Electrolyte and lithium ion battery
By combining electrolytes with perfluoroalkyl nitrile and ether solvents, the problem of unstable SEI film of silicon-based negative electrode materials in lithium-ion batteries is solved, and the dynamic performance and safety performance of lithium-ion batteries are improved.
Patent Information
- Application Number
- CN202411067241.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-01
AI Technical Summary
The volume expansion of silicon-based negative electrode materials in lithium-ion batteries causes instability of the SEI film, which affects cycle stability and kinetic performance. The SEI film formed by existing electrolyte solvents such as linear carbonate and cyclic carbonate has a high content of organic components. Resulting in poor performance.
Using a perfluoroalkyl nitrile and ether solvent combination electrolyte, the perfluoroalkyl nitrile improves the Li+ solvation ability and the stability of the LiF interface film. The ether solvent reduces the viscosity of the electrolyte and brings steric hindrance, forming a powerful anion. Derivatized and well-laminated SEI films.
It improves the first Coulombic efficiency, cycle performance, rate performance and safety performance of lithium-ion batteries, reduces interface side reactions and resistance, and enhances the stability and dynamic performance of the SEI film.
Smart Images

Figure CN118738568A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art
[0002] Anode materials with high specific capacity are an important breakthrough in improving the energy density of lithium-ion batteries. Silicon-based materials are considered to be the most likely anode materials to replace graphite because of their high theoretical specific capacity (Si: 4200mAh / g, SiO: 2650mAh / g), suitable discharge potential and relatively abundant reserves in nature. However, there are many problems in the commercial application of single silicon in lithium-ion batteries. First, silicon-based materials as anodes will have volume expansion problems during battery cycles, and may cause the rupture of active particles, pulverization of pole pieces and the shedding of active materials. Secondly, the silicon anode is accompanied by a large volume expansion during the first cycle. Due to the change in silicon volume, the solid electrolyte interface film (SEI) will rupture. The newly exposed silicon on the surface will produce a new SEI film, and at the same time, it will continuously consume lithium ions in the electrolyte, reducing the first coulomb efficiency. More seriously, due to the volume change of the electrode material during the cycle, the SEI film at the silicon anode interface repeatedly grows and ruptures, greatly affecting the cycle stability.
[0003] Due to the volume effect of silicon-based negative electrode materials, it is difficult for silicon-based negative electrodes to form stable solid electrolyte interface films in the electrolyte, and the electrode structure is destroyed during the battery cycle. New solid electrolyte interface films will continue to form on the exposed silicon-based surface, leading to corrosion of the negative electrode material and capacity attenuation.
[0004] Currently, commonly used electrolyte solvents are linear carbonates and cyclic carbonates, such as dimethyl carbonate, ethyl methyl carbonate, ethylene carbonate and propylene carbonate. The SEI film formed by these solvents has a high content of organic components, resulting in poor SEI film stability and lithium-ion battery kinetic performance. Summary of the invention
[0005] In order to solve the technical problem in the above-mentioned prior art that when the electrolyte solvent is linear carbonate and cyclic carbonate, the formed SEI film has a high organic component content, resulting in poor SEI film stability and lithium ion battery kinetic performance, the purpose of the present invention is to provide an electrolyte and a lithium ion battery.
[0006] The present invention provides an electrolyte, the electrolyte comprising a perfluoroalkyl nitrile and an ether solvent, the general structural formula of the perfluoroalkyl nitrile being at least one of the following formula (I) and formula (II), and the general structural formula of the ether solvent being at least one of the following formula (III) and formula (IV):
[0007]
[0008] Wherein, R1 is -(CF2)n, and n is an integer from 3 to 8;
[0009] R2 is -(CF2)m, m is 4 to 8;
[0010] R3 and R4 are each independently propyl or butyl;
[0011] R5 and R6 are each independently methyl, ethyl, propyl, butyl or pentyl.
