Semiconductor device, manufacturing method thereof and electronic equipment
By using a self-aligned low-energy ion implantation process for high-concentration doping in DRAM, the problem of high contact resistance between the source electrode and the metal layer in vertical channel transistors is solved, improving device performance and avoiding damage to the silicon semiconductor pillars.
Patent Information
- Application Number
- CN202310329995.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
In the field of dynamic random access memory (DRAM), in the manufacturing process of vertical channel transistors, the contact resistance between the source electrode and the metal layer is high, resulting in poor device performance.
A self-aligned low-energy ion implantation process is used to perform high-concentration doping in the second electrode area of the transistor to form a high-concentration doping material to ensure that ohmic contact is formed between the source and drain electrodes and the metal layer, thereby reducing contact resistance.
It achieves high-concentration doping of the source and drain electrodes of the transistor, reduces the contact resistance between the source and drain electrodes and the metal layer, improves device performance, and avoids damage to the silicon semiconductor pillars caused by high-energy injection, without the need for photolithography.
Smart Images

Figure CN118742018A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to, but are not limited to, the field of semiconductor technology, and in particular to a semiconductor device and a manufacturing method thereof, and an electronic device. Background Art
[0002] In the field of dynamic random access memory (DRAM), in the manufacturing process of vertical channel transistors, the contact between the source electrode of the transistor and the metal above it and between the drain electrode and the metal bit line is a gold-semiconductor contact (metal-semiconductor contact), which easily forms a Schottky barrier, resulting in high contact resistance. Summary of the invention
[0003] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of protection of the present disclosure.
[0004] The embodiments of the present disclosure provide a 3D stacked semiconductor device and a manufacturing method thereof, and an electronic device. The manufacturing method can achieve high-concentration doping of the source and drain of a transistor without damaging the transistor.
[0005] An embodiment of the present disclosure provides a semiconductor device, which includes: at least one transistor and a bit line arranged on a substrate; the transistor includes a silicon semiconductor column extending in a direction perpendicular to the substrate, the silicon semiconductor column includes a first electrode region, a channel region, and a second electrode region in sequence along a direction close to the substrate, the bit line is arranged between the second electrode region and the substrate and connected to the second electrode region; the second electrode region contains an impurity material doped by a self-aligned ion implantation process, and the average volume density of the impurity material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
[0006] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the second electrode region may be 5e19 atoms / cm3 to 5e20 atoms / cm3.
[0007] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process is a self-aligned low-energy ion implantation process.
[0008] In an exemplary embodiment of the present disclosure, the doping material is also doped into the first electrode region through the self-aligned low-energy ion implantation process, and the implantation energy of the self-aligned low-energy ion implantation process may be 5kev to 100kev.
[0009] In an exemplary embodiment of the present disclosure, an average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
[0010] In an exemplary embodiment of the present disclosure, doping may be performed simultaneously in the first electrode region and the second electrode region through a single self-aligned low-energy ion implantation process.
[0011] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the first electrode region may be 5e19 atoms / cm3 to 5e20 atoms / cm3.
[0012] In an exemplary embodiment of the present disclosure, the transistors may be distributed in an array along a first direction and a second direction on the substrate, wherein the first direction intersects the second direction;
[0013] The bit line may extend along the first direction, and the second electrode regions of a row of transistors distributed along the first direction may be connected to the same bit line;
[0014] The transistor may further include: a gate electrode surrounding the channel region; the semiconductor device may further include a plurality of word lines extending along the second direction, the gate electrodes of a column of transistors distributed along the second direction being connected to the same word line and serving as part of the connected word line.
[0015] The embodiment of the present disclosure also provides a method for manufacturing a semiconductor device, wherein the semiconductor device comprises at least one transistor and a bit line; the transistor comprises a silicon semiconductor column extending in a direction perpendicular to a substrate;
[0016] The method for manufacturing the semiconductor device comprises:
[0017] Forming a silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column on a silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column sequentially comprises a drain region and a channel region to be formed;
[0018] Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, and annealing and diffusion are performed to form a doped region located between two adjacent silicon semiconductor pillars and the drain region to be formed of the two adjacent silicon semiconductor pillars;
[0019] The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.
[0020] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed before forming the bit line;
[0021] The step of performing ion implantation on the silicon substrate by using a self-aligned ion implantation process and annealing the substrate may include:
[0022] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0023] In a direction perpendicular to the silicon substrate, a self-aligned ion implantation process is used to perform low-energy ion implantation only on the silicon substrate but not on the channel region of the silicon semiconductor column, so that doping material is implanted into the silicon substrate exposed by the groove;
[0024] An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.
[0025] In an exemplary embodiment of the present disclosure, the process of forming the bit line may include:
[0026] After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0027] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0028] The bit line is formed in the bit line groove.
[0029] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed after forming the bit line;
[0030] The bit line forming process may include:
[0031] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0032] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0033] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0034] The bit line is formed in the bit line groove, and the bit line is exposed by the trench.
[0035] In an exemplary embodiment of the present disclosure, the step of performing ion implantation on the silicon substrate using a self-aligned ion implantation process and annealing the diffusion may include:
[0036] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate by using a self-aligned ion implantation process, so that doping material is implanted into the bit line;
[0037] An annealing process is used to diffuse the doping material from the bit line into the drain region of the silicon semiconductor column.
[0038] In an exemplary embodiment of the present disclosure, the silicon semiconductor pillar may further include a source region, wherein the source region is located on a side of the channel region away from the silicon substrate;
[0039] The method for manufacturing the semiconductor device may further include: doping the source region and the drain region simultaneously by a self-aligned ion implantation process, and simultaneously forming the doping region of the source region and the doping region of the drain region by an annealing process. In an exemplary embodiment of the present disclosure, the implantation depth of the doping material in the silicon substrate may be 0 to 45 nm.
[0040] In an exemplary embodiment of the present disclosure, the implantation depth of the doping material in the source region may be 0 to 45 nm.
[0041] In an exemplary embodiment of the present disclosure, the process conditions of the low-energy ion implantation may include: an implantation energy of 5kev to 100kev.
[0042] In an exemplary embodiment of the present disclosure, the process conditions of the annealing may include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 s to 30 s.
