Flame-retardant magic tape
By using polyphenylene sulfide fiber and hot-melt adhesive yarn, combined with specific weaving and heat treatment methods, the problem of flame retardancy and durability of hook and loop tapes in high-temperature venues and transportation fields is solved, and efficient hooking force and resistance are achieved. burning effect.
Patent Information
- Application Number
- CN202380025247.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2023-03-06
- Publication Date
- 2024-10-01
AI Technical Summary
Existing fabric-type hook and loop tapes are prone to problems such as the hooking elements being pulled out from the base fabric after repeated hooking/peeling, the hook and loop tape losing softness, the flame retardant effect is not sustained, and the process is unstable during the manufacturing process. It is difficult to meet the high temperature requirements. High flame retardant requirements in areas such as venues and vehicles.
Polyphenylene sulfide (PPS) fiber is used as the main yarn, combined with hot-melt adhesive yarn, and through specific weaving processes and heat treatment methods, a hook and loop tape with high flame retardancy, pull-out resistance and wide width is formed to ensure hooking. The combined elements are firmly fixed to the base fabric, avoiding heaving and adhesive stability issues.
A hook-and-loop fastener tape with excellent flame retardancy, high hooking force, difficulty in pulling out the hooking elements, and no upward and downward fluctuations has been achieved. It is suitable for use in high-temperature venues, transportation and other fields, and improves production efficiency and product quality.
Smart Images

Figure CN118742235A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a flame-retardant hook and loop fastener of fabric type, which has excellent flame retardancy, is unlikely to have hooking elements pulled out from a fabric base fabric even after repeated hooking / peeling, has little vertical fluctuation, is excellent in hooking force, and can be made wider, and a method for manufacturing the same. Background Art
[0002] In the past, as a Velcro having a fabric base cloth, a combination of a so-called fabric hook fastener and a so-called fabric loop fastener has been widely used in clothing, daily necessities, industrial materials and other application fields because even if the hooking / peeling is repeated, there is little damage to the hooking elements and the reduction in the hooking force is also small. The fabric hook fastener has a plurality of hook-shaped hooking elements formed by monofilament yarn on the surface of the base cloth, and the fabric loop fastener can be hooked with the hook-shaped hooking elements and has a plurality of loop-shaped hooking elements formed by multifilament yarn on the surface of the fabric base cloth.
[0003] In addition, for the so-called hook / loop coexisting type fabric fastener in which a plurality of the above-mentioned hook-shaped hooking elements and loop-shaped hooking elements are present on the same surface of the fabric base cloth, it is possible to combine the functions of both hook fastener and loop fastener in one fastener. Therefore, there is no need to use the hook fastener and loop fastener in combination like the existing fasteners, and it has been widely used.
[0004] In recent years, Velcro has been widely used as a mechanism for fixing indoor walls, ceiling materials, floor materials, structural materials, and thermal insulation materials of vehicles such as cars, trains, ships, and airplanes. Moreover, in these application fields, a high degree of flame retardancy is required, and the Velcro used is also required to have a high degree of flame retardancy. In addition, in the fields of special clothing such as operating clothes and firefighting clothes in high-temperature places such as furnaces and casting factories, and filters for high-temperature gas. Filter fixing materials that require flame retardancy and heat resistance, Velcro with a high degree of flame retardancy is also required.
[0005] As flame-retardant hook and loop fasteners that meet such requirements, various hook and loop fasteners have been proposed. For example, generally speaking, a flame-retardant hook and loop fastener is imparted with flame retardancy by impregnating or coating the surface of a conventional fabric hook and loop fastener with a resin to which a flame retardant is added. However, such hook and loop fasteners have the following problems after repeated hooking / peeling: the flame retardant imparted to the surface peels off; the flame retardant disappears due to washing, etc., and the flame retardant effect cannot be sustained.
[0006] In addition, in the case of a conventional fabric-based hook and loop fastener, in order to prevent the hooking element from being pulled out from the surface of the base fabric due to repeated hooking / peeling, a polyurethane-based or polyacrylic-based adhesive liquid called a back-coating resin is applied to the back of the hook and loop fastener. However, if an adhesive is applied to the back, the hook and loop fastener loses its flexibility and becomes rigid, and the feel of the fabric or the like on which the hook and loop fastener is attached is greatly reduced and becomes more rigid, so that it becomes difficult to hook and the hooking performance is also reduced.
[0007] In addition, in the process of weaving the hook and loop fastener and the process of applying the back-coating resin liquid on the back and drying it, since the process passing speed is very different, the hook and loop fastener needs to be temporarily wound up in the middle, and the manufacture of the hook and loop fastener requires effort and time. In addition, in order to make the hook and loop fastener flame retardant, it is necessary to give a flame retardant to the back-coating adhesive, but if such a back-coating adhesive with a flame retardant is used, the stability of the adhesive liquid and the leakage of the flame retardant will also occur, and the back-coating effect will also be reduced.
[0008] As a technology to eliminate the technical problems of making Velcro flame-retardant by impregnating it with a flame retardant, coating it with a back-coating resin liquid to which a flame retardant is added, a flame-retardant Velcro of a fabric type is proposed, which uses yarn formed by flame-retardant fibers represented by polyphenylene sulfide (hereinafter referred to as PPS) fibers as yarn constituting the Velcro, and uses hot-melt adhesive yarn as a part of the weft yarn. For example, Patent Document 1 describes that PPS-type multifilament yarn is used as warp yarn, and parallel yarn of multifilament yarn formed by PPS-type multifilament yarn and hot-melt adhesive core-sheath type filament is used as weft yarn, and PPS-type multifilament yarn or monofilament yarn is further used as hook element yarn, and a Velcro fabric formed by these warp yarn, weft yarn and hook element yarn is woven, and the hook element yarn is made to protrude in a loop shape on its surface, and then the hot-melt adhesive component of the multifilament yarn formed by the hot-melt adhesive core-sheath type filament is heat-melted to melt and fix the yarn constituting the fabric base cloth, and when the hook element loop is formed by monofilament yarn, one leg of the loop is cut off to make a hook-shaped hook element, thereby obtaining a flame-retardant Velcro.
[0009] In the case of the flame-retardant hook and loop fastener obtained based on the technology described in Patent Document 1, in order to achieve a high degree of flame retardancy that can be used in fields such as automobiles and airplanes that require extremely high levels of flame retardancy, it is effective to increase the ratio of the PPS yarn constituting the hook and loop fastener and reduce the ratio of the multifilament yarn formed of the hot-melt-adhesive core-sheath type filament. However, if only the ratio of the PPS yarn is increased and the ratio of the multifilament yarn formed of the hot-melt-adhesive core-sheath type filament is reduced, the fixation of the hook element based on the hot-melt-adhesive component becomes insufficient, and as a result, if the hooking / peeling is repeated, the fixation of the hook element based on the multifilament yarn formed of the hot-melt-adhesive core-sheath type filament is gradually removed, and the hook element is pulled out from the base fabric, resulting in a problem of reduced hooking force.
[0010] As an improved technology for flame-retardant Velcro using PPS yarn and multifilament yarn formed of hot-melt adhesive core-sheath type filaments, the following technology is recorded in Patent Document 2: a multifilament yarn formed by bundling multiple fine PPS filaments is used in the PPS yarn used as a part of the weft yarn, and a yarn with high heat shrinkage is used as the multifilament yarn formed of hot-melt adhesive core-sheath type filaments used in parallel with the PPS yarn.
[0011] If this technology is used, during hot melting, the multifilament yarn formed by hot-melt adhesive core-sheath type filaments is highly heat-shrunk to tighten the root of the hooking element, and then a plurality of fine PPS filaments can be wound around the yarn for the hooking element. Therefore, the hooking element can be prevented from being pulled out of the base fabric due to repeated hooking / peeling to a certain extent, but it has not yet reached a satisfactory level.
[0012] In addition, if the technology of the patent document 2 is used, when the multifilament yarn formed by the hot-melt adhesive core-sheath type filament is heat-melted, a large heat shrinkage will occur, which will cause the hook and loop fastener base fabric to fluctuate in the vertical direction (that is, the hook and loop fastener bulges or sinks in the vertical direction in the shape of seaweed). Fluctuation occurs in the length direction (warp direction) and width direction (weft direction) of the hook and loop fastener. Since high-contractility yarn is used in the weft, the fluctuation in the width direction becomes larger, which results in a great obstacle in manufacturing the wide hook and loop fastener.
[0013] Particularly for fabric hook and loop fastener, from the aspect of excellent productivity, generally adopt the following method: first, manufacture wide hook and loop fastener, this wide hook and loop fastener respectively has hook and loop element area with hook and loop element and ear area without hook and loop element in the warp direction, and makes hook and loop element area and ear area alternate in the weft direction, and then has multiple hook and loop element areas, finally, makes multiple hook and loop fastener simultaneously by the central part of ear area parallel to the warp direction. Therefore, when the wide hook and loop fastener before slitting fluctuates in the up-down direction, it is difficult to accurately slit the middle part of ear, ear width narrows or widens, and in addition, warp yarn spreads out from ear end after slitting, and deteriorates in quality and appearance.
[0014] In addition, due to the undulation of the Velcro in the up and down directions, when the hook-shaped hooking element is made by cutting off one leg of the loop to form a hook-shaped hooking element, the cutting height of the loop deviates, resulting in a deviation in the hooking force, or both legs are cut off, cut halfway, or are not cut and remain in a loop.
[0015] In addition, when the hook and loop fastener has ears without hooking elements at both ends along the warp direction, if the hook and loop fastener has ups and downs, the ears are also easy to shake in the weft direction. When the hook and loop fastener is installed by sewing, the ears are sewn with sewing yarns, but when the ears shake in the weft direction, the sewing yarns look meandering, which becomes a big problem in appearance.
[0016] In addition, in patent document 3, as a coloring method of the flame-retardant hook and loop fastener using PPS yarn described in the above patent document 1, the following method is described: the flame-retardant hook and loop fastener using PPS yarn manufactured in the above patent document 1 is immersed in a bath containing an aqueous dispersion and a crosslinking agent in which a pigment is dispersed using a polymer dispersant having an ionic group, and then taken out from the bath, and then, while being wound on a heating roller, the drying and heat treatment at 160° C. for 10 minutes are repeated twice, thereby reacting the ionic group with the crosslinking agent, and firmly attaching the pigment to the surface of the hook and loop fastener. However, in this method, in order to prevent the hooking element of the hook and loop fastener wound on the heating roller from falling down during the heat treatment, and in order to prevent the overlapping hooking element surface of the hook and loop fastener wound into a roll from being closely attached to the back surface and undergoing a crosslinking reaction so that the two sides are firmly bonded together, the hook and loop fastener has to be in a soft winding state, and only further winding and heating in this state can basically not improve the undulation problem of the hook and loop fastener. As a result, even using the method of this patent document cannot improve the above-mentioned problems of the Velcro.
[0017] Prior art literature
[0018] Patent Literature
[0019] Patent Document 1: International Publication No. 2008 / 059958
[0020] Patent Document 2: Japanese Patent Application Publication No. 2019-154880
[0021] Patent Document 3: Japanese Patent Application Publication No. 2015-62599 Summary of the invention
[0022] Problems to be solved by the invention
[0023] The present invention can obtain a hook and loop fastener formed of a flame-retardant PPS-based fabric that eliminates the above-mentioned problems. Specifically, the hook and loop fastener has excellent flame retardancy, and even if the hook and loop fastener is repeatedly hooked / peeled off, it is not easy to be pulled out of the base fabric, and the hook and loop fastener basically does not fluctuate in the up-down direction, and can be widened. In addition, it is also possible to weave a wide hook and loop fastener with a hook and loop element region divided in the weft direction by weaving the ear region, and it is also possible to simultaneously obtain a plurality of hook and loop fasteners by cutting the ear region, and a fabric-based flame-retardant hook and loop fastener with no deviation in the single-leg cutting height of the hook-shaped hook and loop element can be obtained. In addition, a flame-retardant fabric-based hook and loop fastener with ears that do not shake in the weft direction can be obtained.
[0024] Solutions to the problem
[0025] That is, the present invention is a flame retardant hook and loop fastener having a base fabric and hook elements present on the surface of the base fabric.
[0026] The base fabric is woven from warp yarns, weft yarns and yarns for hooking elements, wherein the warp yarns are composed of PPS-based multifilament yarns, the weft yarns are composed of parallel yarns of PPS-based multifilament yarns and multifilament yarns composed of hot-melt adhesive filaments, and the yarns for hooking elements are composed of at least one selected from PPS-based multifilament yarns and monofilament yarns.
[0027] The hook element is formed by the hook element yarn.
[0028] The thickness of the warp yarn in the base fabric thickness direction at the part most sunk on the back side of the warp yarn that bulges / sinks above and below with the weft yarn sandwiched therebetween is 0.94 times or less of the thickness of the warp yarn in the base fabric thickness direction at the part most bulged on the front side.
[0029] Furthermore, it is preferred that the thickness of the warp yarn in the base fabric thickness direction at the part of the warp yarn that is most sunken in the back side and that is sandwiched between the weft yarns and that is raised / sunk above and below the weft yarns satisfies the range of 0.70 to 0.90 times the thickness of the warp yarn in the base fabric thickness direction at the part that is most raised on the surface side. In addition, it is preferred that in the above-mentioned flame-retardant hook and loop fastener, the weft yarn is a parallel yarn of a PPS-type multifilament yarn and a hot-melt adhesive multifilament yarn, the above-mentioned PPS-type multifilament yarn is formed by bundling 5 to 90 filaments with a thickness of 3 to 30 dtex and a total thickness of 120 to 300 dtex, and the above-mentioned hot-melt adhesive multifilament yarn is formed by bundling 15 to 40 polyester-type core-sheath type filaments with a thickness of 3 to 8 dtex and a low-melting-point hot-melt adhesive component, and a total thickness of 80 to 150 dtex.
[0030] In addition, in the above-mentioned flame retardant hook and loop fastener, it is preferred that the ear region is cut and made into a wide hook and loop fastener before a plurality of thin hook and loop fasteners are made, wherein, on the surface of the hook and loop fastener, the hook and loop element region with the hook and loop element and the ear region without the hook and loop element are respectively continuous in the warp direction, and in the weft direction, the hook and loop element region and the ear region are alternately present, and there are a plurality of hook and loop element regions. In addition, it is preferred that the hook and loop element is a hook-shaped hook and loop element, and the pull-out force of the hook-shaped hook and loop element from the base fabric is more than 5N. In addition, it is preferred that there is no back-coated resin layer on the back of the base fabric. In addition, it is preferred that it is colored by a pigment or a disperse dye.
