Method for recycling positive electrode material of retired lithium iron phosphate battery

Through the methods of crushing treatment, solvent soaking and wet ball milling followed by sintering, the problem of complex recycling process and secondary pollution of lithium iron phosphate cathode material is solved, efficient and environmentally friendly low carbon content cathode material is prepared, and the utilization rate of metal raw materials is improved. and battery performance.

CN118738633AActive Publication Date: 2024-10-01ZHEJIANG SHANGAO NEW ENERGY CO LTD

Patent Information

Application Number
CN202410713870.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

The existing recycling method of lithium iron phosphate cathode materials is complex and requires a large amount of acid and alkali reagents, which can easily cause secondary pollution. Moreover, the recycled materials have high carbon content and low effective active material content, which affects the energy density.

Method used

After crushing treatment, stir and soak in a solvent, perform ICP detection and add lithium, iron, and phosphorus sources, perform wet ball milling with grinding aids, and then sinter under a nitrogen atmosphere to prepare low-carbon lithium iron phosphate cathode materials. .

Benefits of technology

The process is simplified, the loss of valuable metals is reduced, and the utilization rate of metal raw materials is improved. The obtained cathode material has high gram capacity, good cycle stability and rate performance, and meets the requirements of the battery industry.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of lithium battery material recovery, in particular to a method for recycling a positive electrode material of a retired lithium iron phosphate battery. The method comprises the following steps: crushing a recycled retired lithium iron phosphate battery positive electrode material, adding a solvent into a fragment material, stirring and soaking, filtering, repeatedly washing filter residues with deionized water, and drying to obtain recycled positive electrode material coarse powder; performing ICP (inductively coupled plasma) detection on the coarse powder, supplementing a lithium source, an iron source, a phosphorus source, a grinding aid and absolute ethyl alcohol for wet ball milling, and drying after ball milling to obtain a precursor; and sintering in a nitrogen atmosphere to obtain the lithium iron phosphate positive electrode material. The method for recycling the positive electrode material of the decommissioned lithium iron phosphate battery is simple in process, green, environment-friendly and good in economic benefit, and the recycled positive electrode material meets the use requirements of the battery industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery material recycling, and in particular to a method for recycling retired lithium iron phosphate battery positive electrode materials. Background Art

[0002] While the new energy vehicle industry is growing rapidly, retired power batteries are also increasing year by year, and have begun to become a difficult problem that the industry needs to solve urgently. If a reasonable business model cannot be found, it will undoubtedly become a major hidden danger for the development of the electric vehicle industry. Data show that the cumulative retirement volume of power batteries in my country in 2020 was about 200,000 tons, and the cumulative retirement volume in 2025 is expected to be about 780,000 tons. If calculated based on the current installed capacity of 50kWh to 70kWh power batteries for electric vehicles, then assuming that 600,000 electric vehicles are retired, the corresponding retired power batteries will reach 30GWh. This is an unavoidable problem for new energy vehicles.

[0003] A method for recovering positive electrode materials, the obtained positive electrode materials and their uses (Patent Publication No.: CN111799522B) The method comprises the following steps: sintering the positive electrode materials to be recovered in an oxidizing atmosphere to obtain positive electrode materials; the gas in the oxidizing atmosphere comprises CO2. The present invention aims at the problems in the prior art that the carbon content in the recovered positive electrode materials is significantly high, the content of effective active substances is low, and the energy density is reduced. The present invention adopts an oxidizing atmosphere containing CO2 as a basic oxidant to remove excess carbon components in the recovered positive electrode materials. The obtained positive electrode materials have less carbon content, good cycle stability and rate performance, carbon content ≤2.86wt%, and 200-cycle capacity retention rate ≥99.0%.