[0043] An embodiment of the present disclosure further provides an electronic device, which includes the semiconductor device provided by the above embodiment of the present disclosure.
[0044] The doping concentration of the source and drain electrodes of the transistor of the semiconductor device of the embodiment of the present disclosure is relatively high, and can form ohmic contact with the metal layers above and below the source and drain electrodes. Therefore, the contact resistance between the source and drain electrodes of the transistor and the metal layer is relatively small, and the device performance is relatively good.
[0045] The manufacturing method of the semiconductor device of the embodiment of the present disclosure can achieve high-concentration doping of the first electrode region and the second electrode region of the silicon semiconductor column by low-energy ion implantation, which can avoid damage to the silicon semiconductor column caused by high-energy implantation. In addition, a directional self-aligned ion implantation process is used for ion doping, which can avoid the doping material from entering the channel region. Therefore, the performance of the manufactured semiconductor device is better and no photolithography plate is required.
[0046] Other features and advantages of the present disclosure will be described in the following description, and partly become apparent from the description, or be understood by implementing the present disclosure. The objects and advantages of the present disclosure can be realized and obtained by the structures particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The accompanying drawings are used to provide an understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the technical solution of the present disclosure and do not constitute a limitation on the technical solution of the present disclosure.
[0048] Figure 1A A schematic top view of a semiconductor device provided by an exemplary embodiment of the present disclosure;
[0049] Figure 1B It is a schematic diagram of a longitudinal cross-sectional structure of a local structure of the semiconductor device shown in FIG1 in the a-a' direction;
[0050] Figure 2 A process flow chart of a method for manufacturing a semiconductor device provided for an exemplary embodiment of the present disclosure;
[0051] Figure 3 A schematic diagram of a longitudinal cross-sectional structure in the bb' direction after forming a first trench in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0052] Figure 4 A schematic diagram of a longitudinal cross-sectional structure in the bb' direction after depositing an insulating layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0053] Figure 5A A top view of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a second trench;
[0054] Figure 5B for Figure 5A The longitudinal section structure schematic diagram of the structure in the b-b' direction is shown;
[0055] Figure 5C for Figure 5A The structure shown is a schematic diagram of a longitudinal section in the a-a' direction;
[0056] Figure 6 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after depositing a sacrificial oxide layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0057] Figure 7 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction when ion implantation is performed in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0058] Figure 8 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after forming a doping region in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0059] Fig. 9 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after forming a bit line trench in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0060] Fig.10 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after forming a bit line in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0061] Fig.11 A schematic diagram of a longitudinal cross-sectional structure in the aa' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a bit line trench;
[0062] Fig.12 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a bit line;
[0063] Fig.13 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after removing a portion of a sacrificial oxide layer;
[0064] Fig.14 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction during ion implantation in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0065] Fig.15 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a doped region;
[0066] Fig.16A A doping material distribution diagram of a channel region obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0067] Fig. 16B A distribution diagram of doping materials in the channel region in the bb' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0068] Fig. 16C A distribution diagram of doping materials in the channel region in the a-a' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0069] Fig.17AA doping material distribution diagram of a source-drain electrode obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0070] Fig. 17B A distribution diagram of the doping material of the source and drain electrodes in the bb' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0071] Fig. 17C A distribution diagram of the doping material of the source and drain electrodes in the a-a' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure;
[0072] Fig.18A A doping material distribution diagram of a silicon semiconductor pillar of a device obtained by TCAD simulation according to an exemplary embodiment of the present disclosure;
[0073] Fig.18B A distribution diagram of doping material distribution in the bb' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation according to an exemplary embodiment of the present disclosure;
[0074] Fig.18C A distribution diagram of doping material distribution in the a-a' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation according to an exemplary embodiment of the present disclosure;
[0075] Fig.19 A doping concentration curve of a doping material of a silicon semiconductor pillar of a semiconductor device obtained for an exemplary embodiment of the present disclosure;
[0076] Fig. 20 A distribution diagram of doping material distribution in the bb' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation for another exemplary embodiment of the present disclosure;
[0077] Fig.21 A distribution diagram of doping material distribution in the bb' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation according to another exemplary embodiment of the present disclosure.
[0078] Fig. 22 The doping concentration curve of the doping material of the silicon semiconductor pillar of the semiconductor device obtained in Examples 2 and 3 of the present disclosure;
[0079] Fig.23 A distribution diagram of doping material distribution of a silicon semiconductor pillar of a device in a bb' direction without backscattering obtained by TCAD simulation for another exemplary embodiment of the present disclosure;
[0080] Fig.24A distribution diagram of doping material distribution of a silicon semiconductor pillar of a device in the bb' direction obtained by TCAD simulation in the presence of backscattering for another exemplary embodiment of the present disclosure;
[0081] Fig.25 The doping concentration curves of the doping material of the silicon semiconductor column of the semiconductor device obtained in the embodiment of the present disclosure are respectively obtained without backscattering and with backscattering.
[0082] The meanings of the symbols in the accompanying drawings are:
[0083] 1-silicon substrate; 10-transistor; 20-bit line; 21-bit line groove; 30-silicon semiconductor column; 31-first electrode region; 32-channel region; 33-second electrode region; 34-doping region; 40-gate electrode; 50-word line; 61-first trench; 62-second trench; 70-insulating layer; 80-sacrificial oxide layer. DETAILED DESCRIPTION
[0084] In order to make the purpose, technical solution and advantages of the present disclosure more clear, the embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings. It should be noted that the embodiments and features in the embodiments of the present disclosure can be combined with each other arbitrarily without conflict.
[0085] The embodiments of the present disclosure are not necessarily limited to the dimensions shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically show ideal examples, and the embodiments of the present disclosure are not limited to the shapes or values shown in the drawings.
[0086] In the present disclosure, ordinal numbers such as “first” and “second” are provided to avoid confusion among constituent elements and do not indicate any order, quantity or importance.