[0031] In addition, the present invention is a method for producing a flame-retardant hook and loop fastener, the hook and loop fastener comprising a base fabric and at least one selected from a plurality of hook-shaped hook elements and a plurality of loop-shaped hook elements formed by hook element yarns present on the surface of the base fabric, the base fabric being woven from warp yarns, weft yarns, and hook element yarns, the warp yarns being composed of polyphenylene sulfide multifilament yarns, the weft yarns being composed of polyphenylene sulfide multifilament yarns and multifilament yarns composed of hot-melt adhesive and heat-shrinkable filaments, the hook element yarns being composed of at least one selected from multifilament yarns and monofilament yarns of polyphenylene sulfide,
[0032] The method sequentially performs the following steps A, B, C and D:
[0033] [Step A] A step of weaving a loop fabric by weaving a hook element yarn parallel to the warp yarn when weaving a base fabric from warp yarns and weft yarns, and making the hook element yarn regularly cross over the warp yarns, and making the hook element yarn stand up in a loop shape from the surface of the base fabric at the crossing portion;
[0034] [Step B] A step of introducing the loop fabric into a heating area, heating the loop fabric to a temperature above which the hot-melt component of the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments melts, thermally shrinking the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments, and fixing the hook element yarn to the base fabric by a molten product from the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments;
[0035] [Step C] A step of taking the loop fabric out of the heating zone of step B, and sliding the back side of the base fabric against a fixed surface or a roller surface while the hot-melt adhesive component of the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments is melted;
[0036] [Step D] A step of taking out the loop fabric from step C, cooling the loop fabric, and then, if the engaging element yarn is a monofilament yarn, cutting a single leg of the loop to form a hook-shaped engaging element.
[0037] Furthermore, in such a method for manufacturing a flame-retardant hook and loop fastener, it is preferred that in the above step C, the loop fabric is pressed against a fixed surface while sliding on the surface and advancing, and the advancing direction of the loop fabric is changed on the fixed surface. In addition, it is preferred that the loop fabric taken out from the above step B is not temporarily cooled, and the above step C is performed after the step B using the residual heat of the step B.
[0038] In addition, in such a method for manufacturing a flame-retardant hook and loop fastener, it is preferred that the dry heat shrinkage of the multifilament yarn formed by the hot-melt adhesive and heat-shrinkable filaments at 200°C is in the range of 10 to 24%. In addition, it is preferred that the tension applied to the loop fabric in the above-mentioned step C is set to 50 to 600 g / cm. In addition, it is preferred that the process from the above-mentioned step A to the end of the step D is performed continuously without winding up the fabric in the middle. In addition, it is preferred that the loop fabric is woven in the above-mentioned step A, and on the surface of the loop fabric, the hook element area with the hook element loop and the ear area without the hook element loop are respectively continuously present in the warp direction, and the hook element area and the ear area are alternately present in the weft direction, and there are multiple hook element areas, and then, after the above-mentioned step D, the center of the ear area is cut in the warp direction, and multiple hook and loop fasteners with ears at both ends are manufactured at the same time.
[0039] Effects of the Invention
[0040] In the flame-retardant fabric hook and loop fastener of the present invention, a hot-melt adhesive and heat-shrinkable multifilament yarn is used as a part of the weft yarn. When the yarn is heat-shrinked during hot-melt bonding, the effect of fastening the installation root of the hook element and preventing the hook element from being drawn out from the fabric base cloth can be obtained. On the other hand, the hook and loop fastener will fluctuate in the vertical direction, especially in the vertical direction along the width direction. As a result, it is difficult to obtain a wide hook and loop fastener without fluctuations. In the present invention, by performing step C after the above-mentioned step B, that is, after hot-melt bonding treatment, when the hot-melt adhesive component of the multifilament yarn formed by the hot-melt adhesive and heat-shrinkable filaments has been melted, an operation is performed while pressing the back side of the base cloth to a fixed surface or roller surface while sliding it on the surface, thereby eliminating this problem.
[0041] As a result, a wide flame-retardant fabric hook and loop fastener with substantially no undulation can be obtained. Therefore, if the following technology is used in the present invention: firstly, a wide hook and loop fastener is manufactured, and finally, the hook and loop fastener is slit in parallel along the warp direction, and a plurality of narrow hook and loop fasteners are manufactured at the same time, the hook and loop fastener will not undulate, and therefore, the central portion of the ear region can be accurately slit.
[0042] In particular, if a method is used as step C in which the loop fabric is pressed against a fixed surface and is slid on the surface to advance, and the advancing direction is changed on the fixed surface, the problem of undulation can be solved to a high degree.
[0043] Moreover, since the weft yarn contains heat-shrinkable yarn, the root of the hooking element can be tightened by the heat-shrunk yarn, and the hooking element is fixed to the base cloth with yarn by melting the hot-melt adhesive component. Furthermore, the yarns constituting the base cloth (including the hot-melt adhesive component) are pressed and tightly fitted together through the above-mentioned step C, so that the molten material of the hot-melt adhesive component is squeezed out from the weft yarn due to the pressing, thereby allowing the molten material to penetrate more into the adjacent yarns and improving the bonding force between the yarns. Accordingly, the hooking element is firmly fixed to the base cloth, and the surface proportion of the hot-melt adhesive component that impairs flame retardancy can be reduced. Therefore, although the hot-melt adhesive component is small, the hooking element is basically not pulled out from the base cloth even if the hooking / peeling is repeated. At the same time, with regard to flame retardancy, since the proportion of the component that impairs flame retardancy, i.e., the hot-melt adhesive yarn, is small, a Velcro with excellent flame retardancy can be obtained. In particular, as the above-mentioned step C, by utilizing a method of pressing the loop fabric to a fixed surface while sliding it on the surface and changing the direction of travel on the fixed surface, the proportion of hot-melt adhesive yarn can be further suppressed to a low level, and the effect of preventing the hooking element from being pulled out of the base fabric can be further improved.
[0044] In addition, when the hook fastener is a hook fastener, the undulation of the base fabric in the vertical direction is eliminated by the above-mentioned step C, so the hook-shaped hooking element can be reliably cut off its single leg at the same height by the loop. Therefore, it is possible to prevent the situation where both legs are not cut off, the situation where both legs are cut off, and the situation where the installation root of the single leg is cut off and the front end of the single leg are cut off are mixed, and as a result, it is possible to prevent the situation where an excellent hooking force cannot be obtained, the hooking force is biased, and the appearance is poor.
[0045] In addition, in the flame-retardant hook and loop fastener of the present invention, the base fabric does not undulate in the up and down direction, so even if ears are provided at both ends along the warp direction, the ears do not meander, and therefore, the central portion can be sewn with sewing yarn to give a better appearance.
[0046] Moreover, in the Velcro of the present invention, since there is no need to coat the back of the Velcro base fabric with a flame-retardant back-coating resin liquid as in the existing Velcro, there will be no problems such as the back-coating resin damaging the softness of the Velcro, the back-coating resin liquid being insufficiently stable, the flame retardant added to the back-coating resin liquid seeping out and causing the flame retardancy to deteriorate over time. In addition, there will be no problems such as the working environment being deteriorated due to the solvent vapor of the resin liquid when coating / drying the back-coating resin liquid, or the coating / drying requiring time and thus reducing productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is a diagram schematically showing an example of a heat treatment apparatus in [Step B] and an example of an apparatus that can be preferably used in [Step C] when producing the flame-retardant surface fastener of the present invention.
[0048] Figure 2 This is a diagram schematically showing a cross section of a surface parallel to the warp yarns of a base fabric when [Step C] is performed in a preferred example of the flame-retardant surface fastener of the present invention.
[0049] Figure 3 This is a diagram schematically showing a cross section of a surface parallel to the warp yarns of the base fabric of the flame-retardant surface fastener when [Step C] is not performed.
[0050] Explanation of symbols
[0051] 1: Base fabric (loop fabric)
[0052] 2: Loop for hooking elements
[0053] 3: Heat treatment furnace
[0054] 4: Fixed surface or roller surface
[0055] 5: Warp
[0056] 6: Weft
[0057] 7: Hook-shaped hook element
[0058] K: base fabric thickness direction
[0059] Tb: The thickness of the warp yarn in the base fabric thickness direction at the part that sinks most to the back side
[0060] Ts: The thickness of the warp yarn in the base fabric thickness direction at the most raised part on the surface side DETAILED DESCRIPTION
[0061] The present invention is described in detail below. First, the PPS type fastener of the present invention can be roughly divided into three types: a hook fastener having only hook-shaped hook elements on the surface of a base fabric, a loop fastener having only loop-shaped hook elements on the surface of a base fabric, and a hook / loop coexistence type fastener having both hook-shaped hook elements and loop-shaped hook elements on the surface of a base fabric. In the present invention, the above three types of fasteners are taken as objects.
[0062] Among them, hook fasteners are mainly formed of monofilament yarn for hook-shaped hook elements, multifilament yarn for warp yarns, and multifilament yarn for weft yarns. In addition, loop fasteners are mainly formed of multifilament yarn for loop-shaped hook elements, multifilament yarn for warp yarns, and multifilament yarn for weft yarns. In addition, hook / loop coexistence type fasteners in which hook-shaped hook elements and loop-shaped hook elements coexist on the same surface are mainly formed of monofilament yarn for hook-shaped hook elements, multifilament yarn for loop-shaped hook elements, multifilament yarn for warp yarns, and multifilament yarn for weft yarns.
[0063] Furthermore, in these hook and loop fasteners, if the amount is small, yarns other than the above may be woven in as needed, or yarns other than the above may not be woven in.
[0064] In the present invention, the warp yarn and the yarn for the hook element must be yarns made of PPS resins in order to impart excellent flame retardancy, have excellent fiber properties and weavability, and be able to be bonded to the hot-melt adhesive component by hot-melt bonding. Therefore, PPS multifilament yarns are used for the warp yarns, PPS multifilament yarns are used for the loop-shaped hook element yarns, and PPS monofilament yarns are used for the hook-shaped hook element yarns. In addition, in the present invention, in order to further improve flame retardancy, PPS multifilament yarns are used as the main yarns constituting the weft yarns.
[0065] PPS resin is a resin that is flame retardant and heat resistant, and has excellent fiber forming properties and fiber physical properties. The PPS-based multifilament yarn and PPS-based monofilament yarn used in the present invention can be obtained from a PPS resin with a weight average molecular weight of 20,000 to 100,000, that is, the PPS resin is melt-spun, stretched, and then heat-treated as needed. Such PPS-based multifilament yarns and PPS-based monofilament yarns are currently on sale in various products. In addition, fiber manufacturers can manufacture / provide products with preferred thickness and number of aggregated roots according to user requirements. In addition, flame retardants, colorants, various stabilizers, and other resin components used in small amounts within a range that does not hinder flame retardancy, fiber physical properties, and weaving properties can be added to PPS-based multifilament yarns and monofilament yarns.
[0066] As the warp yarn used in the present invention, from the perspective of covering the surface of the multifilament yarn (hereinafter sometimes referred to as the hot-melt-bonded yarn) formed by the hot-melt-bonded and heat-shrinkable filaments used as part of the weft yarn, improving the bonding based on the hot-melt-bonded yarn, and then achieving a high degree of flame retardancy, it is preferably a PPS multifilament yarn made of 24 to 90 PPS-type filaments with a thickness of 2 to 10 decitex and a total thickness of 150 to 350 decitex. More preferably, it is a PPS multifilament yarn made of 30 to 80 PPS-type filaments with a thickness of 3 to 8 decitex and a total thickness of 200 to 300 decitex. Moreover, from the perspective of weavability, it is preferred to twist such a PPS multifilament yarn by 100 to 800 T / m, and more preferably by twisting by 300 to 600 T / m. It should be noted that T / m is an abbreviation for turn / meter.
[0067] Furthermore, the weft yarn is preferably a yarn composed of a PPS-based multifilament yarn as a main component and a hot-melt adhesive yarn, and is particularly preferably a yarn formed by doubling the above two. Among them, it is preferably a doubling yarn composed of a PPS-based multifilament yarn and a multifilament yarn whose sheath component is a hot-melt adhesive component with a low melting point, and the total decitex of the PPS-based multifilament yarn is greater than the total decitex of the hot-melt adhesive yarn, wherein the PPS-based multifilament yarn is formed by bundling 5 to 90 PPS-based filaments with a thickness of 3 to 30 dtex and having a total thickness of 120 to 300 dtex, and the multifilament yarn whose sheath component is a hot-melt adhesive component with a low melting point is formed by bundling 15 to 40 polyester-based core-sheath type filaments with a thickness of 3 to 8 dtex and having a total thickness of 80 to 150 dtex.
[0068] Among the above-mentioned parallel yarns, it is particularly preferred that the weft yarn is a parallel yarn of a PPS-type multifilament yarn and a multifilament yarn whose sheath component is a low-melting point hot-melt adhesive component, wherein the PPS-type multifilament yarn is a bundle of 6 to 80 filaments with a thickness of 3.5 to 24 dtex and a total thickness of 140 to 280 dtex, and the multifilament yarn whose sheath component is a low-melting point hot-melt adhesive component is a bundle of 20 to 30 polyester-type core-sheath type filaments with a thickness of 3 to 6 dtex and a total thickness of 80 to 140 dtex.
[0069] In particular, when a wide-width Velcro is manufactured and then slit to manufacture multiple narrow-width Velcros at the same time, from the perspective of preventing unraveling from the slit parts, it is preferred to use a parallel yarn of a multifilament yarn consisting of 8 to 80 filaments with a thickness of 3.5 to 20 dtex bundled with a total thickness of 150 to 280 dtex of PPS-type multifilament yarn, and a multifilament yarn consisting of 20 to 30 polyester core-sheath filaments with a thickness of 3 to 6 dtex bundled with a total thickness of 80 to 140 dtex, the sheath component of which is a hot-melt adhesive component with a low melting point, as the weft yarn.
[0070] On the other hand, when manufacturing a thin or wide hook and loop fastener directly through a weaving process without slitting, it is preferred to use a parallel yarn of a multifilament yarn of 6 to 20 filaments having a thickness of 10 to 24 dtex bundled and a total thickness of 140 to 200 dtex of PPS-based multifilament yarn and 20 to 30 polyester core-sheath filaments having a thickness of 3 to 6 dtex bundled and a total thickness of 80 to 140 dtex of a hot-melt adhesive component as the weft yarn in order to improve the appearance quality.
[0071] Moreover, from the perspective of hot-melt adhesive performance and the performance of the Velcro after hot-melt adhesive, it is preferred that the hot-melt adhesive yarn constituting a part of the weft yarn maintains the yarn form even after hot-melt adhesive. Therefore, as the hot-melt adhesive yarn, it is preferred that the multifilament yarn is formed by core-sheath type filaments in which the hot-melt adhesive component becomes the sheath component exposed on the fiber surface and the core component does not melt at the hot-melt adhesive temperature. Moreover, the sheath component as a part of the core-sheath type filament melts at a temperature below 240°C, and the molten material is bonded and fixed to the PPS-type hooking element yarn and warp yarn present nearby. As the hot-melt adhesive yarn, from the perspective of adhesion to PPS-type multifilament yarns and monofilament yarns, water absorption stability, thermal stability, yellowing resistance, etc., it is preferred that the sheath component is a polyester resin.