[0004] A method for wet recycling and reuse of waste lithium iron phosphate positive electrode materials (patent publication number: CN116281916A) comprises separating waste lithium iron phosphate batteries to obtain lithium-containing positive electrode material powder; soaking the lithium-containing positive electrode material powder in an organic solvent; pressing the lithium positive electrode material powder and a binder into blocks and calcining them to obtain a mixture; subjecting the mixture and a reducing agent to high-temperature vacuum reduction, vacuum distillation and vacuum condensation in sequence to obtain metallic lithium and residue; dissolving the residue in an inorganic acid solution and adding a precipitant, and drying the precipitate; heating the dried precipitate, and cooling it to room temperature to obtain battery-grade iron phosphate.

[0005] At present, the recycling of lithium iron phosphate positive electrode materials is mainly based on wet recycling, but this method has a relatively complicated process and requires the use of a large amount of acid and alkali reagents, which can easily cause secondary pollution.

[0006] Based on this, the present invention proposes a method for recycling retired lithium iron phosphate battery positive electrode materials. Summary of the invention

[0007] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a method for recycling retired lithium iron phosphate battery positive electrode materials, which improves the utilization rate of metal raw materials and reduces the loss of valuable metals. The method is economical, environmentally friendly and efficient.

[0008] Another aspect of the present invention provides a positive electrode material for a lithium iron phosphate battery prepared by the above method.

[0009] The purpose of the present invention is achieved through the following technical solutions:

[0010] A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that it comprises the following steps:

[0011] Step 1: crush 100-450 parts of recycled retired lithium iron phosphate battery positive electrode materials, add 1500-6000 parts of solvent to the fragments, stir and soak for 60-120 minutes, filter and repeatedly wash the residue with deionized water and dry to obtain coarse powder of recycled positive electrode materials;

[0012] Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 8-12 hours, and then dried to obtain a precursor;

[0013] Step 3: The precursor is sintered in a nitrogen atmosphere for 2-5 hours to obtain a lithium iron phosphate positive electrode material.

[0014] Optionally, the solvent in step 1 is selected from at least one of N-methylpyrrolidone, acetone, ethylene glycol, N-dimethylacetamide, dimethyl sulfoxide, and tetrahydrofuran.

[0015] Optionally, after the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1-1.12:0.92-1.

[0016] Optionally, in step 2, the phosphorus source is selected from at least one of phosphoric acid, iron phosphate, lithium phosphate, and lithium dihydrogen phosphate.

[0017] Optionally, in step 2, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate.

[0018] Optionally, the iron source in step 2 is selected from at least one of ferrous phosphate, ferrous sulfate, and ferrous oxalate.

[0019] Optionally, in the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball milling is 1:1.5-2:0.8-1.2.

[0020] Optionally, the grinding aid in the ball milling in step 2 accounts for 1-5% of the material mass percentage.

[0021] Optionally, the preparation method of the grinding aid in the ball milling of step 2 is:

[0022] By weight, 2-5 parts of dilithium mercaptosuccinate, 15-30 parts of monoethanolamine thioglycolate, and 20-40 parts of ethylene glycol diglycidyl ether are added to a stirring kettle, and mechanical stirring is continued while N2 protection is passed. After heating to 90-100° C., 3-6 parts of 1,8-bisdimethylaminonaphthalene are added, and the reaction is carried out for 60-120 minutes to obtain a grinding aid.

[0023] Optionally, the sintering temperature in step three is 650-900°C.

[0024] The beneficial effects achieved by the present invention using the above technical solution are as follows:

[0025] In this scheme, dilithium mercaptosuccinate and monoethanolamine thioglycolate are respectively reacted with ethylene glycol diglycidyl ether to undergo a mercapto-epoxy addition reaction, and the mercapto functional group loses chloride ions under the action of 1,8-bisdimethylaminonaphthalene to form a thiol anion and a conjugate acid of a catalyzer; the thiol anion has a strong nucleophilicity, and the epoxy functional group forms an alkoxide anion intermediate after ring opening; the thiol anion can capture hydrogen ions of a potential hydrogen source in the reaction system to form a grinding aid.