[0087] In the present disclosure, for the sake of convenience, the words and phrases indicating the orientation or positional relationship, such as "middle", "upper", "lower", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., are used to illustrate the positional relationship of the constituent elements with reference to the drawings. This is only for the convenience of describing the present specification and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation of the present disclosure. The positional relationship of the constituent elements is appropriately changed according to the direction in which each constituent element is described. Therefore, it is not limited to the words and phrases described in the disclosure and can be appropriately replaced according to the circumstances.
[0088] In the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate, or the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.
[0089] In the present disclosure, a transistor refers to an element including at least three terminals: a gate electrode, a drain electrode, and a source electrode. A transistor has a channel region between a drain electrode (drain electrode terminal, drain region, or drain electrode) and a source electrode (source electrode terminal, source region, or source electrode), and current can flow through the drain electrode, the channel region, and the source electrode. In the present disclosure, a channel region refers to a region where current mainly flows.
[0090] In the present disclosure, the first electrode region of the silicon semiconductor column can be used as the source electrode of the transistor and the second electrode region can be used as the drain electrode of the transistor, or the first electrode region of the silicon semiconductor column can be used as the drain electrode of the transistor and the second electrode region can be used as the source electrode of the transistor. In the case of using transistors with opposite polarities or when the current direction changes during circuit operation, the functions of the "source electrode" and the "drain electrode" are sometimes interchanged. Therefore, in the present disclosure, the "source electrode" and the "drain electrode" can be interchanged.
[0091] In the present disclosure, "electrical connection" includes the case where components are connected together through an element having some kind of electrical function. There is no particular limitation on the "element having some kind of electrical function" as long as it can transmit and receive electrical signals between the connected components. Examples of "element having some kind of electrical function" include not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other elements having various functions.
[0092] In the present disclosure, “parallel” means approximately parallel or almost parallel, for example, a state where the angle formed by two straight lines is greater than -10° and less than 10°, and therefore, a state where the angle is greater than -5° and less than 5° is also included.
[0093] In the present disclosure, "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced with "conductive film" in some cases. Similarly, "insulating film" may be replaced with "insulating layer" in some cases.
[0094] In order to eliminate the Schottky barrier between the metal and the source and drain electrodes of the transistor, the source and drain electrodes of the transistor can be doped with high concentrations. When manufacturing vertical transistors, the source electrode is at the top, and high-concentration doping of the source electrode is easy to achieve. The drain electrode is at the bottom. When high-concentration doping is performed, the doping material must pass through a silicon column of a certain depth to reach the drain electrode at the bottom. Choosing arsenic as the doping material can easily cause amorphization of the single-crystal silicon column, resulting in device performance failure. Choosing phosphorus with a smaller radius as the doping material, although it causes less damage to silicon, has a long diffusion distance and is easy to diffuse into the channel area, resulting in reduced device performance. Therefore, bottom doping of vertical transistors is difficult to achieve.
[0095] Typically, high-energy ion implantation is used to implant ions into the bottom and top of a vertical silicon column, and the high-energy implantation position is the top of the silicon column. The high-energy doped ions pass through the channel region into the drain region to be formed at the bottom of the silicon column, affecting the lattice shape of the silicon column channel region and thus device performance.
[0096] The present invention adopts low-energy ion implantation, the implantation position is the groove area between the silicon pillars, and the ion implantation is carried out laterally into the drain area below the channel through annealing diffusion, which effectively reduces or avoids the damage to the channel and improves the doping effect.
[0097] An embodiment of the present disclosure provides a semiconductor device.
[0098] Figure 1A A schematic top view of a semiconductor device provided by an exemplary embodiment of the present disclosure; Figure 1B It is a schematic diagram of the longitudinal cross-sectional structure of the local structure of the semiconductor device shown in FIG. 1 on the aa′ cross section.
[0099] like Figure 1A and Figure 1B As shown, the semiconductor device includes: at least one transistor 10 and a bit line 20 arranged on a substrate 1; the transistor 10 includes a silicon semiconductor column 30 extending in a direction perpendicular to the substrate 1, the silicon semiconductor column 30 includes a first electrode region 31, a channel region 32 and a second electrode region 33 in sequence along a direction close to the substrate 1, the bit line 20 is arranged between the second electrode region 33 and the substrate 1 and connected to the second electrode region 33; the second electrode region 33 contains an impurity material doped by a self-aligned ion implantation process, and the average volume density of the impurity material in the second electrode region 33 is greater than or equal to 5e19 atoms / cubic centimeter.
[0100] The average volume density can be understood as the average value obtained by testing data at multiple locations.
[0101] The doping concentration of the source and drain electrodes of the transistor of the semiconductor device of the embodiment of the present disclosure is relatively high, and can form ohmic contact with the metal layers above and below the source and drain electrodes. Therefore, the contact resistance between the source and drain electrodes of the transistor and the metal layer is relatively small, and the device performance is relatively good.
[0102] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the second electrode region 33 may be 5e19 atoms / cm 3 to 5e20 atoms / cm 3 .
[0103] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be a self-aligned low-energy ion implantation process, and the implantation energy of the self-aligned low-energy ion implantation process may be 5 kev to 100 kev.
[0104] In an exemplary embodiment of the present disclosure, the doping material may also be doped into the first electrode region by a self-aligned ion implantation process, for example, a self-aligned low-energy ion implantation process.
[0105] In an exemplary embodiment of the present disclosure, an average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
[0106] In an exemplary embodiment of the present disclosure, doping may be performed simultaneously in the first electrode region and the second electrode region through a single self-aligned low-energy ion implantation process.
[0107] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the first electrode region may be 5e19 atoms / cm3 to 5e20 atoms / cm3.
[0108] In an exemplary embodiment of the present disclosure, Figure 1A As shown, the transistors 10 may be arranged in an array along a first direction and a second direction on the substrate 1, the first direction intersecting the second direction, and the first direction and the second direction may be parallel to the substrate 1. The first direction may be as shown in FIG. Figure 1A The a-a' direction shown in FIG. 1 , the second direction may be as follows Figure 1A In the bb' direction shown, a second trench 62 is provided between two transistors 10 adjacent to each other in the first direction, and a first trench 61 is provided between two transistors 10 adjacent to each other in the second direction.
[0109] In an exemplary embodiment of the present disclosure, Figure 1A As shown, the bit line 20 may extend along the first direction.