[0072] In particular, due to the ease of handling during hot-melt bonding, adhesion, and the difficulty in peeling off the core component and the sheath component, it is preferred to use a multifilament yarn formed by filaments having a core-sheath cross-section with a low-melting-point polyester resin as the sheath component and a high-melting-point polyester resin that does not melt at the temperature at which the sheath component is hot-melted as the core component. Specifically, the sheath component is preferably a copolymer of polyethylene terephthalate having a melting point of 220°C or less, particularly 120 to 210°C, which is obtained by copolymerizing copolymer components such as isophthalic acid, sulfoisophthalic acid, adipic acid, and propylene glycol.
[0073] The core component is preferably a polyester with a high melting point, specifically a polyester that has not been copolymerized or has a melting point 50 to 120° C. higher than that of the sheath component resin even if copolymerized, such as polyethylene terephthalate homopolymer and polyethylene naphthalate homopolymer.
[0074] The cross-sectional shape of the core-sheath cross-section filament can be a single core-sheath, or can be a multi-core core-sheath, in addition, can be a concentric core-sheath, or can be an eccentric core-sheath. In addition, it can be a bimetallic cross-section. That is, as long as the low melting point component is exposed on the fiber surface. As the weight ratio of the core component to the sheath component, it is preferably in the range of 75 / 25 to 30 / 70, and particularly preferably in the range of 80 / 20 to 55 / 45.
[0075] In particular, in the present invention, in order to improve the pull-out resistance of the hooking element, the hot melt yarn preferably has heat shrinkability, and specifically, a yarn having a dry heat shrinkage rate of 10 to 24% at 200° C. can be used. More preferably, a yarn having a dry heat shrinkage rate of 12 to 22% at 200° C. is used.
[0076] In addition, regarding the PPS yarn used for the warp yarn, the yarn for the hook element, and the weft yarn, from the perspective of the pull-out resistance of the hook element, it is also preferably a heat-shrinkable yarn. Specifically, in the case of the PPS-type multifilament yarn used for the warp yarn, the weft yarn, and the loop-shaped hook element yarn, it is preferably a yarn with a dry heat shrinkage rate of 3 to 15% at 200°C. In addition, in the case of the monofilament yarn used as the hook-shaped hook element yarn, it is preferably a yarn with a dry heat shrinkage rate of 1 to 4%.
[0077] It should be noted that the dry heat shrinkage rate at 200°C mentioned here refers to the value obtained by placing a 50 cm yarn in a free state in a 200°C gas atmosphere for 1 minute and calculating the shrinkage rate based on the yarn that shrinks after placing it for 1 minute. It is the average measured value of 10 randomly selected yarns.
[0078] Furthermore, the weight ratio of the PPS-based multifilament yarn and the hot melt adhesive yarn constituting the weft yarn is preferably in the range of 80:20 to 52:48, and more preferably in the range of 75:25 to 55:45, from the perspective of both flame retardancy and fixation of the hook element. In particular, when a wide hook and loop fastener is manufactured and then slit to simultaneously manufacture a plurality of narrow hook and loop fasteners, the weight ratio is preferably in the range of 75:25 to 60:40, and when a narrow or wide hook and loop fastener is directly manufactured through a weaving process without slitting, the weight ratio is preferably in the range of 70:30 to 55:45.
[0079] In order to enable the hot-melt resin of the sheath component to function effectively and to firmly fix the hooking element with yarn, the yarn formed by PPS-type multifilament yarn and hot-melt yarn used as weft yarn is preferably a yarn in a so-called untwisted yarn state with a twist number of 0 to 80 T / m.
[0080] It should be noted that in the present invention, a small amount of other filaments may be combined in the warp yarn, weft yarn, and hook element yarn within the range that the flame retardancy, hooking force, and performance of the hook and loop fastener when placed for a long time under high temperature and high humidity conditions are not impaired.
[0081] Furthermore, as the PPS-type monofilament yarn that can be used as a hook-shaped hooking element, from the aspect of the hooking force and from the aspect that the hook shape will not be stretched even if the hooking / peeling is repeated, it is preferably a monofilament yarn with a diameter of 150 to 250 μm formed from a PPS-type resin, more preferably a monofilament yarn with a diameter of 180 to 220 μm, and particularly preferably a monofilament yarn with a diameter of 195 to 210 μm.
[0082] In addition, as a PPS-type multifilament yarn that can be used as a loop-shaped hooking element, from the perspective of hooking force, and further, from the perspective that the hooking element is not easily cut due to repeated hooking / peeling, and further from the perspective that the surface feel of the fastener is excellent, it is preferably a PPS-type multifilament yarn in which 8 to 30 filaments with a thickness of 8 to 30 dtex are bundled and the total thickness is 200 to 500 dtex, and it is particularly preferably a PPS-type multifilament yarn in which 16 to 24 filaments with a thickness of 12 to 20 dtex are bundled and the total thickness is 250 to 450 dtex.
[0083] In general hook and loop fasteners, a multifilament yarn consisting of 8 to 15 filaments is generally used as the yarn for the loop-shaped hook element, but in the flame-retardant hook and loop fastener of the present invention, it is preferred to use a multifilament yarn having a larger number of filaments as the yarn for the loop-shaped hook element, thereby enabling the surface of the base fabric to be densely covered with the PPS-type loop-shaped hook elements, resulting in further improved flame retardancy. In addition, when the yarn for the loop-shaped hook element is made into a hook element, it is preferred to be a non-twisted multifilament yarn in order to increase the hooking force by spreading the multifilament yarn.
[0084] By sequentially performing the above-mentioned steps A to D, a flame-retardant hook and loop fastener made of a textile material can be manufactured from such warp yarns, weft yarns, and hooking element yarns. Next, a method for manufacturing a flame-retardant hook and loop fastener made of a textile material will be described in the order of the steps.
[0085] First, a fabric having a plurality of hooking element loops on the surface is woven by the following step A.
[0086] [Step A] A step of weaving a loop fabric by weaving a hook element yarn parallel to the warp yarn when weaving a base fabric from warp yarns and weft yarns, and making the hook element yarn regularly cross the warp yarns and making the hook element yarn stand up in a loop shape from the surface of the base fabric at the crossing portion.
[0087] As the fabric structure when the loop fabric is weaved through the process A, it is preferably a plain weave structure in which the monofilament yarn for the hook-shaped hooking element and the multifilament yarn for the loop-shaped hooking element are used as a part of the warp yarn, and these hooking element yarns are woven in parallel with the warp yarns, and 3 weft yarns are raised / sunk to stand up from the surface of the base fabric. In the case of a hook fastener, 1 to 3 warp yarns are crossed while the loop is formed, and the 3 weft yarns are penetrated between the warp yarns, and the 3 weft yarns are raised / sunk. Such a fabric structure is preferred from the aspect of easily and efficiently cutting off a single leg of the hook hooking element loop. In addition, in the case of a loop fastener, 1 warp yarn is crossed while the loop is formed and the warp yarns are penetrated. Such a fabric structure is preferred from the aspect of easily fixing the hooking element to the base fabric. In particular, the hook-shaped hooking element loop and the loop-shaped hooking element loop both stand up after three weft yarns are raised / sunk to form a loop, and at the same time cross one warp yarn and penetrate between the warp yarns. For such a fabric structure, the hooking element has excellent resistance to pull-out, and the hooking element is easy to stand up in the same direction, which can obtain a higher hooking force, so it is preferred.
[0088] Generally speaking, from the aspects of ease of production and ease of hooking of hook-shaped hook elements and loop-shaped hook elements, in the case of hook fasteners, a method is adopted in which the yarn for the hook-shaped hook element spans over 2 to 3 warp yarns to form a loop for forming the hook-shaped hook element at that location. In the case of loop fasteners, a method is adopted in which the loop is formed without spanning the warp yarns. In the present invention, it is preferred to adopt a method that is different from such a general spanning method and is a method of forming a loop at a location where both the hook-shaped hook element and the loop-shaped hook element span over one warp yarn.
[0089] The same is true for hook / loop type fasteners, and preferably, the hook-shaped hook element yarn and the loop-shaped hook element yarn are inserted between the warp yarns so that two adjacent warp yarns sandwiching a plurality of warp yarns become the same hook element yarn. In addition, the yarn ratio of the hook-shaped hook element monofilament yarn and the loop-shaped hook element multifilament yarn at this time is preferably in the range of 40:60 to 60:40.
[0090] The weaving density of the fabric is preferably 50 to 90 warp yarns (including hooking element yarns) / cm, particularly 55 to 80 warp yarns / cm, and preferably 10 to 30 weft yarns / cm, particularly 12 to 24 weft yarns / cm. Moreover, from the perspective of taking into account both flame retardancy and the pull-out resistance of the hooking element, the proportion of the hot-melt adhesive yarn in the whole Velcro is preferably 5 to 15 weight %, particularly 6 to 10 weight %.
[0091] In addition, from the perspective of hooking force, and then from the perspective of the degree to which the hooking element is not prone to falling over, the height of the hook-shaped hooking element of the Velcro is preferably 1.2~2.0 mm from the base fabric surface, and the height of the loop-shaped hooking element is preferably 1.9~3.0 mm from the base fabric surface.
[0092] In addition, the density of the hook-shaped hook elements in the hook fastener, the density of the loop-shaped hook elements in the loop fastener, and the total density of the hook-shaped hook elements and the loop-shaped hook elements in the hook / loop coexisting hook fastener are preferably 40 to 80 pieces / cm, respectively, based on the base fabric portion where the hook elements exist and based on the width after heat shrinkage, from the perspective of improving flame retardancy. 2 , 40~80 pieces / cm 2 , 40~80 pieces / cm 2 , particularly preferably 45 to 75 pcs / cm 2 , 45~75 pieces / cm 2 , 45~75 pieces / cm 2 The surface of the hook fastener is covered with a large number of PPS-type hook elements. In addition, in the hook / loop coexistent hook fastener, the ratio of the number of hook-shaped hook elements to the number of loop-shaped hook elements is preferably in the range of 40:60 to 60:40.
[0093] It should be noted that when forming a hook-shaped hooking element loop, in order to easily form a hook-shaped hooking element loop with uniform height, it is preferably used the following method: at the position where the hook-shaped hooking element yarn crosses the warp yarn, metal rods with a uniform longitudinal cross-section are placed side by side with the same number of roots as the hooking element yarn in parallel with the warp yarn in a manner such that the cross-section becomes the height direction, and the hooking element yarn is made to cross the upper part of the metal rods, thereby forming a loop of the same shape. After the loop is formed, the metal rod is pulled out of the loop.
[0094] It should be noted that in the above-mentioned step A, ear areas without hooking element loops on the surface can be set at both ends along the warp direction of the loop fabric. In addition, in addition to the two ends, ear areas (middle ear areas) without hooking element loops on the surface can also be set. In particular, the present invention is suitable for the manufacture of wide-width Velcro, and is therefore suitable for the following method: first, a loop fabric is woven on the surface of a wide-width loop fabric, in which a hooking element area and a middle ear area are continuously present in the warp direction, respectively, and in which the hooking element area and the middle ear area are alternately present in the weft direction, and there are multiple hooking element areas. Then, after the above-mentioned step D, the center of the middle ear area is cut along the warp direction, and a plurality of Velcro strips having ears (at least one of which is an ear generated from the middle ear area) at both ends are manufactured continuously in the warp direction.
[0095] As the width of the hooking element region with the above-mentioned ear, 10 to 50 mm is appropriate, and as the width of the ear region provided at both ends, 1.5 to 4 mm is appropriate, and in the case of the middle ear region, the width of the ear region is preferably 3 to 8 mm. Moreover, in the case of simultaneously manufacturing a plurality of hook and loop fasteners by cutting the middle ear region of the wide hook and loop fastener, the number of the narrow hook and loop fasteners obtained by cutting is preferably 2 to 10, and the width of the hook and loop fastener before cutting is preferably 50 to 300 mm.
[0096] In the case where a middle ear area is provided, a method can be used in which the central portion of the middle ear area is cut after step D to obtain a narrow width of Velcro. In the case of the flame-retardant Velcro of the present invention, there is basically no undulation in the up and down directions. Therefore, the central portion of the middle ear area can be accurately cut, and multiple Velcros of a certain width can be obtained at the same time, with the ears not winding at both ends along the warp direction but connected in a straight line.
[0097] Next, the loop fabric for hook and loop fastener thus obtained is sent to the following step B, and is subjected to a heat treatment for melting the hot-melt component which is the sheath component of the hot-melt yarn.
[0098] [Process B] A process of introducing the loop fabric obtained in process A into a heating area, heating it to a temperature above the temperature at which the hot-melt component of the hot-melt yarn melts, and thermally shrinking the hot-melt yarn, thereby fixing the rising portion of the loop formed by the hooking element yarn to the base fabric through the molten material from the hot-melt yarn.
[0099] Preferably, the loop fabric produced by step A is not taken up midway, but after step A, as Figure 1 As shown, the loop fabric is heat treated in a manner that it is continuously moved in a heat treatment furnace (3) in a long strip state. By this heat treatment, the sheath component of the hot-melt adhesive yarn constituting the weft yarn is melted and shrunk, and the monofilament yarn and multifilament yarn used for the hook element are fixed to the base fabric. Then, it is preferred that the long strip of hook and loop fastener fabric moving in the heat treatment furnace is moved in a manner that does not apply too much tension in the width direction so that it can fully shrink.
[0100] Thus, it is not necessary to apply the back-coating adhesive and dry the back-coating adhesive to the existing fabric-type hook and loop fastener, and the above-mentioned process and performance problems caused by the back-coating adhesive can be prevented. In addition, the loop shape of the hook-shaped hook element is fixed by the heat during the heat treatment, and in the subsequent process D, after the single leg of the hook-shaped hook element loop is cut off to form a hook-shaped hook element, the hook shape can also be ensured and sufficient hooking strength can be obtained. In addition, in the case of the loop-shaped hook element, the loop shape can also become a natural uniform shape by the heat during the heat treatment.
[0101] As the temperature in the heat treatment step B, the temperature at which the hot-melt adhesive component constituting the weft yarn melts or softens but the other components and yarns do not melt, and the shape of the monofilament yarn for the hook-shaped engaging element is fixed in a loop shape, that is, 230 to 260° C., more preferably in the range of 240 to 258° C. is used.
[0102] Such heat treatment is usually performed by running the hook and loop fastener fabric in a heated furnace. Specifically, the heat treatment is completed by running the hook and loop fastener fabric in a heating furnace at a speed of 0.30 to 1.30 m / min while staying there for 20 to 120 seconds.
[0103] The following step C is then performed on the loop fabric in which the heat-fusible component of the heat-fusible yarn is melted and the molten resin is impregnated into the adjacent yarns.
[0104] [Step C] The loop fabric is taken out from the heating zone of step B, and the back side of the base fabric is pressed against a fixed surface or a roller surface while the base fabric is slid on the surface while the heat-fusible component of the heat-fusible yarn is melted.
[0105] That is, in the above step B, if Figure 1 As shown, when the heat-treated Velcro fabric is taken out of the heat treatment furnace (3), the back side of the base fabric (1) is pressed against a fixed surface or roller surface (4) while the base fabric (1) is slid on the surface while the heat-melting component of the heat-melting yarn remains molten. Figure 1 It is described that immediately after being taken out from a heat treatment furnace (3), the back side of the hook and loop fastener fabric (1) is pressed against a fixed surface (4) and slid on the surface.