[0026] The lithium succinate complex can enhance the interaction between particles and promote the fragmentation and mixing of particles. Ethanolamine can reduce the surface tension between particles, help the dispersion of particles and the lubrication during the milling process, reduce the friction between particles, and improve the ball milling efficiency. Ethylene glycol may play a humidifying role in the ball milling process, keep the surface of the particles wet, and help the milling and mixing of particles. The role of the grinding aid may include enhancing the interaction between particles, reducing surface tension, providing lubrication and humidification, thereby promoting the milling and mixing of particles and improving the ball milling efficiency.

[0027] The method for recycling retired lithium iron phosphate battery positive electrode materials is simple in process, green and environmentally friendly, and has good economic benefits. The gram capacity of the positive electrode material after recycling is above 153 mAh / g, and the first efficiency is above 96.3%, which meets the use requirements of the battery industry. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0030] Example test method:

[0031] The positive electrode materials prepared in the examples and comparative examples were assembled into button batteries CR2032, and charge and discharge tests were performed under the conditions of 4.0-2.5V and 0.1C.

[0032] Example 1

[0033] A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that it comprises the following steps:

[0034] Step 1: 100g of recycled retired lithium iron phosphate battery positive electrode material is crushed, 1500g of solvent is added to the fragmented material, stirred and soaked for 60 minutes, and the filter residue is repeatedly washed with deionized water and dried to obtain a coarse powder of the recycled positive electrode material;

[0035] Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 8 hours, and then dried to obtain a precursor;

[0036] Step 3: The precursor is sintered in a nitrogen atmosphere for 2 hours to obtain a lithium iron phosphate positive electrode material.

[0037] The solvent in step 1 is selected from N-methylpyrrolidone.

[0038] After the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1:0.92.

[0039] In the step 2, the phosphorus source is selected from phosphoric acid.

[0040] In the step 2, the lithium source is selected from lithium carbonate.

[0041] In the step 2, the iron source is selected from ferric phosphate.

[0042] In the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball mill is 1:1.5:0.8.

[0043] In the ball milling of step 2, the grinding aid accounts for 1% of the material mass percentage.

[0044] The preparation method of the grinding aid in the ball milling of step 2 is:

[0045] 2 g of dilithium mercaptosuccinate, 15 g of monoethanolamine thioglycolate, and 20 g of ethylene glycol diglycidyl ether were added to a stirring vessel, and mechanical stirring was continued while N2 protection was passed. After heating to 90° C., 3 g of 1,8-bisdimethylaminonaphthalene was added and the reaction was carried out for 60 minutes to obtain a grinding aid.

[0046] The sintering temperature in step three is 650°C.

[0047] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 153.2 mAh / g and a first efficiency of 96.3%.

[0048] Example 2

[0049] A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that it comprises the following steps:

[0050] Step 1: 250g of recycled retired lithium iron phosphate battery positive electrode material was crushed, 3000g of solvent was added to the fragmented material, stirred and soaked for 90 minutes, and the filter residue was repeatedly washed with deionized water and dried to obtain a coarse powder of the recycled positive electrode material;

[0051] Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 10 hours, and then dried to obtain a precursor;

[0052] Step 3: The precursor is sintered for 3 hours in a nitrogen atmosphere to obtain a lithium iron phosphate positive electrode material.

[0053] The solvent in step 1 is selected from acetone.

[0054] After the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1.06:0.94.

[0055] In the step 2, the phosphorus source is selected from lithium phosphate.

[0056] In the step 2, the lithium source is selected from lithium carbonate.

[0057] In the step 2, the iron source is selected from ferrous sulfate.

[0058] In the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball mill is 1:1.6:0.9.

[0059] In the ball milling of step 2, the grinding aid accounts for 2.5% of the material mass percentage.