[0012] The electrolyte of the present invention comprises a perfluoroalkyl nitrile solvent. In a first aspect, the perfluoroalkyl nitrile solvent contains a large amount of fluorine and exhibits a low Li + Solvation ability, thereby improving the kinetic performance of lithium-ion batteries; secondly, perfluoroalkyl nitrile solvents are also easy to form LiF interface films, and the formed LiF interface films have high stability and ionic conductivity, which can improve the initial coulombic efficiency, cycle performance and rate performance of lithium-ion batteries; thirdly, the electrolyte containing perfluoroalkyl nitrile solvents has good stability at high voltage, reducing interface side reactions; fourthly, the nitrile has good thermal stability and contains nitrogen elements, which can improve the safety performance of lithium-ion batteries. Furthermore, since perfluoroalkyl nitrile solvents have a high viscosity, the present invention uses a combination of low-viscosity ether solvents and perfluoroalkyl nitrile solvents. On the one hand, the viscosity of the electrolyte is significantly reduced, thereby increasing the lithium ion transfer rate, which can effectively improve the rate performance of lithium-ion batteries; on the other hand, the terminal groups of the ether solvents provided by the present invention will bring great steric hindrance, thereby greatly reducing the ether solvents to Li + The electrolyte-ether solvent contains a large amount of contact ion pairs (CIP) and ion aggregates (AGG). Compared with the ether-based separation solvent-ion pairs (SSIPs) in the prior art, the anion-rich solvent configuration of the present invention has a higher reduction priority on the silicon surface, which helps to form a strong anion-derived and well-layered SEI film. The electrolyte of the present invention improves the stability of the SEI film and the kinetic performance of the lithium-ion battery through the synergistic effect of perfluoroalkyl nitrile solvents and ether solvents, effectively improving the first coulombic efficiency, cycle performance and rate performance of the lithium-ion battery, and the electrolyte of the present invention is also thermally stable, which improves the safety performance of the lithium-ion battery.
[0013] Preferably, the perfluoroalkyl nitrile comprises at least one of the following structural formulas:
[0014]
[0015] The perfluoroalkyl nitrile described in this scheme includes at least one of the above-mentioned structural formulas perfluoroheptanenitrile, perfluorooctanonitrile, and 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9-hexafluorodecane dinitrile. The above-mentioned perfluoroalkyl nitrile can further improve the stability of the SEI film, the kinetic performance of the lithium ion battery, and the safety performance of the lithium ion battery.
[0016] Preferably, the ether solvent comprises at least one of the following structural formulas:
[0017]
[0018] The ether solvent described in this scheme includes at least one of the above-mentioned structural formulas ethylene glycol dibutyl ether, diethylene glycol diethyl ether, and diethylene glycol dibutyl ether, which can effectively reduce the viscosity of the electrolyte and increase the lithium ion transmission rate, thereby reducing the internal resistance of the lithium ion battery, and has a sufficiently large sterically hindered terminal group to further reduce the Li + The solubility ability of the anion-rich solvent configuration helps to form a strong anion-derived and well-layered SEI film on the silicon surface.
[0019] Preferably, the electrolyte further comprises linear carbonate and cyclic carbonate.
[0020] Preferably, the mass ratio of the linear carbonate to the cyclic carbonate is 10:(5-25).
[0021] Preferably, the linear carbonate includes at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC).
[0022] Preferably, the cyclic carbonate includes at least one of ethylene carbonate (EC), fluoroethylene carbonate (FEC), and propylene carbonate (PC).
[0023] Preferably, the mass ratio of the perfluoroalkyl nitrile to the ether solvent is (30-60):(20-40).
[0024] The mass ratio of the perfluoroalkyl nitrile and the ether solvent in the present embodiment is (30-60): (20-40). When the mass ratio of the perfluoroalkyl nitrile and the ether solvent in the electrolyte is within this range, the thermal stability of the electrolyte, the stability of the SEI film and the kinetic performance of the lithium-ion battery can be further improved, and the viscosity of the electrolyte can be fully reduced, thereby increasing the lithium ion transmission rate and reducing the internal resistance of the lithium-ion battery.
[0025] Preferably, the electrolyte further comprises a fluorine-containing lithium salt, and the fluorine-containing lithium salt comprises LiPF6, LiPO2F2 and LiDFOB.