[0110] In an exemplary embodiment of the present disclosure, Figure 1BAs shown, the second electrode regions 33 of a row of transistors 10 distributed along the first direction may be connected to the same bit line 20 .
[0111] In an exemplary embodiment of the present disclosure, Figure 1A As shown, the transistor 10 may further include: a gate electrode 40 surrounding the channel region 32 .
[0112] Among them, the surrounding can be understood as partial surrounding or full surrounding. In some embodiments, the surrounding can be full surrounding, that is, at least the entire side wall of the channel region 32 is surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 after surrounding is a closed ring. The cross-section is intercepted along the direction perpendicular to the substrate. In some embodiments, the surrounding can be partial surrounding, that is, part of the side wall of the channel region 32 is surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 after surrounding is not closed, but presents a ring shape. For example, a ring with an opening or two independent gate electrodes 40. For example, the opposite side surfaces of the channel region 32 are surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 is a ring with two openings.
[0113] In an exemplary embodiment of the present disclosure, Figure 1A As shown, the semiconductor device may further include a plurality of word lines 50 extending along the second direction.
[0114] In an exemplary embodiment of the present disclosure, the gate electrodes 40 of a column of transistors 10 distributed along the second direction may be connected to the same word line 50 .
[0115] In an exemplary embodiment of the present disclosure, the gate electrodes 40 of a column of transistors 10 distributed along the second direction may be connected to the same word line 50 and serve as a part of the connected word line 50 .
[0116] In an exemplary embodiment of the present disclosure, the transistor may be a vertical gate-all-around (VGAA) transistor; the semiconductor device may be a memory device including a transistor, such as a dynamic random access memory (DRAM), a magnetic random access memory (MRAM), etc.
[0117] The present disclosure also provides a method for manufacturing a semiconductor device, wherein the semiconductor device includes at least one transistor 10 and a bit line; the transistor 10 includes a silicon semiconductor column extending in a direction perpendicular to the substrate. The semiconductor device provided by the above embodiment of the present disclosure can be obtained by the manufacturing method.
[0118] Figure 2A process flow chart of a method for manufacturing a semiconductor device provided for an exemplary embodiment of the present disclosure.
[0119] like Figure 2 As shown, the method for manufacturing the semiconductor device includes:
[0120] A silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column are formed on a silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column comprises a drain region and a channel region to be formed in sequence, and the conductivity of the drain region to be formed is higher than that of the channel region;
[0121] Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, and annealing and diffusion are performed to form a doped region located between two adjacent silicon semiconductor pillars and the drain region to be formed of the two adjacent silicon semiconductor pillars;
[0122] The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.
[0123] The manufacturing method of the semiconductor device of the embodiment of the present disclosure can achieve high-concentration doping of the first electrode region and the second electrode region of the silicon semiconductor column by low-energy ion implantation, which can avoid damage to the silicon semiconductor column caused by high-energy implantation. In addition, a directional self-aligned ion implantation process is used for ion doping, which can avoid the doping material from entering the channel region. Therefore, the performance of the manufactured semiconductor device is better and no photolithography plate is required.
[0124] In an exemplary embodiment of the present disclosure, the implantation energy of the low-energy ion implantation may be 5 keV to 100 keV.
[0125] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed before forming the bit line;
[0126] The step of performing ion implantation on the silicon substrate by using a self-aligned ion implantation process and annealing the substrate may include:
[0127] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0128] In a direction perpendicular to the silicon substrate, a self-aligned ion implantation process is used to perform low-energy ion implantation only on the silicon substrate but not on the channel region of the silicon semiconductor column, so that doping material is implanted into the silicon substrate exposed by the groove;
[0129] An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.
[0130] In an exemplary embodiment of the present disclosure, the process of forming the bit line may include:
[0131] After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0132] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0133] The bit line is formed in the bit line groove.
[0134] In an exemplary embodiment of the present disclosure, a method for manufacturing a semiconductor device may include:
[0135] A silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column are formed on a silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column comprises a drain region and a channel region to be formed in sequence, and the conductivity of the drain region to be formed is higher than that of the channel region;
[0136] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0137] In a direction perpendicular to the silicon substrate, a self-aligned ion implantation process is used to perform low-energy ion implantation only on the silicon substrate but not on the channel region of the silicon semiconductor column, so that doping material is implanted into the silicon substrate exposed by the groove;
[0138] Using an annealing process to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench;
[0139] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0140] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0141] forming the bit line in the bit line groove;
[0142] The average volume density of the ion-implanted doping material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
[0143] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed after forming the bit line;
[0144] The bit line forming process may include:
[0145] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0146] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0147] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0148] The bit line is formed in the bit line groove, and the bit line is exposed by the trench.
[0149] In an exemplary embodiment of the present disclosure, the step of performing ion implantation on the silicon substrate using a self-aligned ion implantation process and annealing the diffusion may include:
[0150] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate by using a self-aligned ion implantation process, so that doping material is implanted into the bit line;
[0151] An annealing process is used to diffuse the doping material from the bit line into the drain region of the silicon semiconductor column.
[0152] In an exemplary embodiment of the present disclosure, a method for manufacturing a semiconductor device may include:
[0153] A silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column are formed on a silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column comprises a drain region and a channel region to be formed in sequence, and the conductivity of the drain region to be formed is higher than that of the channel region;
[0154] Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate;
[0155] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;
[0156] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;
[0157] forming the bit line in the bit line groove, the bit line being exposed by the groove;
[0158] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate by using a self-aligned ion implantation process, so that doping material is implanted into the bit line;
[0159] Using an annealing process to diffuse the doping material from the bit line into the drain region of the silicon semiconductor column;
[0160] The average volume density of the ion-implanted doping material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
[0161] In an exemplary embodiment of the present disclosure, the silicon semiconductor pillar may further include a source region, wherein the source region is located on a side of the channel region away from the silicon substrate;
[0162] The method for manufacturing the semiconductor device may further include: doping the source region and the drain region simultaneously by a self-aligned ion implantation process, and simultaneously forming the doped region of the source region and the doped region of the drain region by an annealing process. In an exemplary embodiment of the present disclosure, the process conditions of the annealing may include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 s to 30 s.
