbenzene sulfonate solution are mixed and stirred thoroughly at a stirring speed of 1000-1500 r / min for 1-2 hours. After the stirring is completed, the mixture is washed with water and dried to obtain an effect-adjusting reinforcing agent.

2. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The power of ultrasonic mixing in step 2 is 350-400 W, and the ultrasonic time is 1 h.

3. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The ultrasonic power of the SO22 ultrasonic modification treatment is 350-400W, and the ultrasonic time is 20-30min; the immersion power of the immersion treatment is 400-500W, and the immersion time is 20-30min.

4. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The mass fraction of the sodium silicate solution is 5-8%; the mass fraction of the chitosan solution is 3-5%; The ball milling speed of the first-stage ball milling treatment in S03 is 450~550r / min, and the ball milling is 1~2h; The ball milling speed of the secondary ball milling treatment in S04 is 750~850r / min, and the ball milling time is 35~50min.

5. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The mass fraction of the sodium lignin sulfonate solution is 4-7%; the mass fraction of the lanthanum chloride solution is 2-5%.

6. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The blending process is performed by ball milling at a speed of 1500 r / min for 1 to 2 hours.

7. The method for preparing a solid-state battery positive electrode material according to claim 1, characterized in that: The mass fraction of the potassium permanganate solution is 3-6%.

Citation Information

Patent Citations

  • Lithium ion battery positive electrode sheet containing electric-conduction coating, and preparation method thereof

    CN108511689A

  • Low-cost positive electrode prefabricated lithium, high-specific-energy electrode, manufacturing method and quasi-solid-state battery

    CN115513415A