[0106] By this operation C, the ups and downs of the Velcro in the vertical direction can be eliminated, as a result, a wide and flat Velcro with flame retardancy that is basically free of ups and downs can be obtained. In addition, by this operation, even if the hooking peeling is repeatedly performed, the hooking element can be further prevented from being extracted from the base fabric. That is, by this operation, the yarn constituting the base fabric is crimped to each other, the hot-melt adhesive component squeezed out by crimping is soaked into adjacent yarn, and the bonding force further improves, and the hooking element is firmly fixed to the base fabric, therefore, the ratio of the hot-melt adhesive component can be reduced, as a result, although the hot-melt adhesive component is few, the hooking element can be prevented from being extracted from the base fabric, and simultaneously, about flame retardancy, the ratio of the hot-melt adhesive component that damages flame retardancy can also be reduced, so the Velcro with flame retardancy excellence can be obtained.
[0107] In the present invention, the warp yarn, the hook element yarn, and the PPS-type yarn used as a part of the weft yarn are significantly stiffer than the yarn formed of the usual synthetic fiber, and therefore, when the back side of the loop fabric formed of such yarn is simply pressed against a fixed surface or roller surface, it is difficult to exhibit the above-mentioned effect, but when the above-mentioned step C is performed by a method of sliding the loop fabric on the fixed surface or roller surface while pressing the loop fabric against the fixed surface or roller surface, the above-mentioned effect can be highly exhibited. That is, in the case of the PPS-type hook and loop fastener, even if the loop fabric is brought into contact with the surface of the roller rotating at the same surface speed as the running speed of the fabric, it will not slide on the surface, and therefore, the effect cannot be expected.
[0108] That is, all of the following conditions must be met: the back side of the loop fabric is pressed against a fixed surface or roller surface; and the hooking element loop existing on the surface opposite to the pressed surface is not crushed by this operation; in addition, the traveling loop fabric is made to slide on a fixed surface (4) or on the surface of a roller rotating at a surface speed different from the traveling speed of the loop fabric (1).
[0109] Thus, by sliding the filaments constituting the warp yarns on the fixed surface or roller surface while pressing them and making them run on the surface, the filaments constituting the warp yarns are promoted to move to a stable position, and the weft yarns are also stabilized in a natural state, and the contraction state is uniformed, resulting in the elimination of strain and the promotion of extrusion of the hot melt component from the weft yarns. Furthermore, by sliding the filaments on the fixed surface or roller surface while pressing them and making them run on the surface, the thickness of the warp yarns sandwiching the weft yarns and bulging / sinking thereon above and below in the base fabric thickness direction at the part most sunken on the back side is 0.94 times or less of the thickness of the warp yarns in the base fabric thickness direction at the part most bulging on the surface side.
[0110] In order to achieve such a state, as described later, it is preferred that after the loop fabric contacts the fixed surface or roller surface, the traveling direction of the loop fabric is changed while applying a tension of about 50 to 600 g / cm. More preferably, a tension of about 100 to 400 g / cm is applied.
[0111] Moreover, in the present invention, it is preferred to carry out the above-mentioned step C by pressing the loop fabric to a fixed surface or roller surface while sliding it on the surface and changing the direction of travel. By changing the direction of travel, pressing against the fixed surface or roller surface becomes easier and the effect of pressing and sliding is improved.
[0112] In addition, it is preferred that the loop fabric taken out from the above step B is not temporarily cooled, and after the step B, the loop fabric is still kept at a high temperature due to the heat given in the step B, that is, the above step C is performed using the residual heat of the step B. Even if the loop fabric is temporarily cooled and then reheated after passing through the step B, a certain degree of effect can be expected, but the strain of the loop fabric fixed by temporary cooling is difficult to eliminate, and it is difficult to fully obtain the effect of the present invention. Therefore, it is preferred that the step C is immediately performed on the hook and loop fastener fabric taken out from the step B near the place where the step B is performed.
[0113] Moreover, the loop fabric for the Velcro fed to this process preferably has its surface and back side completely free from contact with solid objects such as rollers and guides from the time it is placed in a heat treatment furnace (3) until its back side is pressed against a fixed surface or roller surface (4), and the fixed surface or roller surface is the first contact object.
[0114] In the present invention, the fixed surface or roller surface (4) used in step C is preferably a surface having a contact length of 20 to 100 mm and a contact time of 2 to 10 seconds with the back of the base fabric. As specific surfaces, preferred materials include fixed surfaces or roller surfaces made of metal, ceramic, or heat-resistant resin. The surface of the fixed surface or roller surface may be mirror-finished or roughened. In addition, if the back of the loop fabric can be pressed and slid, it may have a small amount of unevenness. In addition, the travel speed when sliding on the fixed surface or roller surface (4) is preferably 5 to 22 mm / second.
[0115] When the roller surface is used in step C, as described above, it is preferred that the roller surface speed and the running speed of the loop fabric that is pressed against the roller surface be different, and the loop fabric be run while sliding on the surface. The difference between the roller surface speed and the speed of the loop fabric that is run on the roller surface is preferably 10 to 100 mm / sec.
[0116] In addition, if Figure 1 As shown, a shape that changes the running direction of the back of the fabric by 30 to 180 degrees along a fixed surface is particularly easy to obtain the effect, and is therefore preferred. Figure 1 In the invention, the Velcro fabric (1) changes its running direction by 90° along a fixed surface (4).
[0117] It should be noted that in order to improve the contact effect, it is preferred to heat such a fixed surface and roller surface (4) to a temperature 80 to 180°C lower than the above-mentioned heat treatment temperature. Usually, the fixed surface and roller surface (4) can be heated by utilizing the residual heat of the base fabric (1) taken out of the heat treatment furnace. The surface pressing the back of the base fabric can be a fixed surface, or can be any of the following surfaces: a roller surface that rotates at a surface speed different from the speed of the base fabric as the contact surface with the base fabric moves, a belt-driven roller surface that actively stretches the base fabric and rotates at a surface speed different from the speed of the base fabric. In the case of the roller surface, as described above, it is necessary to create a difference between the surface speed of the roller and the travel speed of the loop fabric that moves while pressing its surface, and to cause the back of the loop fabric to slide on the roller surface. Therefore, from the perspective of simple structure and easy and reliable effect, it is preferred to use a roller surface such as Figure 1 In addition, it can be a narrow surface of a guide-like shape, preferably a fixed surface having the contact length as described above.
[0118] In the present invention, Figure 1 As shown, the base fabric (1) is advanced and passed through a heat treatment furnace (3), the weft yarn is shrunk as described above by passing through the heat treatment furnace (3), and then taken out of the heat treatment furnace (3), and then continuously advanced on a fixed surface (4), so that the base fabric (1) is in a state where tension is applied in the warp direction while being pressed against the fixed surface or roller surface (4). From the perspective of improving the effect, it is preferred that the tension applied to the base fabric immediately after the base fabric passes through the fixed surface (4) is a tension of about 50 to 600 g / cm. It is more preferred that a tension of about 100 to 400 g / cm is applied.
[0119] In the case of the fabric-based hook and loop fastener of the present invention, the warp yarns clamp the weft yarns and bulge / sink above and below them, so that the back side of the base fabric is covered by the warp yarns, and therefore the weft yarns containing the hot melt adhesive component basically do not directly contact the fixed surface or the roller surface (4). Therefore, the molten material of the hot melt adhesive component directly adheres to the surface of the fixed surface or the roller surface (4), and basically no adverse conditions are caused by this reason.
[0120] As mentioned above, from the aspect of improving the effect of the present invention, in addition from the aspect of productivity, it is preferred not to temporarily cool the hook and loop fastener fabric after the heat treatment by step B, but Figure 1As described, the operation of sliding the Velcro fabric (1) while pressing its back side against a fixed surface or roller surface (4) while the hot-melt adhesive component constituting the weft yarn is molten is carried out in a continuous manner with the heat treatment in the heat treatment furnace (3) using the residual heat from the heat treatment. However, the Velcro fabric can also be taken out of the heat treatment furnace (3), temporarily cooled, and then the back side of the base fabric is reheated so that the hot-melt adhesive component of the weft yarn on the back side of the Velcro fabric is in a molten state, and the operation of pressing it against a fixed surface or roller surface (4) is carried out in this state, but the effect obtained is low.
[0121] By pressing the back side of the base fabric (1) against a fixed surface or a roller surface (4) while the hot melt adhesive component is molten, and sliding the base fabric (1) on the fixed surface (4) [Step C], Figure 2 As shown, the thickness (Tb) of the warp yarns sandwiching the weft yarns and bulging / sinking up and down at the part most sunk on the back side in the direction of the base fabric thickness is less than 0.94 times the thickness (Ts) of the warp yarns in the direction of the base fabric thickness at the part most bulging on the surface side. In particular, as described above, by pressing against a fixed surface while sliding on the surface, moving on the surface, and changing the moving direction, it is possible to satisfy that the thickness of the warp yarns sandwiching the weft yarns and bulging / sinking up and down at the part most sunk on the back side in the direction of the base fabric thickness is less than 0.90 times the thickness of the warp yarns in the direction of the base fabric thickness at the part most bulging on the surface side, and thus it is preferred. It should be noted that in Figure 2 and Figure 3 In the figure, K represents the thickness direction of the base fabric.
[0122] Among them, when (Tb) is excessively reduced, the back side of the Velcro base fabric becomes dense and flat due to heat melting, and the advantages of the base fabric as a fabric, namely softness, feel, and air permeability / liquid permeability, are damaged, so it is not preferred. Therefore, it is preferred that (Tb) be 0.7 times or more of (Ts), especially 0.75 times or more.
[0123] Figure 2 The cross-sectional state of the fabric hook and loop fastener which achieves the effect of the present invention is schematically shown by pressing the back side of the base fabric (1) against a fixed surface or roller surface (4) while sliding the base fabric on the surface while the hot melt adhesive component is molten, i.e., the case where (Tb) is less than 0.94 times (Ts) (hereinafter, sometimes expressed as the ratio of (Tb) / (Ts) or the ratio of (Tb) to (Ts)). On the other hand, Figure 3 This is a diagram schematically showing the cross-sectional state of a fabric hook and loop fastener when the operation of pressing the back side of the base fabric (1) to a fixed surface or roller surface (4) while the hot-melt adhesive component is molten is not performed. In this case, (Tb) becomes a value substantially the same as (Ts), and the (Tb) / (Ts) ratio as described above does not satisfy a value below 0.94.
[0124] It should be noted that even if the operation of pressing the back side of the base fabric to a fixed surface or roller surface while sliding it on the surface while the hot-melt adhesive component is molten is not performed, that is, if [Process C] is not performed, the value of (Tb) may become slightly smaller than the value of (Ts) due to the natural gravity of the Velcro in the manufacturing process of the Velcro fabric, but the reduction is very small and (Tb) will not be lower than 0.96 times of (Ts).
[0125] Next, the method for measuring (Tb) and (Ts) of the warp yarns which are raised and sunken above and below the weft yarns is described.
[0126] First, a region with little influence from the hooking element is selected in the region where the hooking element exists on the surface, and a safety razor used for shaving is used as a cutting device to cut the hook and loop fastener parallel to the warp yarn in such a way as to cut the raised central portion of the warp yarn. The obtained cross section is magnified 200 times and photographed. As a result, the photograph schematically showing the obtained cut portion is as follows: Figure 2 . From the photograph, randomly select 3 locations where the warp yarns are most deeply sunken on the back side, and randomly select 3 locations where the warp yarns are most raised on the surface side, and measure the thickness of each location in the direction of the base fabric thickness. Perform the same measurement at any 10 locations of the Velcro to measure the thickness of each location in the direction of the base fabric thickness. From a total of 30 measured values of the thickness in the direction of the base fabric thickness at the location most deeply sunken on the back side and a total of 30 measured values of the thickness in the direction of the base fabric thickness at the location most raised on the surface side, remove 5 values from the highest value and 5 values from the lowest value, and calculate the average value of the remaining 20 values. The average values obtained are the warp yarn thickness (Tb) in the direction of the base fabric thickness at the location most sunk on the back side and the warp yarn thickness (Ts) in the direction of the base fabric thickness at the location most raised on the surface side.
[0127] It should be noted that, even when the hot melt adhesive component of weft yarn keeps the molten state, the Velcro fabric is pressed to a fixed surface or roller surface, nor is it that the position of the warp yarn present in the back side of Velcro fabric that is most sunk into the back side is all pressed to a fixed surface or roller surface, wherein, sometimes there is also a position that is not pressed to a fixed surface or roller surface, the thickness (Tb) of the back side of the warp yarn and the thickness (Ts) of the surface side do not change substantially, and in the present invention, such a position is also included in the position selected arbitrarily. Therefore, it can be considered that (Tb) / (Ts) limited by the present invention is a mean value obtained by also including these positions.
[0128] on the other hand, Figure 3 1 is a diagram showing a case where the hook and loop fastener fabric is not pressed to a fixed surface or roller surface as described above. Figure 3In such a case, i.e., when (Tb) and (Ts) are substantially the same value, the effect obtainable by using process C, i.e., reducing the undulation of the Velcro in the up and down directions, and thereby highly preventing the hooking element from being pulled out of the base fabric due to repeated hooking and peeling of the hooking element, cannot be obtained.
[0129] In the present invention, the ratio of (Tb) to (Ts) is mainly determined by the pressing strength when the hook and loop fastener base fabric is pressed to a fixed surface or roller surface while being slid. Therefore, the hook and loop fastener base fabric is slid on a fixed surface or roller surface under tension and is advanced. Figure 1 As shown, this value can be freely varied by changing the direction of travel along a fixed surface or roller surface.
[0130] It should be noted that, in the present invention, the hot melt adhesive composition constituting the weft yarn has kept the moment of molten state, when the back side of the Velcro base cloth is pressed to a fixed face or roller surface, it is necessary to make the surface side of the Velcro base cloth of the existence of the hooking element of Velcro not be pressed to a fixed face or roller surface with a circle. That is, when the Velcro base cloth is sandwiched between rollers and the operation of pressing the Velcro base cloth from top to bottom is performed, the hooking element circle upright on the surface of the base cloth can be overwhelmed by the pressing from top with great difficulty, and is fixed to the surface of the base cloth under this state, therefore, as the hooking ability of Velcro is reduced, and the outward appearance of Velcro is also deteriorated. In addition, when the surface side of the Velcro base cloth and the two sides of the back side are pressed to a fixed face or roller surface, (Tb) is substantially the same as (Ts), and it is impossible to satisfy that the (Tb) / (Ts) ratio limited by the present invention is below 0.94.
[0131] Next, when the engaging element loop is a hook-shaped engaging element loop, the fabric having the engaging element loop on the surface is sent to the following step D to cut the single leg of the hook-shaped engaging element loop to obtain a hook-shaped engaging element.
[0132] [Step D] The loop fabric is extracted from step C, cooled, and then, if the yarn for hooking elements is a monofilament yarn, the single legs of the loop are cut to form hook-shaped hooking elements.