[0163] The technical solution of this embodiment is further described below through the manufacturing process of the semiconductor device of this embodiment. Deposition can adopt known processes such as sputtering, evaporation, chemical vapor deposition, etc., coating can adopt known coating processes, and etching can adopt known methods, which are not specifically limited here.
[0164] Figure 3 A schematic diagram of a longitudinal cross-sectional structure in the bb' direction after forming a first trench in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Figure 4 A schematic diagram of a longitudinal cross-sectional structure in the bb' direction after depositing an insulating layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application;
[0165] Figure 5A A top view of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a second trench; Figure 5B for Figure 5A The longitudinal section structure schematic diagram of the structure in the b-b' direction is shown;
[0166] Figure 5C for Figure 5A The structure shown is a schematic diagram of a longitudinal section in the a-a' direction; Figure 6 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after depositing a sacrificial oxide layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Figure 7 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction when ion implantation is performed in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Figure 8 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after forming a doping region in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Fig. 9 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction after forming a bit line trench in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Fig.10 It is a schematic diagram of the longitudinal cross-sectional structure in the aa' direction of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a bit line.
[0167] like Figures 3 to 10 As shown, in an exemplary embodiment of the present disclosure, the method for manufacturing the semiconductor device may include:
[0168] S10: providing a silicon substrate 1, depositing a mask plate on the silicon substrate 1, and forming a plurality of first grooves 61 extending along a first direction and spaced apart along a second direction on the silicon substrate 1 through a patterning process and an etching process, wherein the first direction and the second direction may be perpendicular to each other; the first grooves 61 expose the silicon substrate 1, and the plurality of first grooves 61 space the upper portion of the silicon substrate 1 into a plurality of semiconductor walls extending along the first direction and spaced apart along the second direction, such as Figure 3 shown.
[0169] Exemplarily, the silicon substrate may be a single crystal silicon substrate, or a silicon-on-insulator substrate, such as a silicon-on-sapphire (SOS) substrate, a silicon-on-glass (SOG) substrate, or an epitaxial layer of silicon on a base semiconductor. The silicon substrate may be doped or undoped.
[0170] S20: depositing an insulating layer 70 covering the first trench 61 on the silicon substrate 1, and planarizing the insulating layer 70 and removing the insulating layer 70 on the top surface of the semiconductor wall by chemical mechanical polishing (CMP), such as Figure 4 shown.
[0171] Exemplarily, the insulating layer may be a silicon oxide (SiOx) layer, or a low-K dielectric layer, i.e., a dielectric layer with a dielectric constant K<3.9, such as any one or more of silicon nitride (SiNx), silicon oxynitride (SiON), and silicon carbide (SiC).
[0172] S30: etching on the silicon substrate 1 to form a plurality of second grooves 62 extending along the second direction and spaced apart along the first direction; the plurality of second grooves 62 space the upper portion of the silicon substrate 1 into a plurality of silicon semiconductor pillars 30 spaced apart and spaced apart along the first direction and the second direction and spaced apart and arranged in an array, the second grooves 62 expose the sidewalls of the silicon substrate 1 and the silicon semiconductor pillars 30; the second grooves 62 include a bottom wall and sidewalls, and from the bottom wall of the second groove 62 to the opening direction of the second groove 62, the silicon semiconductor pillars 30 sequentially include a second electrode region 33, a channel region 32 and a first electrode region 31, wherein the first electrode region 31 is a source region, and the second electrode region 33 is a drain region, such as FIG. 5A to FIG. 5C Here, Figure 5C The longitudinal section in is perpendicular to the silicon substrate and does not pass through the silicon semiconductor column.
[0173] S40: Depositing a sacrificial oxide layer 80 on the silicon substrate 1 to cover the end surface of the first electrode region 31, the bottom wall and the side wall of the second trench 62, and the side wall of the silicon semiconductor pillar 30 is also covered by the sacrificial oxide layer 80. Figure 6 shown.
[0174] There are gaps in the crystal lattice of single crystal silicon, etc. The role of the sacrificial oxide layer 80 is to prevent the energetically injected ions from damaging the crystal lattice of the single crystal silicon, etc. below during ion implantation, thereby protecting the crystal lattice.
[0175] S50: With the top surface of the first electrode region 31 and the opening of the second trench 62 as self-aligned windows, a self-aligned ion implantation process is used to simultaneously perform low-energy ion implantation (implant doping) on the end surface of the first electrode region 31 and the bottom wall of the second trench 62 in a direction perpendicular to the silicon substrate 1, so that the doping material is simultaneously implanted into the silicon substrate 1 below the first electrode region 31 and the second trench 62, as shown in FIG. Figure 7 shown. Figure 7The arrow in represents the direction of self-aligned ion implantation, i.e., the direction perpendicular to the silicon substrate 1 (the angle between the silicon semiconductor column 30 and the silicon semiconductor column 30 is 0°), so ion implantation will not be performed on the channel region of the silicon semiconductor column. The energy of the low-energy ion implantation is 5kev to 100kev; the implantation depth of the doping material in the first electrode region 31, i.e., the distance between the position of the doping material in the first electrode region 31 and the top surface of the first electrode region 31 after the ion implantation is completed, can be 0 to 45nm; the implantation depth of the doping material in the silicon substrate 1, i.e., the distance between the position of the doping material in the silicon substrate 1 and the bottom wall of the second groove 62 after the ion implantation is completed, can be 0 to 45nm. The scheme of this embodiment adopts low-energy ion implantation to achieve high-concentration doping of the first electrode region and the second electrode region of the silicon semiconductor column, which can avoid damage to the silicon semiconductor column caused by high-energy implantation, and adopts a directional self-aligned ion implantation process for ion doping, which can avoid the doping material from entering the channel region, so the performance of the manufactured semiconductor device is better, and no photolithography is required.
[0176] For example, for N-type metal-oxide-semiconductor (NMOS) transistors, the doping material may include but is not limited to any one or more of phosphorus (P) and arsenic (As); for P-type metal-oxide-semiconductor (PMOS) transistors, the doping material may include but is not limited to any one or more of boron (B) and gallium (Ga). The doping depth and doping concentration of the doping material can be adjusted according to actual needs.