[0026] The fluorine-containing lithium salts described in this scheme include LiPF6, LiPO2F2 and LiDFOB. These three fluorine-containing lithium salts can form dense and high-strength LiF, improve the stability of SEI film and the kinetic performance of lithium-ion batteries; LiPO2F2, as a lithium salt additive, can form a SEI film rich in LixPOyFz and LiF components on the surface of the negative electrode, which is beneficial to reduce the battery interface impedance and improve the battery cycle performance; LiDFOB has good thermal stability, and will preferentially reduce and oxidize with solvent molecules on the surface of the negative electrode and high-nickel positive electrode to form a strong, highly electronically insulating boron-rich interface film, which effectively inhibits the consumption of active lithium and the serious decomposition of the electrolyte. Therefore, the three fluorine-containing lithium salts LiPF6, LiPO2F2 and LiDFOB work synergistically in the electrolyte of this scheme, effectively improving the first cycle coulomb efficiency, ring performance and rate performance of lithium-ion batteries.
[0027] Preferably, in the electrolyte, the concentration of LiPF6 is 1.3-2 mol / L, the mass fraction of LiPO2F2 is 0.5%-1%, and the mass fraction of LiDFOB is 0.1%-0.3%.
[0028] In the electrolyte of this scheme, the concentration of LiPF6 is 1.3-2 mol / L, the mass fraction of LiPO2F2 is 0.5%-1%, and the mass fraction of LiDFOB is 0.1%-0.3%. The concentrations of these three fluorine-containing lithium salts are within this range. Firstly, a SEI film rich enough in LixPOyFz and LiF components can be formed, which is beneficial to reducing the battery interface impedance; secondly, a sufficiently strong, highly electronically insulating boron-rich interface film can be formed, which effectively inhibits the consumption of active lithium and the serious decomposition of the electrolyte; thirdly, it can ensure that LiPO2F2 and LiDFOB with sufficient strong redox ability preferentially react to form a film on the surface of the positive and negative electrodes to protect the solvent; fourthly, LiPO2F2 and LiDFOB can be fully dissolved in the solvent and avoid precipitation in the later stage of the cycle.
[0029] The present invention also provides a lithium ion battery comprising the electrolyte. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0031] Example 1
[0032] The structural formula of the perfluoroalkyl nitrile used in the electrolyte of this embodiment is as follows:
[0033]
[0034] Perfluorooctanonitrile
[0035] Preparation of electrolyte
[0036] S1. Mix dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), perfluoroalkyl nitrile, and ethylene glycol dibutyl ether in a mass ratio of 10:5:5:50:30, and stir until uniformly mixed to obtain a first mixture;
[0037] S2. Add lithium hexafluorophosphate LiPF6 to the first mixture and stir, and after stirring and mixing evenly, obtain a second mixture;
[0038] S3. Add lithium salt additives lithium difluorophosphate LiPO2F2 and lithium difluorooxalate borate LiDFOB to the second mixture and stir. After stirring and mixing evenly, an electrolyte is obtained. In the electrolyte of this embodiment, the concentration of LiPF6 is 1.5 mol / L, the mass fraction of LiPO2F2 is 0.8%, and the mass fraction of LiDFOB is 0.2%.
[0039] Example 2
[0040] The perfluoroalkyl nitrile used in the preparation of the electrolyte of this embodiment is perfluoroheptanenitrile, and the structural formula is as follows:
[0041] Other than that, the same as in Example 1.
[0042] Example 3
[0043] The perfluoroalkyl nitrile used in the preparation of the electrolyte of this embodiment is 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9-hexafluorodecanonitrile, the structural formula of which is as follows:
[0044] Other than that, the same as in Example 1.
[0045] Example 4
[0046] The perfluoroalkyl nitrile used in the preparation of the electrolyte of this embodiment is 19-fluorodecane nitrile, and the structural formula is as follows:
[0047] Other than that, the same as in Example 1.
[0048] Example 5
[0049] The ether solvent used in the preparation of the electrolyte of this embodiment is diethylene glycol diethyl ether, and the structural formula is as follows:
[0050] Other than that, the same as in Example 1.
[0051] Example 6
[0052] The ether solvent used in the preparation of the electrolyte of this embodiment is ethylene glycol dipropyl ether, and the structural formula is as follows:
[0053] Other than that, the same as in Example 1.
[0054] Example 7
[0055] The preparation of the electrolyte of this embodiment is the same as that of Embodiment 1, except that the mass ratio of dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), perfluoroalkyl nitrile, and ethylene glycol dibutyl ether is 10:5:5:70:10.