[0060] The preparation method of the grinding aid in the ball milling of step 2 is:

[0061] 3 g of dilithium mercaptosuccinate, 20 g of monoethanolamine thioglycolate, and 30 g of ethylene glycol diglycidyl ether were added to a stirring vessel, and mechanical stirring was continued with N2 protection. After heating to 95° C., 4 g of 1,8-bisdimethylaminonaphthalene was added and the reaction was carried out for 80 minutes to obtain a grinding aid.

[0062] The sintering temperature in step three is 750°C.

[0063] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 155.0 mAh / g and a first efficiency of 96.7%.

[0064] Example 3

[0065] A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that it comprises the following steps:

[0066] Step 1: 380g of recycled retired lithium iron phosphate battery positive electrode material was crushed, 4500g of solvent was added to the fragmented material, stirred and soaked for 100 minutes, and the filter residue was repeatedly washed with deionized water and dried to obtain a coarse powder of the recycled positive electrode material;

[0067] Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 10 hours, and then dried to obtain a precursor;

[0068] Step 3: The precursor is sintered in a nitrogen atmosphere for 4 hours to obtain a lithium iron phosphate positive electrode material.

[0069] The solvent in step 1 is selected from dimethyl sulfoxide.

[0070] After the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1.12:0.97.

[0071] In the step 2, the phosphorus source is selected from iron phosphate.

[0072] In the step 2, the lithium source is selected from lithium nitrate.

[0073] In the step 2, the iron source is selected from ferric phosphate.

[0074] In the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball mill is 1:1.8:1.

[0075] In the ball milling of step 2, the grinding aid accounts for 3.8% of the material mass percentage.

[0076] The preparation method of the grinding aid in the ball milling of step 2 is:

[0077] 4 g of dilithium mercaptosuccinate, 25 g of monoethanolamine thioglycolate, and 30 g of ethylene glycol diglycidyl ether were added to a stirring vessel, and mechanical stirring was continued with N2 protection. After heating to 95° C., 5 g of 1,8-bisdimethylaminonaphthalene was added and the reaction was carried out for 100 minutes to obtain a grinding aid.

[0078] The sintering temperature in step three is 800°C.

[0079] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 156.4 mAh / g and a first efficiency of 97.1%.

[0080] Example 4

[0081] A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that it comprises the following steps:

[0082] Step 1: 450g of recycled retired lithium iron phosphate battery positive electrode material was crushed, 6000g of solvent was added to the fragmented material, stirred and soaked for 120 minutes, and the filter residue was repeatedly washed with deionized water and dried to obtain a coarse powder of the recycled positive electrode material;

[0083] Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 12 hours, and then dried to obtain a precursor;

[0084] Step 3: The precursor is sintered in a nitrogen atmosphere for 5 hours to obtain a lithium iron phosphate positive electrode material.

[0085] The solvent in step 1 is selected from tetrahydrofuran.

[0086] After the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1.12:1.

[0087] In the step 2, the phosphorus source is selected from lithium dihydrogen phosphate.

[0088] In the step 2, the lithium source is selected from lithium nitrate.

[0089] In the step 2, the iron source is selected from ferrous oxalate.

[0090] In the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball mill is 1:2:1.2.

[0091] In the ball milling of step 2, the grinding aid accounts for 5% of the material mass percentage.

[0092] The preparation method of the grinding aid in the ball milling of step 2 is:

[0093] 5 g of dilithium mercaptosuccinate, 30 g of monoethanolamine thioglycolate, and 40 g of ethylene glycol diglycidyl ether were added to a stirring vessel, and mechanical stirring was continued while N2 protection was passed. After heating to 100° C., 6 g of 1,8-bisdimethylaminonaphthalene was added and the reaction was carried out for 120 minutes to obtain a grinding aid.

[0094] The sintering temperature in step three is 900°C.

[0095] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 158.2 mAh / g and a first efficiency of 97.3%.

[0096] Comparative Example 1

[0097] In this example, no grinding aid is added in step 2, and the remaining operations are consistent with those in Example 1.