[0133] As a cutting device used for this purpose, it is preferable to have a structure in which a single leg of the hook-shaped hook element loop of the hook fastener base fabric or the hook / loop combined type hook fastener base fabric running in the warp direction is cut between two fixed knives by the reciprocating motion of the movable cutting knife. The fabric after the single leg of the hook-shaped hook element loop is cut can be used as a hook fastener or a hook / loop combined type hook fastener.
[0134] Then, since the loop fabric taken out from step C has no undulations in the up and down directions, the single leg of the hook-shaped hooking element can be reliably cut off at a position with basically the same height of the loop in the following step D. Therefore, it is possible to prevent the situation where both legs are not cut off, both legs are cut off, and the situation where the legs cut off near the installation root of the single leg and the legs cut off near the front end of the single leg are mixed, etc., which can prevent the deviation of the hooking force and also prevent the appearance of the Velcro from being deteriorated.
[0135] Through the present invention, even though the proportion of hot-melt adhesive yarn that impairs flame retardancy is small, a flame-retardant fabric hook and loop fastener with excellent resistance to pull-out of the hook element from the base fabric due to repeated hooking / peeling can be obtained. In particular, when the hook element is a hook-shaped hook element, it is very difficult to achieve the pull-out resistance of the hook-shaped hook element without impairing flame retardancy. Through the present invention, the pull-out resistance of the hook-shaped hook element from the base fabric with a pulling force of more than 5N can be obtained.
[0136] In addition, the existing flame-retardant Velcro lacks softness when there is a back-coated resin layer on the back side. Also, when hot-melt adhesive and heat-shrinkable yarn is used in the weft yarn to give the hooking element resistance to pull-out, it will undulate in the vertical direction due to the hot-melt adhesive treatment, making it difficult to manufacture a wide flame-retardant Velcro with commercial value. However, through the present invention, a wide Velcro with a flat surface without undulations in the vertical direction can be obtained.
[0137] In particular, the present invention is suitable for manufacturing a hook and loop fastener having a width of 15 to 200 mm in the weft direction and no undulation in the vertical direction. In addition, the present invention can provide a flame-retardant hook and loop fastener having no hooking elements and ears of a certain width on both sides in a straight line without meandering in the warp direction. In addition, the present invention is also suitable for, for example, the following method: first, a wide Velcro with a width of 50 to 300 mm is made, and finally, it is cut along the warp direction to simultaneously manufacture multiple narrow Velcros. In this case, it is also suitable for the following method: in the above-mentioned step A, a loop fabric is woven, and on the surface of the above-mentioned loop fabric, a hooking element area with a hooking element loop and an ear area without a hooking element loop are respectively continuously present in the warp direction, and the hooking element area and the ear area are alternately present in the weft direction, and there are multiple hooking element areas. Then, after the above-mentioned step D, the center of the ear area is cut along the warp direction, thereby simultaneously manufacturing multiple Velcros with ears of uniform width on both sides, so that the Velcro can be obtained in which the ears are not winding in the warp direction but exist in a straight line. Of course, in the case of a Velcro with a width of less than 15 mm, the present invention can provide a Velcro in which the hooking element is not easily pulled out from the base fabric even if the Velcro is repeatedly hooked / peeled off, and the Velcro has basically no ups and downs. In addition, the ears at both ends are not tortuous, and the single-leg cutting height of the hook-shaped hooking element does not deviate.
[0138] In addition, in the present invention, from the aspect of being easy to obtain the effect of the present invention, from the aspect of productivity, and from the aspect of being easy to obtain hook-shaped and loop-shaped hook fasteners having hooking elements of the same shape, it is preferred that the fabric is not rolled up in the middle and the process is continuously performed from the above-mentioned step A to step D. That is, in the case of the existing fabric hook fastener, the process of applying the back-coated resin liquid to the back of the base fabric and drying the resin liquid takes time, so the fabric must be temporarily rolled up before applying the back-coated resin liquid and rolled up again at the moment of drying the resin liquid, but in the present invention, such operation is not required, and it can be considered that the productivity is very excellent.
[0139] In addition, if winding is performed in the middle of the process, the hook element loop will lie down due to winding, and the shape of the hook element loop will be crushed, and the hook element loop will be pressed from above, thereby causing the hook element to collapse into the base fabric, which will cause adverse effects even after passing through process D. However, in the present invention, it is possible to proceed from process A to process D at the same speed, and as a result, it is not necessary to wind up in the middle, so the above-mentioned adverse effects can be avoided. In addition, if winding is performed multiple times in the middle of production, losses will occur at the beginning of unwinding and the end of winding, and the yield will be reduced. However, in the present invention, there is no intermediate winding, and the yield reduction is small accordingly.
[0140] The fabric-based Velcro of the PPS system thus obtained is a white Velcro with a color slightly brownish due to the influence of the PPS yarn. The Velcro is used for the industrial application field where the human eye cannot observe or pays no attention to the tone of the Velcro, and therefore, it is not necessary to dye by dyes, pigments, etc., but in the case of being observable by the human eye, etc., it can be dyed by disperse dyes according to the user's requirement and used. Generally speaking, the fiber product of the PPS class is not easy to be dyed, and therefore, the Velcro of the present invention is also not easy to be dyed into a dark color, but by using disperse dyes as dyes and dyeing water as a medium under high temperature and high pressure, a certain degree of dark product can be obtained.
[0141] When using disperse dyes as dyes and water as a medium for dyeing under high temperature and high pressure, the hook and loop fastener of the present invention is dyed in an aqueous solution containing disperse dyes in a temperature range of 120 to 145° C. for more than 90 minutes, so that a PPS-based hook and loop fastener dyed to a certain degree of dark color can be obtained. The type of disperse dye used is not particularly limited, and the dyeing of polyester fiber products can use any disperse dye used in the past, for example, disperse dyes of nitroarylamines such as aminoazobenzenes, anthraquinones, and nitrodiphenylamine derivatives. In particular, PPS fiber products can be used for heat-resistant and flame-retardant purposes, and therefore, preferably black disperse dyes that can obtain the color tone required for products for these purposes are used.
[0142] The PPS fabric fastener obtained by the method described in detail above is suitable for applications requiring high flame retardancy and heat resistance, for example, it is suitable as interior materials, raw materials for seats, installation materials such as curtains, etc. for vehicles such as automobiles, airplanes, trains, and ships. It is particularly suitable as a locking material for fixing the cushioning bodies and surface materials of the seats of these vehicles. It is also suitable as a fixing material for carpets on the floors of the above-mentioned vehicles and an installation material for curtains. It is also suitable for special clothing fields such as operating clothes and fire suits in high-temperature places such as furnaces, casting factories, and glass product factories. It is also suitable as a fixing material in fields requiring flame retardancy and heat resistance, such as high-temperature gas filter fixing materials.
[0143] Example
[0144] Hereinafter, the present invention will be specifically described through examples and comparative examples. It should be noted that in the examples and comparative examples, the flame retardancy was measured according to the vertical flame retardancy test method [14 CFR PART25 Sec25.853 (a)]. Specifically, in a combustion tester, the exposed surface of the Velcro is installed in a U-shaped fixture in a manner of 5.08 cm × 30.48 cm in length, the sample is made vertical, and the burning state when the flame of the hand-held burner is contacted from below for 12 seconds is observed, and the time from removing the burner to self-extinguishing is measured. Five measurements were carried out and the average value was calculated.
[0145] In addition, the hooking force was measured according to JIS L 3416-2000. Then, as the hooking object at this time, when the hooking tape of the embodiment and the comparative example is a hook hooking tape, the loop hooking tape as the hooking object was measured using B48000 (made by Kuraray Loop Fastener Co., Ltd.), and in the case of the loop hooking tape, the hook hooking tape as the hooking object was measured using A48600 (made by Kuraray Loop Fastener Co., Ltd.), and in the case of the hook / loop coexisting type ...
[0146] For the pull-out force of the hook-type element, the method for measuring the pull-out force of the hook-type element is to use a tensile testing machine made by SHIMADZU Company, and the hook-type hook-type element of the hook-type element provided is bent along the width direction (weft direction) and arranged on the chuck of the tensile testing machine in a way that is easy to clamp the hook-type hook-type element, and the hook-type hook-type element is pulled out from the base fabric at a tensile speed of 100mm / min, and the maximum strength when the hook-type hook-type element is pulled out from the base fabric of the hook-type element is measured. In the case of the loop hook-type element, the loop that will become the object of measurement is sunk into the base fabric and then the loop-type hook-type element that is raised on the base fabric surface is cut off with yarn at the top of the base fabric surface, which is the value measured by the above method in this state. In addition, in the case of the hook / loop coexistence type hook-type element, the value of the pull-out force of the hook-type hook-type element is used as the pull-out force of the hook-type element. Randomly select any 10, measure their pull-out forces, and adopt their average value.
[0147] Example 1
[0148] As the warp yarn, weft yarn, and monofilament yarn for hook-shaped engaging elements constituting the base fabric of the flame-retardant hook fastener, the following yarns were prepared, respectively.
[0149] [Warp]
[0150] ·PPS multifilament yarn
[0151] Total decimal point and number of filaments: 250dtex, 60 filaments
[0152] ·Twist number 419T / m
[0153] Dry heat shrinkage at 200°C: 7.7%
[0154] [Weft yarn (untwisted parallel yarn of the following two types of multifilament yarns)]
[0155] ·Multifilament yarn made of core-sheath composite filament
[0156] Core material: Polyethylene terephthalate
[0157] · Sheath component: 25 mol% isophthalic acid copolymerized polyethylene terephthalate (softening point: 190°C)
[0158] Core sheath ratio (weight ratio): 70:30
[0159] Total decimal point and number of filaments: 99dtex, 24 filaments
[0160] Dry heat shrinkage at 200°C: 17.1%
[0161] ·PPS multifilament yarn
[0162] Total decimal point and number of filaments: 167dtex, 10 filaments
[0163] ·Dry heat shrinkage at 200°C: 9.0%
[0164] [Monofilament yarn for hook-shaped hooking elements]
[0165] ·Monofilament yarn made of PPS
[0166] Diameter (before heat shrinkage): 0.20mm
[0167] Dry heat shrinkage at 200°C: 2.8%
[0168] [Manufacture of hook and loop fasteners]
[0169] The above-mentioned warp yarn, weft yarn and monofilament yarn for hook-shaped hook-shaped hooking elements are used, and a plain weave is used as the fabric structure. The monofilament yarn for hook-shaped hooking elements is woven in parallel with the warp yarn in a ratio of 1 yarn to 4 warp yarns so that the weaving density (after heat shrinkage treatment) reaches 56 yarns / cm for the warp yarn and 16.5 yarns / cm for the weft yarn. After three weft yarns are raised / sunk, they cross over one warp yarn, and a loop is formed on the base fabric in a manner that a loop is formed at the crossed portion.
[0170] It should be noted that when forming a loop for a hook-shaped hooking element, the following method is used: at the position where the hook-shaped hooking element yarn crosses over the warp yarn, metal rods with a uniform longitudinal cross-section, the same number of which is parallel to the warp yarn and has the same number of roots as the hooking element yarn, are placed upright and side by side in a manner such that the longitudinal direction of the cross-section becomes the height direction of the hook-shaped hooking element loop, the hooking element yarn crosses over the upper part of the metal rods, and the metal rods are pulled out of the loop after the loop is formed.
[0171] The hook fastener tape woven under the above conditions was run in a heat treatment furnace for 60 seconds at 246°C, a temperature at which only the sheath component of the weft yarn is heat-melted and the warp yarn, the monofilament yarn for the hook-shaped ...
[0172] Then, while the hot melt adhesive component (sheath component) of the weft yarn remains in a molten state, Figure 1According to the invention, after the hook fastener fabric tape is passed through a fixed surface of stainless steel having a mirror-finished surface provided next to the exit of a heat treatment furnace, it is moved under a tension of 200 g / cm, its back side is pressed against the fixed surface for 5 seconds, and it is slid on the surface at a speed of 10 mm / sec for 5 seconds, and the moving direction is bent 90 degrees along the surface. Then, the obtained fabric is cooled, and the single leg portion of the hook-shaped hook element loop is cut off to form a hook-shaped hook element.
[0173] In the above results, no fluctuation in the vertical direction of the hook fastener was observed, and as a result, the single leg cutting of the hook-shaped hook element could be performed without any problem. In addition, from the above-mentioned weaving step to the heat treatment step, the step of crimping to the fixed surface, and then the single leg cutting step of the hook-shaped hook element, no winding was performed in the middle and the single leg cutting step of the hook-shaped hook element was performed continuously.
[0174] [Performance of the obtained hook fastener, etc.]
[0175] The obtained hook fastener fabric had a width of 20 mm in the region where the hook elements were present, and had ears with a width of 2.5 mm without hook elements at both ends that were parallel to the warp direction without zigzagging. The flame retardancy of the hook fastener was measured and found to be 3.4 seconds, which was very excellent and a level that was sufficiently qualified for aircraft use.
[0176] In this hook fastener, the density of hook-shaped hook elements is 56 pieces / cm 2 , the height of the hook-shaped hook-engaging element from the base fabric surface is 1.8mm. The cut state of the hook-shaped hook-engaging element of the Velcro was observed, and the result was that any hook-shaped hook-engaging element was cut off at a position 70% of the height from the installation root of one leg. In addition, the warp yarn thickness (Tb) of the hook Velcro in the base fabric thickness direction of the position most sunk into the back side and the warp yarn thickness (Ts) of the base fabric thickness direction of the most raised position on the surface side were measured, and the result was that (Tb) was 0.125mm and (Ts) was 0.107mm, so (Tb) / (Ts) was 0.86.
[0177] The pull-out force of the hook-shaped hooking element of the hook fastener from the base fabric was measured and the result was 6.3 N, indicating that the pull-out resistance was also very excellent. In addition, the hook fastener was observed to have no up-and-down fluctuations by placing it on a flat glass plate without applying a load, and the result was that no fluctuations were observed at all.
[0178] In addition, the hooking force of the hook fastener was measured. The results showed that the initial hooking force was 12.4 N / cm in shear strength. 2, the peel strength is 1.39N / cm, and the hooking force after 1000 hooking / peeling is 11.2N / cm in shear strength 2 The peel strength is 1.26 N / cm. Even after 1000 times of hooking / peeling, no hook-shaped hooking elements were pulled out from the surface of the hook fastener, and no hook-shaped hooking elements were observed that were broken by stretching in the hook state and lost their hooking ability. Although there is no back coating, it is very excellent as a hook fastener.
[0179] In addition, the hook fastener is soft, so although the ears are sewn by a sewing machine to be attached to the cuffs of clothing, the appearance of the clothing will not be deteriorated. In this case, the sewing yarn can be sewn in a manner that the ears do not meander and the central part of the ears is present in a straight line, which is also excellent in appearance.
[0180] Comparative Example 1
[0181] [Manufacture of hook and loop fasteners]
[0182] The following method is used: in the above-mentioned Example 1, the stainless steel fixed surface set next to the outlet of the heat treatment furnace is removed, and the back side of the fastener is not pressed against the fixed surface while the hot-melt adhesive multifilament yarn after heat treatment remains in a molten state. Instead, the fastener is taken out from the heat treatment furnace and cooled and then pulled with a roller. Except for this, the same method as the above-mentioned Example 1 is carried out to produce a hook fastener.