[0177] S60: using an annealing process to diffuse the doping material into the first electrode region 31, and the doping material diffuses from the silicon substrate 1 into the second electrode region 33, forming a doping region 34 in the first electrode region 31 and the second electrode region 33, such as Figure 8 As shown; wherein, the average volume density of the ion-implanted doping material in the first electrode region 31 is greater than or equal to 5e19 atoms / cubic centimeter, and the average volume density of the ion-implanted doping material in the second electrode region 33 is greater than or equal to 5e19 atoms / cubic centimeter; the doping material is basically uniformly distributed in the first electrode region 31, and the doping material is basically uniformly distributed in the second electrode region 33.
[0178] For example, the annealing process may be thermal annealing or spike annealing, and the ions may be activated and the ion diffusion region may be expanded by annealing. The annealing temperature may be 850° C. to 1100° C., and the annealing time may be 5 s to 30 s.
[0179] S70: etching and removing the sacrificial oxide layer 80 on the bottom wall of the second trench 62, so that the second trench 62 exposes the silicon substrate 1; etching the exposed silicon substrate 1, so that the second trench 62 extends into the silicon substrate 1 and extends toward the bottom of the second electrode region 33, and forming a bit line groove 21 extending along the first direction below the second electrode region 33 of a row of silicon semiconductor pillars 30 distributed along the first direction, such as Fig. 9 As shown;
[0180] S80: depositing a conductive layer in the bit line groove 21 to form the bit line 20, such as Fig.10 shown.
[0181] Exemplarily, the deposition of the conductive layer may include: depositing a first metal layer on the inner wall of the bit line groove 21, then performing rapid thermal annealing (RTA) to react the silicon in the silicon substrate with the first metal in the first metal layer to form a silicide of the first metal, and then using a second metal layer to fill the bit line groove 21. The first metal may include but is not limited to at least one of cobalt (Co) and titanium (Ti), and the second metal may be tungsten (W) or the like.
[0182] Exemplarily, the depth of the first trench 61 is greater than the depth of the second trench 62 , and two adjacent bit lines 20 may be insulated by an insulating layer deposited at the bottom of the first trench 61 .
[0183] Fig.11 A schematic diagram of a longitudinal cross-sectional structure in the aa' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a bit line trench; Fig.12 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after forming a bit line; Fig.13 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application after removing a portion of a sacrificial oxide layer; Fig.14 A schematic diagram of a longitudinal cross-sectional structure in the a-a' direction during ion implantation in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application; Fig.15 It is a schematic diagram of the longitudinal cross-sectional structure in the aa' direction after forming a doping region in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present application.
[0184] like Figures 3 to 6 and Figures 11 to 15 As shown, in another exemplary embodiment of the present disclosure, the method for manufacturing the semiconductor device may include:
[0185] Steps S10' to S40' are substantially the same as steps S10 to S40 of the above embodiment, except that in step S20', the insulating layer 70 on the top surface of the semiconductor wall is not removed during CMP, and the insulating layer 70 with a thickness of about 5 nm to 10 nm is retained.
[0186] S50′: etching and removing the sacrificial oxide layer 80 on the bottom wall of the second trench 62, so that the second trench 62 exposes the silicon substrate 1; using the sacrificial oxide layer 80 on the side wall of the second trench 62 as a barrier layer, etching the exposed silicon substrate 1, so that the second trench 62 extends into the silicon substrate 1 and extends toward the bottom of the second electrode region 33, and forming a bit line groove 21 extending along the first direction below the second electrode region 33 of a row of silicon semiconductor pillars 30 distributed along the first direction, as shown in FIG. Fig.11 shown.
[0187] S60': depositing a conductive layer in the bit line groove 21 to form the bit line 20, and the bit line 20 is exposed by the second trench 62, such as Fig.12 shown.
[0188] S70': etching and removing the sacrificial oxide layer 80 on the sidewall of the second trench 62, and the sacrificial oxide layer 80 on the end surface of the first electrode region 31 of the silicon semiconductor pillar 30 can be removed together, and then using the insulating layer 70 of a suitable material as the sacrificial oxide layer, such as Fig.13 As shown, alternatively, the sacrificial oxide layer 80 on the end surface of the first electrode region 31 of the silicon semiconductor pillar 30 is retained with a certain thickness.
[0189] S80′: With the top surface of the first electrode region 31 and the opening of the second trench 62 as self-aligned windows, ion implantation is performed simultaneously on the end surface of the first electrode region 31 and the bit line 20 exposed by the second trench 62 in a direction perpendicular to the silicon substrate 1 by a single self-aligned low-energy ion implantation process, so that the doping material is implanted into the first electrode region 31 and the bit line 20 at the same time, as shown in FIG. Fig.14 shown. Fig.14 The arrow in the figure indicates the direction of the self-aligned ion implantation, i.e., the direction perpendicular to the silicon substrate 1 (the angle between the silicon semiconductor column 30 and the silicon semiconductor column 30 is 0°). The low-energy ion implantation energy is 5kev to 100kev; the implantation depth of the doping material in the first electrode region 31, i.e., the distance between the position of the doping material in the first electrode region 31 and the top surface of the first electrode region 31 after the ion implantation is completed, can be 0 to 45nm; the implantation depth of the doping material in the silicon substrate 1, i.e., the distance between the position of the doping material in the silicon substrate 1 and the bottom wall of the second trench 62 after the ion implantation is completed, can be 0 to 45nm.
[0190] S90′: using an annealing process to diffuse the doping material into the first electrode region 31, and the doping material diffuses from the bit line 20 into the second electrode region 33, forming a doping region 34 in the first electrode region 31 and the second electrode region 33, such as Fig.15 As shown, wherein the average volume density of the ion-implanted doping material in the first electrode region 31 and the second electrode region 33 is greater than or equal to 5e19 atoms / cm3. Arsenic (As) plasma can enter the second electrode region 33 through lateral straggling.
[0191] In an exemplary embodiment of the present disclosure, methods of forming the first trench and the second trench may be independently selected from any one or more of dry etching and wet etching.