[0056] Example 8
[0057] The preparation of the electrolyte of this embodiment is the same as that of Embodiment 1, except that the mass ratio of dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), ethylene carbonate (EC), perfluoroalkyl nitrile, and ethylene glycol dibutyl ether is 10:5:5:20:60.
[0058] Example 9
[0059] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of LiPO2F2 is 1.3% and the mass fraction of LiDFOB is 0.5%.
[0060] Example 10
[0061] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of LiPO2F2 is 0.3% and the mass fraction of LiDFOB is 0.05%.
[0062] Comparative Example 1
[0063] The preparation of the electrolyte of this comparative example is the same as that of Example 1, except that the mass of ethylene glycol dibutyl ether and perfluoroalkyl nitrile in Example 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 10:5:5).
[0064] Comparative Example 2
[0065] The preparation of the electrolyte of this comparative example is the same as that of Example 1, except that the mass of perfluoroalkyl nitrile in Example 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 10:5:5).
[0066] Comparative Example 3
[0067] The preparation of the electrolyte of this comparative example is the same as that of Example 1, except that the mass of ethylene glycol dibutyl ether in Example 1 is replaced by the base solvent (DMC, FEC, and EC are configured as the base solvent in a mass ratio of 10:5:5).
[0068] Comparative Example 4
[0069] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that heptafluorobutyronitrile is used to replace the perfluoroalkyl nitrile in Example 1. The structural formula of heptafluorobutyronitrile is as follows:
[0070]
[0071] Comparative Example 5
[0072] The preparation of the electrolyte of this comparative example is the same as that of Example 1 except that the following structural perfluoroalkyl nitrile is used to replace the perfluoroalkyl nitrile in Example 1. The structural formula of the perfluoroalkyl nitrile used in the electrolyte of this comparative example is as follows:
[0073]
[0074] Comparative Example 6
[0075] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that 2-fluorosuccinonitrile is used to replace the perfluoroalkyl nitrile in Example 1. The structural formula of 2-fluorosuccinonitrile is as follows:
[0076]
[0077] Comparative Example 7
[0078] The preparation of the electrolyte in this comparative example is the same as that in Example 1 except that ethylene glycol dimethyl ether is used to replace ethylene glycol dibutyl ether in Example 1.
[0079] Preparation of lithium-ion batteries
[0080] (1) Preparation of positive electrode sheet
[0081] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3 and added to a solvent N-methylpyrrolidone (NMP). The mixture is evenly mixed to obtain a positive electrode slurry with a solid content of 45%. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil to form a positive electrode active coating. After vacuum drying, a positive electrode sheet is obtained.
[0082] (2) Preparation of negative electrode sheet
[0083] Silicon-carbon negative electrode material (SiC), conductive agent conductive carbon black (SP), single-walled carbon nanotubes (SWCNT) and binder polyacrylic acid (PAA) are mixed in a mass ratio of 80:9:1:10 and added to a solvent deionized water, mixed evenly, to prepare a negative electrode slurry with a solid content of 25%, and the negative electrode slurry is coated on both surfaces of the negative electrode current collector copper foil to form a negative electrode active coating, and after vacuum drying, a negative electrode sheet is prepared.
[0084] (3) Selection of electrolyte
[0085] The electrolytes obtained in the above-mentioned embodiments and comparative examples and the common electrolyte of the control group (EC:DMC:DEC mass ratio of 30:40:30, LiPF6 1 mol / L) were selected to prepare lithium-ion batteries.
[0086] (4) Selection of isolation membrane
[0087] The isolation film includes a polyethylene (PE) film and ceramic layers respectively arranged on two surfaces of the PE film, wherein the total thickness of the two ceramic layers is 3 μm, the thickness of the PE film is 9 μm, and the total thickness of the isolation film is 12 μm.
[0088] (5) Preparation of lithium-ion batteries
[0089] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, and the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, so as to prepare a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0090] Performance Testing
[0091] The rate performance of the battery was tested under lithium-ion battery test conditions. The battery was tested at room temperature (25°C) on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage was limited to 2.5V~4.2V, and a high voltage cycle of 2.5~4.4V was designed. The first coulomb efficiency (first efficiency), cycle performance and rate performance are shown in Table 1 below.
[0092] 1) First Coulomb efficiency
[0093] At 25°C, the lithium-ion battery was charged to 4.2V at a constant current and constant voltage rate of 0.33C and allowed to stand for 10 minutes. Then, the lithium-ion battery was discharged to 2.5V at a constant current rate of 0.33C and allowed to stand for 10 minutes. The first coulombic efficiency of the lithium-ion battery was calculated.