[0183] [Performance of the obtained hook fastener, etc.]
[0184] The hook fastener tape had a hook element area with a width of 20 mm, and ears with an average width of 2.5 mm without hook elements were present at both ends parallel to the warp direction. The hook fastener tape had a hook element density of 56 pieces / cm 2 The height of the hook-shaped hook element from the base fabric surface was 1.8 mm, and the flame retardancy was 3.6 seconds, which was as good as the hook fastener of Example 1. Then, the cut state of the hook-shaped hook element was observed, and the result was that the situation of being cut at a position close to the installation root of the hook-shaped hook element and the situation of being cut at a position close to the top existed continuously. In addition, among the hook-shaped hook elements, a circular hook-shaped hook element without cutting the root of one leg, a hook-shaped hook element with both legs cut and not forming a hook shape, and a hook-shaped hook element only cut to the middle of one leg were scattered. Then, the fastener was placed on a horizontal glass plate, and large and small ups and downs were observed, and the part protruding from the glass plate was repeatedly observed.
[0185] The pull-out force of the hook-shaped hooking element of the hook fastener was measured and the result was 4.2 N, which was significantly worse than that of Example 1. In addition, the hooking force of the hook fastener was measured and the result was that the initial hooking force was 11.6 N / cm in terms of shear strength. 2 , the peel strength is 1.28N / cm, and the hooking force after 1000 hooking / peeling is 9.7N / cm in shear strength 2 The peel strength was 1.02 N / cm. After 1000 repetitions of hooking / peeling, hook-shaped hooking elements were scattered and seen being pulled out from the surface of the hook fastener.
[0186] The (Tb) / (Ts) of the hook fastener was 0.96. In addition, the hook fastener was attached to the cuff of the garment by sewing the sewing yarn using the ear portion as in Example 1. However, due to the winding of the ear portion, it was difficult to sew the central portion thereof with the sewing yarn. The sewing yarn of the hook fastener of the cuff that was sewn was winding in many places, which was inferior to Example 1 in terms of appearance.
[0187] Example 2
[0188] [Manufacturing of Velcro]
[0189] In the method for manufacturing the hook fastener of Example 1, the hook element yarn was changed to the following loop hook element multifilament yarn, and plain weave was used as the fabric structure, and the weaving density (after heat shrinkage treatment) was 54 warp yarns / cm and 18.8 weft yarns / cm. Then, the loop hook element multifilament yarn was woven in parallel with the warp yarns at a ratio of 1 yarn to 4 warp yarns, and after 3 weft yarns were raised / sunk, one warp yarn was crossed and a loop was formed at the crossed position, so that a loop was formed on the base fabric. The loop fastener was produced by the same method as in Example 1. Since the hook element was a loop hook element, the cutting of the single leg of the loop in step D performed in Example 1 was not performed. In addition, from the above-mentioned weaving step to the heat treatment step and the step of crimping to the fixing surface, winding was not performed in the middle and the process was performed continuously.
[0190] [Yarn for loop hook elements]
[0191] ·Multifilament yarn formed from PPS
[0192] Total decimal point and number of filaments: 334dtex, 20 filaments
[0193] Dry heat shrinkage at 200°C: 9.1%
[0194] [Performance of the obtained loop fastener, etc.]
[0195] The width of the loop hook and loop fastener fabric obtained was 20 mm in width in the region where the hook element existed, and the ears without the loop hook element existed at both ends with a width of 2.5 mm in parallel with the warp direction with a uniform width. The flame retardancy of the loop hook and loop fastener was measured and the result was 3.0 seconds, which was very excellent. It was found that it was at a level that could be qualified for aircraft use as in Example 1, and it was found that it could be used in combination with Example 1.
[0196] The density of the loop hook elements of the loop fastener is 63 pieces / cm 2 , and the height of the loop-shaped hooking element from the base fabric surface is 2.1 mm. In addition, the (Tb) / (Ts) of the loop hook and loop fastener is 0.88.
[0197] Next, the pull-out force of the loop-shaped hook element was measured and the result was 10.3 N, indicating that the pull-out resistance was also very excellent. In addition, the hook and loop fastener was placed on a flat glass plate and the presence or absence of undulation in the vertical direction of the loop fastener was observed, and the result was that no undulation was observed.
[0198] In addition, the hooking force of the loop of hook and loop fastener was measured. The results showed that the initial hooking force was 12.2 N / cm in shear strength. 2 , the peel strength is 1.38N / cm, and the hooking force after 1000 hooking / peeling is 11.1N / cm in shear strength 2 The peel strength is 1.24 N / cm. Even after repeated hooking / peeling 1000 times, no loop-shaped hooking elements were observed to be pulled out from the surface of the loop fastener. Although there is no back coating, the loop fastener has very excellent hooking force.
[0199] Moreover, the hook fastener is very soft, so when the ears are attached to the cuffs of clothes by sewing with sewing yarn, the sewing yarn does not cause the ears to meander, and the central part of the ears exists in a straight line, which is also excellent in appearance.
[0200] Comparative Example 2
[0201] [Manufacturing of Velcro]
[0202] In the above-mentioned Example 2, the stainless steel fixed surface arranged next to the outlet of the heat treatment furnace is removed, and the back side of the Velcro is not pressed to the fixed surface while the hot-melt adhesive multifilament yarn after heat treatment remains in a molten state. Instead, it is pulled with a roller after cooling. Except for this, the loop Velcro is produced in the same manner as in the above-mentioned Example 2.
[0203] [Performance of the obtained loop fastener, etc.]
[0204] The width of the area with hook elements in the obtained loop fastener was 20 mm, and ears without hook elements with an average width of 2.5 mm were present at both ends parallel to the warp direction. The density of the loop hook elements in the loop fastener was 63 pieces / cm 2 The height of the looped hook element from the base fabric surface was 2.1 mm, and the flame retardancy was 3.1 seconds. Then, the hook fastener was placed on a horizontal glass plate, and the result was that large and small ups and downs were observed in the same manner as the hook fastener of Comparative Example 1.
[0205] In addition, the pull-out force of the loop-shaped hook element from the base fabric surface was measured, and the result was 8.7 N, which was a worse result than Example 2. In addition, the hooking force of the loop hook and loop fastener was measured, and the result was that the initial hooking force was 11.4 N / cm in shear strength. 2 , the peel strength is 1.26N / cm, and the hooking force after 1000 hooking / peeling is 9.6N / cm in shear strength 2 The peel strength was 1.01 N / cm, which was worse than that of Example 2 in terms of hooking force. In addition, after 1000 repetitions of hooking / peeling, unlike Example 2, loop-shaped hooking elements were observed to be pulled out from the surface of the loop fastener in many places.
[0206] The (Tb) / (Ts) of the loop fastener is 0.97. As in the case of Example 2, the loop fastener is attached to the cuff of clothing by sewing using the ear portion and sewing yarn, but it is difficult to sew the central portion of the ear portion with the sewing yarn, and as a result, it can be observed that the sewing yarn is slightly meandering, which is also inferior to Example 2 in terms of appearance.
[0207] Example 3
[0208] [Manufacturing of Hook / Loop Type Velcro]
[0209] Using the warp yarns, weft yarns, monofilament yarns for hook-shaped engaging elements, and multifilament yarns for loop-shaped engaging elements used in Examples 1 and 2, a hook / loop combined type surface fastener was produced.
[0210] Specifically, a plain weave was used as the fabric structure at this time, and the weaving density (after heat shrinkage treatment) was 54 warp yarns / cm and 16.5 weft yarns / cm, and a loop was formed on the base fabric by making the loop-shaped engaging element multifilament yarn or the hook-shaped engaging element monofilament yarn rise / sink after three weft yarns were raised / sunk, and then crossing over one warp yarn, so that a loop was formed at the crossing position. At this time, the loop-shaped engaging element multifilament yarn and the hook-shaped engaging element monofilament yarn were woven in such a manner that two yarns each were continuously and alternately present.
[0211] The hook / loop type hook and loop fastener was manufactured by weaving in the same manner as in Example 1, and heat treatment, pressing to the fixed surface, and cutting of the single leg of the hook-shaped hook element loop were performed in the same manner as in Example 1. Then, the above-mentioned weaving step to the heat treatment step, the step of crimping to the fixed surface, and the step of cutting of the single leg of the hook-shaped hook element were performed continuously without winding up in the middle.
[0212] [Performance of the obtained hook / loop type fastener, etc.]
[0213] The width of the obtained hook / loop type hook fastener fabric was 20 mm in width in the region where the hook elements were present, and 2.5 mm wide ears without hook elements were present at both ends in parallel with the warp direction with a uniform width. The density of hook-shaped hook elements was 28 pieces / cm 2 , the density of the loop hook elements is 28 pieces / cm 2 In addition, the height of the hook-shaped hook element from the base fabric surface is 1.8 mm, and the height of the loop-shaped hook element from the base fabric surface is 2.1 mm. The flame retardancy of the hook / loop coexisting type fastener is 3.2 seconds, which is the same level as that of Examples 1 and 2 that can be used in aircraft applications.
[0214] The cut state of the hook-shaped hooking element of the hook / loop type fastener was observed, and the result was that any hook-shaped hooking element was cut at a position 70% of the height from the installation root of one leg. The (Tb) / (Ts) of the hook / loop type fastener was 0.87.
[0215] Next, the pull-out force of the hook-shaped hook element and the loop-shaped hook element was measured, and the results were 6.5 N and 9.9 N, respectively, indicating that the pull-out resistance was also very excellent. In addition, the hook and loop fastener was placed on a flat glass plate in the same manner as in Examples 1 and 2, and the hook and loop fastener was observed to see if there was any undulation in the vertical direction, and the result was that no undulation was observed at all.
[0216] In addition, the hooking force of the hook / loop fastener was measured, and the initial hooking force was 10.1 N / cm in shear strength. 2 , the peel strength is 1.02N / cm, and the hooking force after 1000 hooking / peeling is 9.6N / cm in shear strength 2 The peel strength was 0.97 N / cm, which is a very excellent value for a hook / loop type fastener. Moreover, even after 1000 times of hooking / peeling, no hooking elements were observed to be pulled out from the surface of the hook / loop type fastener, which shows that although there is no back coating, it is very excellent as a hook / loop type fastener.
[0217] The hook / loop coexisting type fastener is very soft, so when the ears are sewn to the cuffs of clothes by sewing with sewing yarn, the sewing yarn does not meander and the center of the ears can be sewn into a straight line, which is also excellent in appearance.
[0218] Comparative Example 3
[0219] [Manufacturing of Hook / Loop Type Velcro]
[0220] In the above-mentioned Example 3, the fixing surface installed next to the outlet of the heat treatment furnace is removed, and the process of pressing the back side of the Velcro to the fixing surface while the hot-melt adhesive multifilament yarn after heat treatment remains in a molten state is omitted. The Velcro taken out of the heat treatment furnace is pulled with a roller after cooling. Except for this, the same procedure as the above-mentioned Example 3 is carried out to produce a hook / loop coexisting type Velcro.
[0221] [Performance of the obtained hook / loop type fastener, etc.]
[0222] The obtained hook / loop type fastener has a hook element area with a width of 20 mm, and ears with an average width of 2.5 mm without hook elements are present at both ends parallel to the warp direction. The density of hook elements of the hook / loop type fastener is 28 pieces / cm 2 , the density of the loop hook elements is 28 pieces / cm 2 In addition, the height of the hook-shaped hooking element from the base fabric surface is 1.8 mm, and the height of the loop-shaped hooking element from the base fabric surface is 2.1 mm. Moreover, the flame retardancy of the hook / loop coexisting type fastener is 3.4 seconds, which is excellent.
[0223] The cut state of the hook-shaped hooking element of the hook / loop coexisting hook and loop fastener was observed, and the result was the same as that of Comparative Example 1, and although the amount was small, it was observed that it was cut near the root, and it was almost cut near the top, etc. Then, the hook and loop fastener was placed on a horizontal glass plate, and the undulation state was observed. The result was the same as that of the hook hook and loop fastener of Comparative Example 1 and Comparative Example 2, and large undulations and small undulations were frequently observed in the up and down direction.
[0224] In addition, the pull-out force of the hook-shaped hook element and the pull-out force of the loop-shaped hook element were measured, and the results were 4.1N and 8.6N, respectively, both of which were worse than those in Example 3. In addition, the hook-in force of the hook / loop type fastener was measured, and the initial hook-in force was 9.2N / cm in shear strength. 2 The peel strength is 0.92N / cm, and the hook strength after 1000 hooking / peeling is 8.1N / cm in shear strength. 2The peel strength was 0.80 N / cm. After 1000 repetitions of hooking / peeling, a small amount of hook-shaped hooking elements were observed to be pulled out from the surface of the hook / loop combined type fastener.
[0225] The (Tb) / (Ts) of the hook / loop coexisting type fastener is 0.97. As with the fastener of Example 3, the hook / loop coexisting type fastener is sewed to the cuffs of clothes using sewing yarn using its ears, but it is difficult to sew the central part of the ears using sewing yarn, and as a result, the sewing yarn is observed to meander, which is also inferior to Example 3 in terms of appearance.
[0226] Example 4
[0227] [Manufacture of hook and loop fasteners]
[0228] In the above-mentioned Example 1, the fixed surface to be pressed was replaced with the mirror-finished roller surface made of stainless steel with a rough surface when the hot-melt adhesive core-sheath type filament was kept in a molten state, and the hook fastener was manufactured in the same manner as in Example 1. It should be noted that the above-mentioned roller surface was rotated at a speed 5 mm / second slower than the travel speed of the hook fastener fabric that was in contact and moving, and the contact time between the back of the base fabric and the roller surface was 5 seconds. The hot-melt adhesive fiber was pressed to the roller surface while being kept in a molten state, and it was made to slide on the roller surface. Moreover, a tension of 250 g / cm was applied to the base fabric after passing through the roller surface. It should be noted that from the above-mentioned weaving process to the heat treatment process, the process of crimping to the roller surface, and then the single-leg cutting process of the hook-shaped hooking element, it was not wound up in the middle and was carried out continuously.
[0229] [Performance of the obtained hook fastener, etc.]
[0230] The width of the obtained hook fastener fabric was 20 mm in the region where the hook elements were present, and ears with a width of 2.5 mm without hook elements were present at both ends in parallel with the warp direction with a uniform width. The density of hook-shaped hook elements and the height of hook-shaped hook elements from the base fabric surface of the hook fastener were the same as those of Example 1. In addition, the flame retardancy of the hook fastener was 3.5 seconds, which was also very excellent as in Example 1. (Tb) / (Ts) of the hook fastener was 0.92.