[0192] In an exemplary embodiment of the present disclosure, the bit line trench may be formed by side-etching the lower portion of the second trench using any one or more of dry etching and wet etching.
[0193] In an exemplary embodiment of the present disclosure, the method of depositing the insulating layer may be selected from any one of atomic layer deposition (ALD) and chemical vapor deposition (CVD).
[0194] In an exemplary embodiment of the present disclosure, the method of depositing the sacrificial oxide layer may be atomic layer deposition (ALD).
[0195] In an exemplary embodiment of the present disclosure, the method for manufacturing the semiconductor device may further include: etching away the insulating layer and the sacrificial oxide layer on the side walls of the channel region of the silicon semiconductor column, sequentially depositing a gate insulating layer and a gate electrode surrounding the side walls of the channel region on the side walls of the channel region, and connecting the gate electrode to the word line.
[0196] In an exemplary embodiment of the present disclosure, the material of the gate insulating layer may be selected from any one or more of silicon oxide (e.g., SiO2), hafnium oxide (e.g., HfO2), zirconium oxide (e.g., ZrO) and aluminum oxide (e.g., Al2O3). The gate insulating layer may be a single-layer structure or a multi-layer structure, for example, it may include a two-layer structure formed by silicon oxide and hafnium oxide, wherein the silicon oxide layer is in contact with the channel region, and the hafnium oxide layer is in contact with the gate. The thickness of the gate insulating layer may be set according to actual electrical requirements, for example, it may be 2nm to 5nm.
[0197] According to TCAD (Technology Computer Aided Design) simulation, the manufacturing method of the above-mentioned semiconductor device provided in the embodiment of the present disclosure can make the average volume density of the doping material in the first electrode area 31 greater than or equal to 5e19 atoms / cubic centimeter, and the average volume density in the second electrode area 33 greater than or equal to 5e19 atoms / cubic centimeter. Therefore, the manufacturing method of the above-mentioned semiconductor device provided in the embodiment of the present disclosure is feasible.
[0198] The feasibility of the disclosed solution is illustrated below through several TCAD simulation examples.
[0199] Example 1
[0200] In the method for manufacturing a semiconductor device of the exemplary embodiment of the present disclosure, after the ion implantation of the source and drain electrodes is completed, TCAD is used for simulation; wherein,
[0201] The doping material of the channel region is As, the ion implantation energy is 60kev to 180kev, and the average volume density of the doping material in the channel region is 5e12 atoms / cm3 to 8e13 atoms / cm3; the annealing temperature is 850°C to 1100°C, and the annealing time is 5s to 30s;
[0202] The doping material of the source and drain electrodes is As, the energy of low-energy ion implantation is 15kev to 50kev, the doping concentration is 2e14 atoms / cubic centimeter to 3e15 atoms / cubic centimeter; the annealing temperature is 850°C to 1100°C, and the annealing time is 5s to 30s.
[0203] The simulation results are as follows FIG. 16A to FIG. 19 As shown. Among them, Fig.16A A doping material distribution diagram of a channel region obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig. 16B A distribution diagram of doping materials in the channel region in the bb' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig. 16C A distribution diagram of doping materials in the channel region in the a-a' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig.17A A doping material distribution diagram of a source-drain electrode obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig. 17B A distribution diagram of the doping material of the source and drain electrodes in the bb' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig. 17C A distribution diagram of the doping material of the source and drain electrodes in the a-a' direction obtained by TCAD simulation for an exemplary embodiment of the present disclosure; Fig.18AA doping material distribution diagram of a silicon semiconductor pillar of a device obtained by TCAD simulation according to an exemplary embodiment of the present disclosure; Fig.18B 18C is a distribution diagram of the doping material distribution of the silicon semiconductor column of the device in the direction of a-b' obtained by TCAD simulation according to an exemplary embodiment of the present disclosure; 18C is a distribution diagram of the doping material distribution of the silicon semiconductor column of the device in the direction of a-a' obtained by TCAD simulation according to an exemplary embodiment of the present disclosure; Fig.19 This is a doping concentration curve of the doping material of the silicon semiconductor column of the semiconductor device obtained according to an exemplary embodiment of the present disclosure, wherein the abscissa is the depth from the upper surface (source electrode end surface) of the silicon semiconductor column to the inside of the silicon semiconductor column.
[0204] Example 2
[0205] In the method for manufacturing a semiconductor device of the exemplary embodiment of the present disclosure, the doping material of the channel region is As, the energy of ion implantation is 60kev to 180kev, and the doping concentration is 5e12 atoms / cm3 to 8e13 atoms / cm3;
[0206] The doping material of the source and drain electrodes is As, the energy of the low-energy ion implantation is 15kev to 50kev, and the doping concentration is 2e14 atoms / cubic centimeter to 3e15 atoms / cubic centimeter.
[0207] The simulation results are as follows Fig. 20 shown. Fig. 20 A distribution diagram of doping material distribution in the bb' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation according to another exemplary embodiment of the present disclosure.
[0208] Example 3
[0209] In the method for manufacturing a semiconductor device of the exemplary embodiment of the present disclosure, the doping material of the channel region is As, the energy of ion implantation is 60kev to 180kev, and the doping concentration is 5e12 atoms / cm3 to 8e13 atoms / cm3;
[0210] The doping material of the source and drain electrodes is P, the energy of the low-energy ion implantation is 5kev to 20kev, and the doping concentration is 5e14 atoms / cubic centimeter to 5e15 atoms / cubic centimeter.
[0211] The simulation results are as follows Fig.21 shown. Fig.21 A distribution diagram of doping material distribution in the bb' direction of a silicon semiconductor pillar of a device obtained by TCAD simulation according to another exemplary embodiment of the present disclosure.
[0212] Fig. 22This is a doping concentration curve of the doping material of the silicon semiconductor column of the semiconductor device obtained in Examples 2 and 3 of the present disclosure, wherein the abscissa is the depth from the upper surface (source electrode end surface) of the silicon semiconductor column to the inside of the silicon semiconductor column.