[0094] First coulombic efficiency (%) = total capacity of the lithium-ion battery discharged at 0.33C for the first time / total capacity of the lithium-ion battery charged at 0.33C for the first time × 100%.
[0095] 2) Room temperature 2.5 ~ 4.2V, 1C / 1C cycle 900 weeks capacity retention rate
[0096] At 25°C, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0097] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0098] 3) 2.5~4.4V at room temperature, 1C / 1C cycle 900 weeks capacity retention rate
[0099] At 25°C, the lithium-ion battery is charged to 4.4V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0100] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0101] 4) 1C / 8C discharge capacity retention rate at room temperature
[0102] At 25°C, the divided lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C; it is left to stand for 10 minutes; then the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C, and its discharge capacity Q is recorded. 1C As the initial discharge capacity; then charge the lithium-ion battery to 4.2V at 1C rate at 25°C, with a cut-off current of 0.05C; let it stand for 10 minutes; then discharge the fully charged battery to 2.5V at 8C rate, and record its discharge capacity Q 8C ; Calculate the discharge capacity retention rate (%) of the lithium-ion battery at 1C / 8C rate = discharge capacity Q at 8C rate 8C / Discharge capacity at 1C rate Q 1C ×100%.
[0103] 5) Battery thermal runaway ARC (adiabatic accelerated calorimeter) test
[0104] The lithium-ion battery is heated from room temperature to 45±2℃ in the chamber. After being left for 90 minutes, the temperature rise rate of the battery is detected. If the temperature rise exceeds 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR>0.02℃ / min), it is considered that a self-exothermic reaction occurs inside the lithium-ion battery, and the adiabatic environment is maintained until the lithium-ion battery has thermal runaway; if the temperature rise does not exceed 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR≤0.02℃ / min), continue to the next step temperature rise test; each temperature step is 5℃, and the steps are repeated on each step. The ARC test temperature range is 45-300℃, the self-heating starting temperature is T1 (temperature rise rate SHR>0.02℃ / min), and the thermal runaway starting temperature is T2 (temperature rise rate SHR>1℃ / min).
[0105] Table 1
[0106]
[0107]
[0108] From the analysis of Table 1, we can see that:
[0109] After the electrolytes of Examples 1 to 10 of the present invention are used to prepare lithium-ion batteries, they show good performance in the first coulombic efficiency, cycle capacity retention rate (including 2.5 to 4.2V cycles and high voltage cycles 2.5 to 4.4V), high-rate discharge capacity retention rate (fast charge and discharge) and battery thermal runaway ARC test (self-heating starting temperature T1 and thermal runaway starting temperature T2), while Comparative Examples 1 to 7 and the control group do not belong to the technical scheme of the present invention, so their performance in the above four aspects is significantly deteriorated. This fully demonstrates that the electrolyte prepared using the technical scheme of the present invention is applied to lithium batteries, which can effectively improve the first coulombic efficiency, cycle performance, rate performance and thermal stability (i.e., safety performance) of lithium-ion batteries.
[0110] The perfluoroalkyl nitrile in the electrolyte of Example 2 is perfluoroheptanenitrile, the perfluoroalkyl nitrile in the electrolyte of Example 4 is 19fluorodecanenitrile, the perfluoroalkyl nitrile in the electrolyte of Comparative Example 4 is heptafluorobutyronitrile, and Comparative Example 5 uses a chain perfluoroalkyl nitrile containing twelve carbon atoms. From the test results in Table 1, the lithium-ion batteries prepared using the electrolytes of Examples 2 and 4 also show good technical effects in the first coulomb efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test; while the technical effects of Comparative Examples 4 and 5 in the above four aspects are significantly reduced. This shows that in the technical solution of the present invention, the carbon number of the chain perfluoroalkyl nitrile used is in the range of 5 to 10, which is a necessary technical feature to achieve the technical effect of the present invention.
[0111] The perfluoroalkyl nitrile in the electrolyte of Example 3 is 2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9-hexafluorodecanedinitrile, which belongs to the class of perfluoroalkyl dinitrile compounds. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Example 3 also shows good technical effects in the first coulombic efficiency, cycle capacity retention rate, high rate discharge capacity retention rate and battery thermal runaway ARC test.