[0231] In addition, it can be seen that the pull-out force of the hook-shaped hook element of the hook fastener is 6.0N, and the pull-out resistance is also excellent. In addition, the hook fastener is placed on a flat glass plate, and the hook fastener is observed to have ups and downs. The result is that although basically no large ups and downs are observed, a few parts are observed to be slightly raised from the glass surface. Regarding the cut state of the hook-shaped hook element, although any hook-shaped hook element is cut at a position of approximately 70% of the height of one leg, it is observed that the cut position is slightly offset in the up and down direction.
[0232] Furthermore, the hooking force of the hook fastener was measured, and the initial hooking force was 12.0 N / cm in terms of shear strength. 2 , the peel strength is 1.35N / cm, and the hooking force after 1000 hooking / peeling is 10.9N / cm in shear strength 2 , and the peel strength was 1.21 N / cm, which is an excellent value. Moreover, even after 1000 times of hooking / peeling, almost no hook-shaped hooking elements were observed to be pulled out from the surface of the hook fastener. When the ear of the hook fastener is used and sewn on the cuff of clothing with sewing yarn, the sewing yarn does not meander and the center of the ear can be sewn in a substantially straight line, but it is also observed that a part of the center is slightly deviated.
[0233] Example 5
[0234] [Manufacturing of Velcro]
[0235] In the above-mentioned Example 2, as in Example 4, the fixed surface that is pressed while the hot-melt-adhesive core-sheath type filaments are kept in a molten state is replaced with a stainless steel roller surface with a roughened surface, and a loop fastener is manufactured in the same manner as in Example 2. The rotation speed and tension of the roller surface at this time are the same as those in Example 2.
[0236] [Performance of the obtained loop fastener, etc.]
[0237] The width of the loop hook and loop fastener fabric obtained and the width of the ear portion are the same as those in Example 2, and the ear portion is parallel to the warp direction with a uniform width. Moreover, the density of the loop hook elements of the loop hook and the height of the loop hook elements from the base fabric surface of the loop hook and loop fastener are the same as those in Example 2. The flame retardancy of the loop hook and loop fastener is 3.3 seconds, which is very excellent. The (Tb) / (Ts) of the loop hook and loop fastener is 0.93.
[0238] In addition, it can be seen that the pull-out force of the loop hook element of the loop fastener is 9.6 N, and the pull-out resistance is also excellent. In addition, the fastener is placed on a flat glass plate to observe whether the fastener has ups and downs in the vertical direction. As a result, no large ups and downs are observed, but similar to the fastener of Example 4, parts slightly raised from the glass surface are observed in many places.
[0239] In addition, the hooking force of the loop of hook and loop fastener was measured, and the result was that the initial hooking force was 11.8 N / cm in shear strength. 2 , the peel strength is 1.31N / cm, and the hooking force after 1000 hooking / peeling is 10.5N / cm in shear strength 2 When the ear of the loop hook and loop fastener is sewn on the cuff of clothing with sewing yarn, the sewing yarn basically does not meander, and the center of the ear can be sewn into a straight line, but as in the case of the above-mentioned Example 4, a part of the center is observed to deviate, and the appearance is slightly worse than that of Example 2.
[0240] Comparative Example 4
[0241] [Manufacture of hook and loop fasteners]
[0242] In the above-mentioned Example 1, instead of using the parallel yarn of the polyphenylene sulfide-based multifilament yarn and the multifilament yarn formed of the hot-melt adhesive filament as the weft yarn, the following yarn consisting of only the multifilament yarn formed of the core-sheath type composite filament was used, and the hook fastener was manufactured in the same manner as in Example 1.
[0243] [Weft yarn (multifilament yarn formed of core-sheath type composite filaments)]
[0244] The core component, sheath component and core-sheath ratio are the same as those used for the weft yarn of Example 1.
[0245] Total decimal point and number of filaments: 240dtex, 48 filaments
[0246] Dry heat shrinkage at 200°C: 17.0%
[0247] [Performance of the obtained hook fastener, etc.]
[0248] The obtained hook fastener had no problems with the undulation in the vertical direction, the pull-out resistance of the hook element, the hooking force, etc., but the flame retardancy was 19.2 seconds, which was significantly worse than that of Example 1 and was a flame retardancy level that could not be used for aircraft applications.
[0249] Example 6
[0250] [Manufacture of hook and loop fasteners]
[0251] In the above-mentioned Example 1, the PPS type multifilament yarn used as the weft yarn and the PPS type multifilament yarn used for the parallel yarn of the multifilament yarn formed by the hot-melt adhesive filaments were replaced with the following PPS type multifilament yarn, and then the same method as in Example 1 was used to manufacture a wide hook and loop fastener tape having four 20 mm wide regions with hook elements in parallel to the warp direction, an ear portion with a width of 2.5 mm at one end thereof, three 5 mm wide middle ear regions sandwiched by the hook element regions in parallel to the warp direction, and the hook element regions and the middle ear regions alternately in the weft direction, and finally, the central portion of the middle ear region was cut in parallel to the warp direction to manufacture four hook and loop fastener tapes. It should be noted that the manufacturing conditions other than this were the same as those in Example 1.
[0252] [Multifilament yarn made of PPS used for parallel yarn of weft]
[0253] Total decimal point and number of filaments: 250dtex, 60 filaments
[0254] Dry heat shrinkage at 200°C: 7.8%
[0255] [Performance of the obtained hook fastener, etc.]
[0256] The density of the hook-shaped hook elements and the height of the hook-shaped hook elements from the base fabric surface of the four hook fasteners obtained were substantially the same as those of Example 1. With regard to the cut state of the hook-shaped hook elements of the fastener, any hook-shaped hook element was cut at a position approximately 70% of the height of one leg. Moreover, the flame retardancy of the hook fastener was measured and the result was 2.0 seconds, which was also very excellent as in Example 1. In addition, the (Tb) / (Ts) of the hook fastener was 0.87.
[0257] The pull-out force of the hook-shaped hooking element of the hook fastener is 6.1N, and the pull-out resistance is slightly worse than that of Example 1, but still very excellent. In addition, similar to Example 1, no fluctuation of the hook fastener in the vertical direction is observed, and the central part of the middle ear area is accurately cut, and the width of the ear portion produced is also constant at 2.5mm. When the hook fastener is cut into a length of 15cm and washed repeatedly 50 times, no scattering from the cut ear end is observed.
[0258] Furthermore, the hooking force of the hook fastener was measured, and the initial hooking force was 12.2 N / cm in terms of shear strength. 2 The peel strength is 1.36N / cm, and the hook strength after 1000 hooking / peeling is 11.1N / cm in shear strength. 2The peel strength was 1.24 N / cm, which is a very excellent value. Even after 1000 repetitions of hooking / peeling, almost no hook-shaped hooking elements were pulled out from the surface of the hook fastener, and no hook-shaped hooking elements were observed to be broken by tension in the hook state.
[0259] When the ear portion of the hook and loop fastener is used and sewn on the cuff of clothing with sewing yarn, the sewing yarn can easily sew the center portion of the ear portion into a straight line.
[0260] Comparative Example 5
[0261] [Manufacture of hook and loop fasteners]
[0262] In the above-mentioned Example 6, the fixed surface made of stainless steel arranged next to the outlet of the heat treatment furnace was removed, and the operation of pressing the back side of the Velcro while the hot-melt adhesive multifilament yarn remained in a molten state after the heat treatment was not performed. A method of pulling with a roller after cooling was used. Except for this, four hook fasteners were produced in the same manner as in the above-mentioned Example 6.
[0263] [Performance of the obtained hook fastener, etc.]
[0264] For the hook Velcro tape obtained, all the same as Example 6, the width in the hooking element zone of wide 20mm is 20mm, and there is the ear of average width 2.5mm parallel to the warp direction at its two ends.The cut-off state of the hook-shaped hooking element of this hook Velcro tape is observed, and the result is the same as Comparative Example 1, and the ups and downs condition of the up-down direction of this Velcro tape also does not observe big ups and downs, tiny ups and downs in the same manner as Comparative Example 1, and can observe the position that rises from the glass plate repeatedly.For the ear after the slitting, because ups and downs are difficult to the middle ear accurately slitting with the central part of the region so that width becomes 2.5mm, the position of wide width and the position of narrow width can be seen everywhere.In addition, when this Velcro tape is cut into length 15cm and repeatedly washed 50 times, in about 20% Velcro tape, the situation that the end of the ear of the warp yarn after the slitting is observed to have occurred is scattered.
[0265] The pull-out force and hooking force of the hook-shaped hooking elements of the hook fastener were substantially the same as those of Comparative Example 1, and the number of hook-shaped hooking elements pulled out from the surface after 1,000 repetitions of hooking / peeling was also the same as that of Comparative Example 1. (Tb) / (Ts) of the hook fastener was 0.96, the same as that of Comparative Example 1. In addition, when the hook fastener was attached to the cuff of clothing using an ear portion with a sewing machine, it was difficult to sew the center portion with sewing yarn because the width of the ear portion was uneven and meandering.
[0266] Example 7
[0267] [Manufacturing of Velcro]
[0268] In the above-mentioned Example 2, the PPS type multifilament yarn used as the weft yarn and the PPS type multifilament yarn used for the parallel yarn of the multifilament yarn formed by the hot-melt adhesive filaments were replaced with the same PPS type multifilament yarn as the PPS type multifilament yarn used in the above-mentioned Example 6. In addition, the same method as in Example 2 was used to manufacture a loop fastener in which a hook element area with a width of 20 mm and an ear area with a width of 5 mm alternately existed in the weft direction, and finally the central part of the ear area was cut parallel to the warp direction to manufacture 4 loop fasteners. It should be noted that the manufacturing conditions other than this were the same as those in Example 2 except that the tension after passing through the fixed surface was changed from 200 g / cm to 400 g / cm.
[0269] [Performance of the obtained loop fastener, etc.]
[0270] The density and height of the loop-shaped hook elements from the base fabric surface of the obtained four-loop hook and loop fastener were substantially the same as those of Example 2. The flame retardancy of the loop hook and loop fastener was measured and the result was 3.3 seconds, which was also very excellent as in Example 2. In addition, the (Tb) / (Ts) of the loop hook and loop fastener was 0.82.
[0271] The pull-out force of the loop-shaped hooking element of this loop hook and loop fastener is 9.8N, and about pull-out resistance, it is also very excellent. In addition, similarly to Example 2, the ups and downs of this hook and loop fastener in the vertical direction are not observed at all, and in addition, the width of the ear produced by the middle ear region by slitting is 2.5mm, and exists in a straight line parallel to the warp direction. In addition, when this hook and loop fastener is cut into a length of 15cm and repeatedly washed 50 times, similarly to the hook hook and loop fastener of above-mentioned Example 6, the warp yarn is not observed to be scattered from the ear after slitting at all.
[0272] In addition, the hooking force of the loop of hook and loop fastener was measured, and the result was that the initial hooking force was 12.0 N / cm in shear strength. 2 , the peel strength is 1.34N / cm, and the hooking force after 1000 hooking / peeling is 10.8N / cm in shear strength 2 , and the peel strength was 1.21 N / cm, which is a very excellent value. Even after 1000 times of hooking / peeling, no loop-shaped hooking element was observed to be pulled out from the surface of the loop hook and loop fastener. When the ear of the loop hook and loop fastener is sewn on the cuff of clothing with sewing yarn, the sewing yarn can sew the center of the ear into a straight line, which is also excellent in appearance.
[0273] Comparative Example 6
[0274] [Manufacturing of Velcro]
[0275] In the above-mentioned Example 7, the stainless steel fixed surface arranged next to the outlet of the heat treatment furnace was removed, and the operation of pressing the back side of the Velcro while the hot-melt adhesive multifilament yarn remained in a molten state after the heat treatment was not performed. Instead, a method of pulling with a roller after cooling was used. Except for this, the same procedure as the above-mentioned Example 7 was carried out to produce 4 loop Velcro.
[0276] [Performance of the obtained loop fastener, etc.]
[0277] The obtained loop fasteners were all the same as those in Example 7, with a width of 20 mm in the hooking element region of 20 mm, and ears with an average width of 2.5 mm at both ends parallel to the warp direction. As for the ups and downs of the loop fastener, large ups and downs and small ups and downs were observed in the same manner as in Comparative Example 2. As for the ears after slitting, it was difficult to accurately slit the central part of the middle ear region due to the ups and downs, and wide and narrow parts were frequently observed.
[0278] The pull-out force and hooking force of the loop hooking element of the loop hook and loop fastener are substantially the same as those of Comparative Example 2. The (Tb) / (Ts) of the hook hook and loop fastener is 0.97, which is the same as that of Comparative Example 2. In addition, when the loop hook and loop fastener is attached to the cuff of a garment using its ears by a sewing machine, it is difficult to sew the center portion of the ears with sewing yarn because of the uneven width and the winding shape of the ears.
[0279] Example 8
[0280] [Manufacture of hook and loop fasteners]
[0281] In the above-mentioned Example 1, a hook fastener was produced under the same conditions as in Example 1 except that the tension after passing through the fixed surface was changed from 200 g / cm to 640 g / cm.
[0282] [Performance of the obtained hook fastener, etc.]
[0283] The density of hook-shaped hook elements and the height of hook-shaped hook elements from the base fabric surface of the obtained hook fastener are exactly the same as those in Example 1, and the cut state of the hook-shaped hook elements of the hook fastener is also very uniform as in Example 1. In addition, the flame retardant performance is also very excellent as in Example 1.
[0284] The warp thickness (Tb) of the hook fastener in the base fabric thickness direction at the most sunken portion on the back side and the warp thickness (Ts) of the hook fastener in the base fabric thickness direction at the most raised portion on the front side were measured. The result showed that (Tb) / (Ts) was 0.76.
[0285] The pull-out force of the hook-shaped hooking element of the hook fastener was 6.2 N, and the pull-out resistance was also very excellent as in Example 1. In addition, no ups and downs of the hook fastener were observed at all as in Example 1. In addition, the hooking force of the hook fastener was measured, and the result was that the initial hooking force was 12.2 N / cm in terms of shear strength. 2 The peel strength is 1.36N / cm, and the hook strength after 1000 hooking / peeling is 11.1N / cm in shear strength. 2 The peel strength was 1.24 N / cm, which was a very excellent value. Even after 1000 repetitions of hooking / peeling, no hook-shaped hooking elements were pulled out from the surface of the hook fastener, and no hook-shaped hooking elements were observed to be broken by tension in the hook state.
[0286] When the ear of the hook fastener is used and sewn on the cuff of clothing with sewing yarn, the sewing yarn can sew the center of the ear into a straight line. However, since the base fabric of the hook fastener is more rigid than that of Example 1, the operability is slightly worse when it is installed on the cloth. In addition, due to its rigidity, it is not necessarily suitable for use in contact with the human body such as clothing.
[0287] Example 9
[0288] [Manufacturing of Velcro]
[0289] In the above-mentioned Example 2, a loop fastener was produced under the same conditions as in Example 2 except that the tension after passing through the fixed surface was changed from 200 g / cm to 560 g / cm.
[0290] [Performance of the obtained loop fastener, etc.]
[0291] The density of the loop hook elements and the height of the loop hook elements from the base fabric surface of the obtained loop fastener were exactly the same as those in Example 2. In addition, the flame retardant performance was also very excellent as in Example 2. The (Tb) / (Ts) of the loop fastener was 0.74.