[0213] Fig.23 A distribution diagram of doping material distribution of a silicon semiconductor pillar of a device in a bb' direction without backscattering obtained by TCAD simulation for another exemplary embodiment of the present disclosure; Fig.24 A distribution diagram of doping material distribution of a silicon semiconductor pillar of a device in the bb' direction in the presence of backscattering is obtained by TCAD simulation for another exemplary embodiment of the present disclosure. Fig.25 The doping concentration curves of the doping material of the silicon semiconductor column of the semiconductor device obtained in the embodiment of the present disclosure are respectively without backscattering and with backscattering, wherein the horizontal axis is the depth from the upper surface (source electrode end surface) of the silicon semiconductor column to the inside of the silicon semiconductor column. Fig.23 and Fig.24 Compare or based on Fig.25 The backscatter dose can be considered negligible).
[0214] It can be seen that the method for manufacturing a semiconductor device provided by the embodiment of the present disclosure can achieve high-concentration doping of the source and drain electrodes of the transistor, so that the doping concentration of the source and drain electrodes is much higher than the doping concentration of the channel region.
[0215] An embodiment of the present disclosure further provides an electronic device, which includes the 3D stacked semiconductor device provided by the above embodiment of the present disclosure.
[0216] In an exemplary embodiment of the present disclosure, the electronic device may be: a storage device, a smart phone, a computer, a tablet, an artificial intelligence device, a wearable device, or a mobile power supply, etc. The storage device may include a memory in a computer, etc., which is not limited here.
[0217] Although the embodiments disclosed in the present disclosure are as above, the contents described are only embodiments adopted for facilitating the understanding of the present disclosure and are not intended to limit the present disclosure. Any technician in the field to which the present disclosure belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present disclosure, but the protection scope of the present disclosure shall still be subject to the scope defined by the attached claims.
Claims
1. A semiconductor device, characterized in that: include: At least one transistor and a bit line are arranged on a substrate; the transistor includes a silicon semiconductor column extending in a direction perpendicular to the substrate, the silicon semiconductor column includes a first electrode region, a channel region and a second electrode region in sequence along a direction close to the substrate, the bit line is arranged between the second electrode region and the substrate and connected to the second electrode region; the second electrode region contains an impurity material doped by a self-aligned ion implantation process, and the average volume density of the impurity material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
2. The semiconductor device according to claim 1, wherein: The average volume density of the doping material in the second electrode region is 5e19 atoms / cubic centimeter to 5e20 atoms / cubic centimeter.
3. The semiconductor device according to claim 1, wherein: The self-aligned ion implantation process is a self-aligned low-energy ion implantation process; the doping material is also doped into the first electrode region through the self-aligned low-energy ion implantation process, and the implantation energy of the self-aligned low-energy ion implantation process is 5kev to 100kev; and / or Doping the first electrode region and the second electrode region simultaneously by a self-aligned low-energy ion implantation process; and / or, The average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.
4. The semiconductor device according to claim 3, characterized in that The average volume density of the doping material in the first electrode region is 5e19 atoms / cubic centimeter to 5e20 atoms / cubic centimeter.
5. The semiconductor device according to any one of claims 1 to 4, characterized in that The transistors are distributed in an array along a first direction and a second direction on the substrate, and the first direction intersects with the second direction; The bit line extends along the first direction, and the second electrode regions of a row of transistors distributed along the first direction are connected to the same bit line; The transistor further includes: a gate electrode surrounding the channel region; the semiconductor device further includes a plurality of word lines extending along the second direction, the gate electrodes of a column of transistors distributed along the second direction are connected to the same word line and serve as part of the connected word line.
6. A method for manufacturing a semiconductor device, characterized in that: The semiconductor device comprises at least one transistor and a bit line; the transistor comprises a silicon semiconductor column extending in a direction perpendicular to the substrate; The method for manufacturing the semiconductor device comprises: Forming a silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column on a silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column sequentially comprises a drain region and a channel region to be formed; Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, and annealing and diffusion are performed to form a doped region located between two adjacent silicon semiconductor pillars and the drain region to be formed of the two adjacent silicon semiconductor pillars; The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.
7. The method for manufacturing a semiconductor device according to claim 6, wherein: The self-aligned ion implantation process is performed before forming the bit line; The step of using a self-aligned ion implantation process to implant ions into the silicon substrate and then annealing and diffusing the ions comprises: Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate; In a direction perpendicular to the silicon substrate, a self-aligned ion implantation process is used to perform low-energy ion implantation only on the silicon substrate but not on the channel region of the silicon semiconductor column, so that doping material is implanted into the silicon substrate exposed by the groove; An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.
8. The method for manufacturing a semiconductor device according to claim 7, wherein: The bit line forming process includes: After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate; Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate; The bit line is formed in the bit line groove.
9. The method for manufacturing a semiconductor device according to claim 6, wherein: The self-aligned ion implantation process is performed after forming the bit line; The bit line forming process includes: Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate; Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate; Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate; The bit line is formed in the bit line groove, and the bit line is exposed by the trench.
10. The method for manufacturing a semiconductor device according to claim 9, wherein: The step of using a self-aligned ion implantation process to implant ions into the silicon substrate and then annealing and diffusing the ions comprises: Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate by using a self-aligned ion implantation process, so that doping material is implanted into the bit line; An annealing process is used to diffuse the doping material from the bit line into the drain region of the silicon semiconductor column.
11. The method for manufacturing a semiconductor device according to any one of claims 6 to 10, characterized in that: The silicon semiconductor column further comprises a source region, and the source region is located on a side of the channel region away from the silicon substrate; The method for manufacturing the semiconductor device further includes: doping the source region and the drain region simultaneously by a self-aligned ion implantation process, and simultaneously forming the doping region of the source region and the doping region of the drain region by an annealing process.
12. The method for manufacturing a semiconductor device according to claim 11, wherein: The implantation depth of the doping material in the silicon substrate and / or the source region is 0 to 45 nm.
13. The method for manufacturing a semiconductor device according to any one of claims 6 to 10, characterized in that: The process conditions of the low energy ion implantation include: implantation energy of 5kev to 100kev; and / or, The annealing process conditions include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 seconds to 30 seconds.
14. An electronic device, characterized in that: Comprising the semiconductor device according to any one of claims 1 to 5.