[0112] The ether solvent in the electrolyte of Example 5 is diethylene glycol diethyl ether, and the ether solvent in the electrolyte of Example 6 is ethylene glycol dipropyl ether. The structural formula of diethylene glycol diethyl ether is compared with that of ethylene glycol dibutyl ether in Example 1, which is equivalent to that the butyl group at the end of the structural formula of ethylene glycol dibutyl ether is replaced by propoxyethyl and ethyl, respectively. The steric hindrance of propoxyethyl is also large, thereby greatly reducing the ether solvent to Li + The electrolyte-ether solvent contains a large number of contact ion pairs (CIP) and ion aggregates (AGG), and the anion-rich solvent configuration has a higher reduction priority on the silicon surface, which helps to form a strong anion-derived and well-layered SEI film. The ethyl steric hindrance at the end of diethylene glycol diethyl ether is smaller than the butyl group in ethylene glycol dibutyl ether in Example 1. Therefore, from the test results in Table 1, the technical effect of the lithium-ion battery prepared using the electrolyte of Example 5 in the high-rate discharge capacity retention test is reduced. The ether solvent in the electrolyte of Example 6 is ethylene glycol dipropyl ether. Since the end of the structural formula of ethylene glycol dipropyl ether is propyl, it is smaller than the butyl group in ethylene glycol dibutyl ether in Example 1, which reduces the ether solvent to Li + The dissolving ability of the electrolyte is weakened, the contact ion pairs (CIP) and ion aggregates (AGG) contained in the electrolyte-ether solvent are reduced, the anion-rich solvent configuration is reduced, and the formation of a strong anion-derived and well-layered SEI film is reduced. Therefore, from the test results in Table 1, the technical effects of the lithium-ion battery prepared using the electrolyte of Example 6 in the first coulomb efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test are not as good as those of Example 1 and Example 5.
[0113] Compared with Example 1, the electrolyte of Example 7 uses more perfluoroalkyl nitrile - the mass ratio of perfluoroalkyl nitrile to ether solvent is 70:10, and the electrolyte of Example 8 uses less perfluoroalkyl nitrile - the mass ratio of perfluoroalkyl nitrile to ether solvent is 20:60. Both Example 7 and Example 8 are not within the further preferred range of the mass ratio of perfluoroalkyl nitrile to ether solvent of (30-60): (20-40). In Example 7, the amount of perfluoroalkyl nitrile used is relatively large, the viscosity of the prepared electrolyte is relatively large, and the lithium ion transmission rate is reduced. From the test results in Table 1, the technical effects of the lithium ion battery prepared using the electrolyte of Example 7 in the high-rate discharge capacity retention rate and battery thermal runaway ARC test are reduced. In Example 8, the amount of perfluoroalkyl nitrile used is relatively small, which leads to the formation of less LiF interface film with high stability and ionic conductivity, and the thermal stability and stability of the electrolyte at high voltage are reduced, as well as the reduction of Li + The solvation capacity is also reduced, and the technical effects of the lithium-ion battery prepared using the electrolyte of Example 8 in terms of cycle capacity retention (2.5-4.4V) and battery thermal runaway ARC test are reduced.
[0114] Compared with Example 1, the mass fractions of LiPO2F2 and LiDFOB in the electrolytes of Examples 9 and 10 are not within a further preferred range—the mass fraction of LiPO2F2 is 0.5% to 1%, and the mass fraction of LiDFOB is 0.1% to 0.3%. The mass fractions of LiPO2F2 and LiDFOB in the electrolyte of Example 9 are both greater than the preferred range, and the mass fractions of LiPO2F2 and LiDFOB in the electrolyte of Example 10 are both less than the preferred range. From the test results in Table 1, the technical effects of the lithium-ion batteries prepared using the electrolytes of Examples 9 and 10 in the first coulombic efficiency, cycle capacity retention rate, high rate discharge capacity retention rate, and battery thermal runaway ARC test are reduced.