[0292] The pull-out force of the loop hook element of the loop hook tape was 10.2 N, and the pull-out resistance was also very excellent as in Example 2. In addition, no ups and downs of the loop hook tape were observed at all as in Example 2. The hook force of the loop hook tape was measured, and the initial hook force was 12.0 N / cm in shear strength. 2 , the peel strength is 1.34N / cm, and the hooking force after 1000 hooking / peeling is 10.7N / cm in shear strength 2The peel strength was 1.20 N / cm, which was a very excellent value. Even after the hooking / peeling was repeated 1,000 times, no loop-shaped hooking elements were observed to be pulled out from the surface of the loop fastener.
[0293] When the ear of the loop fastener is used and sewn on the cuff of clothing by sewing yarn, the sewing yarn makes the central part of the ear exist in a straight line. However, since the base fabric of the fastener is slightly more rigid than that of Example 2, it is considered that it is not necessarily the most suitable for contacting the human body, just like the hook fastener of Example 8.
[0294] Comparative Example 7
[0295] [Manufacture of hook and loop fasteners]
[0296] In the above-mentioned Example 1, a fixed surface made of stainless steel with a mirror-finished surface disposed next to the outlet of the heat treatment furnace was placed 85 cm away from the outlet, and heated from the back side of the fixed surface in such a manner that the surface temperature of the fixed surface reached 160° C. The hook fastener fabric tape of the above-mentioned Example 1 which had been heat-treated was pulled out from the outlet of the heat treatment furnace, and allowed to travel 85 cm (it was confirmed that the tape was naturally cooled during the travel, and the hot melt adhesive component used for the weft yarn was fully solidified), the back side of the cooled tape was pressed against the fixed surface having a surface temperature of 160° C. for 5 seconds, and was slid on the surface, and the travel direction was further bent 90 degrees along the surface, and the operation of pulling it out under a tension of 200 g / cm after passing through the fixed surface was implemented. The hook fastener tape was manufactured by the same method as in Example 1 except that the hook fastener tape was pulled out under a tension of 200 g / cm after passing through the fixed surface.
[0297] [Performance of the obtained hook fastener, etc.]
[0298] The obtained hook fastener had very similar performance to that of Comparative Example 1, that is, it had excellent flame retardancy as that of Example 1, but when placed on a horizontal glass plate, large and small fluctuations in the vertical direction were observed. In addition, it was observed in many places that the root of one leg of the hook-shaped hook element was not cut off and remained in a loop, both legs were cut off, and only one leg was cut halfway. The density of the hook-shaped hook element was 56 pieces / cm 2 The height of the hook-shaped hook element from the base fabric surface was 1.8 mm. Regarding the single-leg cut state of the hook-shaped hook element, it was also observed that the hook-shaped hook element was cut at a position close to the installation root and at a position close to the top.
[0299] In addition, the pull-out force of the hook-shaped hooking element was 4.4 N, which was significantly inferior to that of Example 1. In addition, the hooking force of the hook fastener was measured, and the initial hooking force was 11.8 N / cm in terms of shear strength. 2, the peel strength is 1.29N / cm, and the hook strength after 1000 hooking / peeling is 9.9N / cm in shear strength 2 The peel strength was 1.04 N / cm. After 1000 repetitions of hooking / peeling, hook-shaped hooking elements were scattered and seen being pulled out from the surface of the hook fastener.
[0300] The (Tb) / (Ts) of the hook fastener was 0.96. When the hook fastener was attached to the blank using the sewing yarn using the ear portion, it was difficult to sew the center of the ear portion with the sewing yarn, and as a result, the sewing yarn was observed to meander, which was inferior to Example 1 in terms of appearance.
[0301] Comparative Example 8
[0302] [Manufacture of hook and loop fasteners]
[0303] With the hook element surface facing the outside, the hook fastener made by the above-mentioned comparative example 1 was wound into a roll without being pressed onto a stainless steel heating roller with a diameter of 12.5 cm and having a smooth surface, and a heat treatment of 195° C. was performed for 20 minutes in this state. It should be noted that in order to prevent the hook element from being overwhelmed by the pressure during winding as much as possible, a winding method in which the hook fastener of the lower layer is wound without being pressed by the hook fastener of the upper layer, that is, the winding method in which the hook fastener is not wound tightly as much as possible, is utilized. Moreover, after the heat treatment is completed, the hook fastener is cooled and removed from the heating roller, and the performance of the hook fastener after the heat treatment, the state of the hook-shaped hook element, etc. are observed / measured.
[0304] [Performance of the obtained hook fastener, etc.]
[0305] The result is that at first glance, there is basically no change compared to Comparative Example 1. However, when the Velcro is placed statically on a horizontal glass plate, large and small undulations in the up and down directions are observed. It does not adhere tightly to the glass plate, and the effect of eliminating undulations brought about by the above-mentioned heat treatment is not obtained at all.
[0306] The pull-out force of the hook-shaped hooking element of the hook fastener was measured, and the result was 4.1 N, which was approximately the same as that of Comparative Example 1. In addition, the hooking force of the hook fastener was measured, and the result was that both the initial hooking force and the hooking force after 1000 hooking / peeling were approximately the same as those of Comparative Example 1. After 1000 times of hooking / peeling, hook-shaped hooking elements were scattered and seen being pulled out from the surface of the hook fastener.
[0307] The (Tb) / (Ts) of the hook fastener was 0.96, which was unchanged from that of Comparative Example 1. In addition, when the hook fastener was attached to the cuff of clothing by sewing with the sewing yarn using the ear portion, it was difficult to sew the central portion of the ear portion with the sewing yarn, and the sewing yarn of the fastener of the cuff that was sewn was meandering in many places.
[0308] Comparative Example 9
[0309] [Manufacture of hook and loop fasteners]
[0310] In Example 4, a hook fastener was produced in the same manner as in Example 4 except that the surface speed of the roller surface was made the same as the running speed of the hook fastener fabric and the back side of the fabric was pressed against the roller surface but not slid on the roller surface.
[0311] [Performance of the obtained hook fastener, etc.]
[0312] Although the cut state of the hook-shaped hooking element of the obtained hook fastener was improved compared with the state of Comparative Example 1, it was observed that the hook-shaped hooking element was cut at a position close to the installation root, cut at a position close to the top, the root of one leg was not cut and was looped, both legs were cut and did not form a hook shape, and only one leg was cut halfway. Although the undulation of the hook fastener was improved compared with Comparative Example 1, large undulation was observed in a part, and fine undulation was observed.
[0313] The pull-out force and hooking force of the hook-shaped hooking elements of the hook fastener tape, and the state of the hook-shaped hooking elements being pulled out from the surface of the hook fastener tape after 1000 repetitions of hooking / peeling were the same as those of Comparative Example 1. In addition, (Tb) / (Ts) of the hook fastener tape was 0.95.
[0314] In addition, the condition of attaching the ear portion of the hook fastener to the clothes using the sewing yarn was slightly improved compared with Comparative Example 1, but the result was roughly similar to that of Comparative Example 1.
[0315] Comparative Example 10
[0316] [Manufacturing of Velcro]
[0317] In the above-mentioned Example 5, the surface speed of the roller surface is made the same as the traveling speed of the loop fastener fabric as in the above-mentioned Comparative Example 9, and the back side of the loop fastener fabric is pressed onto the roller surface but does not slide on the roller surface. Except for this, the loop fastener is manufactured by the same method as Example 5.
[0318] [Performance of the obtained loop fastener, etc.]
[0319] The (Tb) / (Ts) of the obtained loop fastener was 0.96, and the pull-out force of the loop hook element was 8.8 N, which was similar to the performance of Comparative Example 2. In addition, the undulation of the loop fastener in the vertical direction was not substantially improved, and a large number of raised parts were observed in the same manner as in Comparative Example 2. In addition, the hooking force of the loop fastener, the ease of sewing using the ear portion, etc. were poor results, similar to those of Comparative Example 9.
[0320] Example 10
[0321] The hook fastener obtained in Example 1, the loop fastener obtained in Example 2, and the hook / loop combined fastener obtained in Example 3 were dyed under the following dyeing conditions to obtain three types of fasteners dyed in deep black.
[0322] [Dyeing conditions]
[0323] Dye: Tuxedo Black H (made by DEISTER) 7% owf
[0324] Additive: Niccasunsalt SN SN130 (manufactured by Nikka Chemical Co., Ltd.) 2g / l
[0325] Texport SN10 (manufactured by Nikka Chemical Co., Ltd.) 2g / l
[0326] Sunmall 1201g / l
[0327] Acetic acid 2g / l
[0328] MYS0.10%
[0329] Bath ratio: 1:15
[0330] Dyeing temperature / time: 135°C x 120 minutes (30 minutes to raise the temperature from 40°C to 135°C, and keep at 135°C for 120 minutes)
[0331] Reduction cleaning: caustic soda 1g / l
[0332] Thiourea dioxide 0.5g / l
[0333] Escudo NEO‐2E1g / l
[0334] 80℃×15min
[0335] Wash with water; 15 minutes
[0336] Drying: 60℃×30min
[0337] All the hook and loop fasteners were dyed in dark colors, and the color fastness to friction and hot water of the dyed products were excellent, and were able to withstand use under extremely harsh conditions. In addition, the flame retardancy and hook strength did not change compared to before dyeing, and the (Tb) / (Ts) ratio did not change compared to before dyeing.
Claims
1. A flame retardant hook and loop fastener comprising a base fabric and hook elements present on the surface of the base fabric, The base fabric is woven from warp yarns, weft yarns, and yarns for hooking elements, wherein the warp yarns are composed of polyphenylene sulfide multifilament yarns, the weft yarns are composed of polyphenylene sulfide multifilament yarns and multifilament yarns composed of hot-melt adhesive filaments, and the yarns for hooking elements are composed of at least one selected from polyphenylene sulfide multifilament yarns and monofilament yarns. The hook element is formed by the hook element yarn, The thickness of the warp yarn in the base fabric thickness direction at the part most sunk on the back side of the warp yarn that bulges / sinks above and below with the weft yarn sandwiched therebetween is 0.94 times or less of the thickness of the warp yarn in the base fabric thickness direction at the part most bulged on the front side.
2. The flame retardant hook and loop fastener according to claim 1, which satisfies: The thickness of the warp yarn in the base fabric thickness direction at the part most sunken on the back side of the warp yarn that bulges / sinks above and below the weft yarn is in the range of 0.70 to 0.90 times the thickness of the warp yarn in the base fabric thickness direction at the part most bulging on the front side.
3. The flame retardant hook and loop fastener according to claim 1 or 2, in, The weft yarn is a parallel yarn of a polyphenylene sulfide multifilament yarn and a hot-melt adhesive multifilament yarn, wherein the polyphenylene sulfide multifilament yarn is formed by bundling 5 to 90 filaments having a thickness of 3 to 30 dtex and a total thickness of 120 to 300 dtex, and the hot-melt adhesive multifilament yarn is formed by bundling 15 to 40 polyester core-sheath type filaments having a thickness of 3 to 8 dtex and a sheath component having a low melting point hot-melt adhesive component, and a total thickness of 80 to 150 dtex.
4. The flame-retardant hook and loop fastener according to any one of claims 1 to 3, in, On the surface of the hook fastener, the hook element area with hook elements and the ear area without hook elements are continuous in the warp direction, and the hook element area and the ear area alternate in the weft direction, and there are multiple hook element areas.
5. The flame-retardant hook and loop fastener according to any one of claims 1 to 4, in, The hooking element is a hook-shaped hooking element, and the pulling force of the hook-shaped hooking element pulled out from the base fabric is 5N or more.
6. The flame-retardant hook and loop fastener according to any one of claims 1 to 5, in, There is no back-coating resin layer on the back of the base fabric. 7 . The flame-retardant hook and loop fastener according to claim 1 , which is colored with a pigment or a disperse dye.
8. A method for manufacturing a flame-retardant hook and loop fastener, the hook and loop fastener comprising a base fabric and at least one of a plurality of hook-shaped hook elements and a plurality of loop-shaped hook elements formed by hook element yarns present on the surface of the base fabric, the base fabric being woven from warp yarns, weft yarns, and hook element yarns, the warp yarns being composed of polyphenylene sulfide multifilament yarns, the weft yarns being composed of polyphenylene sulfide multifilament yarns and multifilament yarns composed of hot-melt adhesive and heat-shrinkable filaments, the hook element yarns being composed of at least one of multifilament yarns and monofilament yarns selected from polyphenylene sulfide, The method sequentially performs the following steps A, B, C and D: [Step A] When weaving a base fabric from warp yarns and weft yarns, a hook element yarn is woven in parallel with the warp yarns, and at the same time, the hook element yarn is made to regularly cross over the warp yarns, and the hook element yarn is made to stand up in a loop shape from the surface of the base fabric at the crossing portion to weave a loop fabric; [Step B] A step of introducing the loop fabric into a heating area, heating the loop fabric to a temperature above which the hot-melt component of the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments melts, thermally shrinking the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments, and fixing the hook element yarn to the base fabric by a molten product from the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments; [Step C] A step of taking the loop fabric out of the heating zone of step B, and sliding the back side of the base fabric against a fixed surface or a roller surface while the hot-melt adhesive component of the multifilament yarn formed of the hot-melt adhesive and heat-shrinkable filaments is melted; [Step D] A step of taking out the loop fabric from step C, cooling the loop fabric, and then, if the engaging element yarn is a monofilament yarn, cutting a single leg of the loop to form a hook-shaped engaging element.
9. The method for producing the flame-retardant hook and loop fastener according to claim 8, in, In the step C, the loop fabric is moved forward while the back surface of the loop fabric is pressed against the fixed surface and the loop fabric is slid on the fixed surface, and the moving direction of the loop fabric is changed on the fixed surface.
10. The method for producing the flame-retardant hook and loop fastener according to claim 8 or 9, in, The loop fabric taken out from the step B is not temporarily cooled, and the step C is performed after the step B using the residual heat of the step B.
11. The method for producing the flame-retardant hook and loop fastener according to any one of claims 8 to 10, in, The dry heat shrinkage rate of the multifilament yarn formed of the heat-fusible and heat-shrinkable filaments at 200° C. is in the range of 10 to 24%.
12. The method for producing the flame-retardant hook and loop fastener according to any one of claims 8 to 11, in, The tension applied to the loop fabric in step C is set to 50 to 600 g / cm.
13. The method for producing the flame-retardant hook and loop fastener according to any one of claims 8 to 12, in, From step A to step D, the process is performed continuously without winding up in the middle.
14. A method for producing a flame-retardant hook and loop fastener according to any one of claims 8 to 13, in, In the step A, a loop fabric is woven, and on the surface of the loop fabric, a hooking element region with hooking element loops and an ear region without hooking element loops are respectively present continuously in the warp direction, and the hooking element region and the ear region are alternately present in the weft direction, and there are a plurality of hooking element regions. Then, after the step D, the center of the ear region is cut in the warp direction, and a plurality of hook and loop fasteners that are continuous in the warp direction and have ears at both ends are manufactured at the same time.