[0098] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 148.5 mAh / g and a first efficiency of 95.1%.

[0099] Comparative Example 2

[0100] In this example, dilithium mercaptosuccinate was not added during the preparation of the grinding aid, and the remaining operations were consistent with those in Example 1.

[0101] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 149.5 mAh / g and a first efficiency of 95.2%.

[0102] Comparative Example 3

[0103] In this example, monoethanolamine thioglycolate was not added during the preparation of the grinding aid, and the remaining operations were consistent with those in Example 1.

[0104] After testing and analysis, the button battery assembled with the positive electrode material in this example has a discharge capacity of 151.8 mAh / g and a first efficiency of 95.7%.

[0105] The present invention has been described above through specific implementation methods and examples, but these descriptions are only illustrative and should not be understood as limiting the scope of protection of the present invention. Without departing from the spirit and scope of protection of the present invention, those skilled in the art may make various improvements, modifications or equivalent substitutions to the technical solutions and implementation methods of the present invention, all of which should fall within the scope of protection of the present invention.

Claims

1. A method for recycling retired lithium iron phosphate battery positive electrode materials, characterized in that: The following steps are involved: Step 1: crush 100-450 parts of recycled retired lithium iron phosphate battery positive electrode materials, add 1500-6000 parts of solvent to the fragments, stir and soak for 60-120 minutes, filter and repeatedly wash the residue with deionized water and dry to obtain coarse powder of recycled positive electrode materials; Step 2: The coarse powder is subjected to ICP testing, and lithium source, iron source, phosphorus source, grinding aid, and anhydrous ethanol are added for wet ball milling for 8-12 hours, and then dried to obtain a precursor; Step 3: The precursor is sintered in a nitrogen atmosphere for 2-5 hours to obtain a lithium iron phosphate positive electrode material.

2. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The solvent in step 1 is selected from at least one of N-methylpyrrolidone, acetone, ethylene glycol, N-dimethylacetamide, dimethyl sulfoxide and tetrahydrofuran.

3. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: After the phosphorus source, lithium source and iron source are added in step 2, the molar ratio of P:Li:Fe in the material is 1:1-1.12:0.92-1.

4. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: In the step 2, the phosphorus source is selected from at least one of phosphoric acid, iron phosphate, lithium phosphate, and lithium dihydrogen phosphate.

5. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: In the step 2, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium nitrate.

6. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: In the step 2, the iron source is selected from at least one of ferrous phosphate, ferrous sulfate and ferrous oxalate.

7. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: In the step 2, the mass ratio of the material, the ball milling beads and the ethanol in the ball mill is 1:1.5-2:0.8-1.

2.

8. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: In the ball milling of step 2, the grinding aid accounts for 1-5% of the material mass percentage.

9. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The preparation method of the grinding aid in the ball milling of step 2 is: By weight, 2-5 parts of dilithium mercaptosuccinate, 15-30 parts of monoethanolamine thioglycolate, and 20-40 parts of ethylene glycol diglycidyl ether are added to a stirring kettle, and mechanical stirring is continued while N2 protection is passed. After heating to 90-100° C., 3-6 parts of 1,8-bisdimethylaminonaphthalene are added, and the reaction is carried out for 60-120 minutes to obtain a grinding aid.

10. The method for recycling retired lithium iron phosphate battery positive electrode materials according to claim 1, characterized in that: The sintering temperature in step three is 650-900°C.

Citation Information

Patent Citations

  • Method for recycling positive material from water-system waste lithium iron phosphate battery

    CN103449395A

  • Mercapto group-containing polymer

    JP1989036622A

Cited By

  • Method for repairing and regenerating waste lithium iron phosphate positive electrode material through self-assembly supramolecules

    CN121215960A

  • Method for repairing and regenerating waste lithium iron phosphate positive electrode material by self-assembly supramolecule

    CN121215960B