[0115] Compared with Example 1, Comparative Example 1 does not use perfluoroalkyl nitrile and ether solvent, that is, the solvent is only the base solvent (DMC, FEC, EC are configured as the base solvent according to the mass ratio of 10:5:5), Comparative Example 2 does not use perfluoroalkyl nitrile, that is, the solvent is the base solvent and the ether solvent, and Comparative Example 3 does not use an ether solvent, that is, the solvent is the base solvent and perfluoroalkyl nitrile. From the test results in Table 1, the lithium ion batteries prepared using the electrolytes of Comparative Examples 1 to 3 have significantly reduced technical effects in the first coulomb efficiency, cycle capacity retention rate, high rate discharge capacity retention rate and battery thermal runaway ARC test. This shows that in the technical solution of the present invention, if only perfluoroalkyl nitrile or ether solvent is used alone to prepare the electrolyte, and the electrolyte is applied to lithium ion batteries, the technical effects of the above four aspects are significantly reduced.
[0116] Comparative Example 6 uses 2-fluorosuccinonitrile, which is not perfluorinated. From the test results in Table 1, the lithium-ion battery prepared using the electrolyte of Comparative Example 6 has significantly reduced technical effects in the first coulombic efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test.
[0117] Comparative Example 7 uses ethylene glycol dimethyl ether to replace the ethylene glycol dibutyl ether in Example 1. The terminal of the ethylene glycol dimethyl ether structure is a methyl group, which is much smaller than the butyl group in the ethylene glycol dibutyl ether in Example 1, thereby reducing the ether solvent's effect on Li + The dissolving ability is significantly weakened, the contact ion pairs (CIP) and ion aggregates (AGG) contained in the electrolyte-ether solvent are significantly reduced, the anion-rich solvent configuration is significantly reduced, and the formation of a strong anion-derived and well-layered SEI film is significantly reduced. From the test results in Table 1, the lithium-ion battery prepared using the electrolyte of Comparative Example 7 has significantly reduced technical effects in the first coulombic efficiency, cycle capacity retention rate, high-rate discharge capacity retention rate and battery thermal runaway ARC test, which shows that even if an ether solvent with low viscosity but small structural terminal steric hindrance is used, the technical effects of the above four aspects are also significantly reduced. The ether solvent in the technical solution of the present invention needs to simultaneously meet the technical characteristics of low viscosity and large structural terminal steric hindrance.
[0118] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte comprises a perfluoroalkyl nitrile and an ether solvent, wherein the general structural formula of the perfluoroalkyl nitrile is at least one of the following formula (I) and formula (II), and the general structural formula of the ether solvent is at least one of the following formula (III) and formula (IV): Wherein, R1 is -(CF2)n, and n is an integer from 3 to 8; R2 is -(CF2)m, m is 4 to 8; R3 and R4 are each independently propyl or butyl; R5 and R6 are each independently methyl, ethyl, propyl, butyl or pentyl.
2. The electrolyte according to claim 1, characterized in that: The perfluoroalkyl nitrile comprises at least one of the following structural formulas:
3. The electrolyte according to claim 1, characterized in that: The ether solvent includes at least one of the following structural formulas:
4. The electrolyte according to claim 1, characterized in that: The electrolyte also includes linear carbonates and cyclic carbonates.
5. The electrolyte according to claim 4, characterized in that: The linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate and methyl propyl carbonate.
6. The electrolyte according to claim 4, characterized in that: The cyclic carbonate includes at least one of ethylene carbonate, fluoroethylene carbonate and propylene carbonate.
7. The electrolyte according to claim 1, characterized in that: The mass ratio of the perfluoroalkyl nitrile to the ether solvent is (30-60):(20-40).
8. The electrolyte according to claim 1, characterized in that: The electrolyte also includes a fluorine-containing lithium salt, and the fluorine-containing lithium salt includes LiPF6, LiPO2F2 and LiDFOB.
9. The electrolyte according to claim 8, characterized in that: In the electrolyte, the concentration of LiPF6 is 1.3-2 mol / L, the mass fraction of LiPO2F2 is 0.5%-1%, and the mass fraction of LiDFOB is 0.1%-0.3%.
10. A lithium ion battery, characterized in that: Comprising the electrolyte as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Electrolyte and lithium-ion battery
CN109888383A
Non-aqueous electrolyte and lithium ion battery
CN110911753A
Flame retardants for battery electrolytes
CN117157792A
Nonaqueous electrolytic solution and lithium secondary battery
KR1020180050781A
Lithium metal battery and electronic apparatus