Pad and method for manufacturing same
Through the twisting and interweaving of inorganic fibers and the use of appropriate binders, the problem of insufficient surface pressure of paper-made mats is solved, the elasticity and shape maintenance of the fibers are improved, and efficient mat performance is achieved.
Patent Information
- Application Number
- CN202480001305.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-11
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-22
AI Technical Summary
The surface pressure of the existing paper-made mats is insufficient, the alumina fibers are easy to break, and the fibers become shorter after the massive condensed fibers are opened, resulting in insufficient fiber interweaving and insufficient elasticity, making it difficult to increase the surface pressure.
Inorganic fibers are used to intertwine and form fiber bundles in a twisting manner. The average length of the fiber bundles is 5 to 15 mm and the width is 0.2 to 1.0 mm, including the crimped fiber bundles. The drawing length measurement method is used to ensure that the drawing length of the fiber bundles is larger than the actual length. The length should be 0.1mm or more, and organic and inorganic binders should be used for moderate bonding. Water-soluble organic polymers, alumina and other materials are preferably used.
The surface pressure of the paper-made mat is increased, the elasticity and shape maintenance of the fibers are enhanced, the inorganic fibers are prevented from breaking due to pressure, the fibers are inhibited from falling off and flying, and the overall performance of the mat material is improved.
Smart Images

Figure CN118742689A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a papermaking mat and a method for producing the papermaking mat. Background Art
[0002] Exhaust gas discharged from internal combustion engines such as diesel engines contains particulate matter (hereinafter also referred to as PM), and in recent years, the harm caused by PM to the environment and human body has become a problem. In addition, since the exhaust gas also contains harmful gas components such as CO, HC, and NOx, there are also concerns about the impact of these harmful gas components on the environment and human body.
[0003] Therefore, various exhaust gas purification devices have been proposed as exhaust gas purification devices for capturing PM in exhaust gas or purifying harmful gas components, which include: an exhaust gas treatment body composed of porous ceramics such as silicon carbide or cordierite, a shell for accommodating the exhaust gas treatment body, and a holding sealing material (mat) arranged between the exhaust gas treatment body and the shell. The holding sealing material (mat) is mainly arranged for the following purposes: preventing the exhaust gas treatment body from contacting with the shell covering its outer periphery and being damaged due to vibration or impact generated by the driving of the car, etc.; preventing exhaust gas from leaking from between the exhaust gas treatment body and the shell; etc.
[0004] In order to increase the force (surface pressure) of the mat member in holding the exhaust gas treatment body, Patent Document 1 discloses a mat member in which the surface pressure is increased by producing an alumina fiber aggregate using a specific spinning aid.
[0005] In addition, Patent Document 2 discloses that a needle punched sheet is prepared, the needle punched sheet is dry-opened to obtain opened fibers containing bulk agglomerated fibers, and then a paper sheet is prepared using the opened fibers containing bulk agglomerated fibers. Furthermore, Patent Document 2 describes that the surface pressure of the paper sheet is increased by including bulk agglomerated fibers.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2018 / 012423
[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-82310 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The mat material described in Patent Document 1 has the problem that the alumina fibers are easily broken and the surface pressure is easily reduced.
[0012] Since the paper-made sheet described in Patent Document 2 is a needle-punched sheet subjected to dry fiber opening, the fibers after fiber opening become shorter, and the fibers constituting the bulk coagulated fibers also become shorter. Therefore, in the bulk coagulated fibers, the fibers are not fully intertwined, and the bulk coagulated fibers do not have a twisted shape. In addition, the length of the bulk coagulated fibers is also shortened. Therefore, the elasticity of the bulk coagulated fibers does not become sufficiently high, and there is a problem that the surface pressure of the manufactured paper-made sheet is difficult to become sufficiently high.
[0013] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a papermaking mat having a sufficiently high surface pressure.
[0014] Means for solving problems
[0015] That is, the papermaking mat of the present invention is a papermaking mat composed of inorganic fibers, characterized in that the above-mentioned papermaking mat contains a fiber bundle formed by interweaving more than 10 of the above-mentioned inorganic fibers in a twisted manner and the above-mentioned inorganic fibers that do not constitute the above-mentioned fiber bundle, the average length of the above-mentioned fiber bundle is 5 to 15 mm, the average width of the above-mentioned fiber bundle is 0.2 to 1.0 mm, the above-mentioned fiber bundle includes a fiber bundle in a curled state, and the drawing length of the above-mentioned fiber bundle in the curled state measured by the following drawing length measurement method is longer than the length of the above-mentioned fiber bundle in the curled state by more than 0.1 mm.
[0016] Method for measuring drawing length:
[0017] The crimped fiber bundle is placed on a flat surface.
[0018] Observe the curled fiber bundle after standing still from above, trace along the curled fiber bundle from one end to the other end of the curled fiber bundle, and define the traced distance as the "tracing length of the curled fiber bundle."
[0019] The papermaking mat of the present invention comprises a fiber bundle having a predetermined size.
[0020] This fiber bundle is formed in a manner that 10 or more inorganic fibers are interwoven in a twisted manner and have a predetermined length and width, and support each other, so that it is not deformed by pressure. Therefore, when pressure is applied to the paper-made mat, the fiber bundle acts as a core material and can alleviate the pressure on the inorganic fibers that do not constitute the fiber bundle. Therefore, it is possible to prevent the inorganic fibers that do not constitute the fiber bundle from breaking due to pressure. As a result, the surface pressure of the paper-made mat of the present invention increases.
[0021] The paper mat of the present invention includes a crimped fiber bundle, wherein the drawn length of the crimped fiber bundle measured by the drawn length measuring method is 0.1 mm or more longer than the length of the crimped fiber bundle.
[0022] The fiber bundle in a crimped state has elasticity, and the surface pressure of a papermaking mat including such a fiber bundle becomes high.
[0023] The paper-made mat of the present invention preferably contains 0.1 to 20 parts by weight of an organic binder and 0.1 to 10 parts by weight of an inorganic binder based on 100 parts by weight of the inorganic fibers.
[0024] The organic binder and the inorganic binder bond the inorganic fibers to each other and maintain the shape of the paper-made mat.
[0025] When the content of the organic binder and the inorganic binder is within the above range, the inorganic fibers are appropriately bonded to each other, and both the flexibility and the shape retention of the paper-made mat can be achieved.
[0026] In addition, it is possible to suppress the inorganic fibers from falling off and scattering from the papermaking mat.
[0027] In the papermaking mat of the present invention, the glass transition temperature Tg of the organic binder is preferably 5° C. or less.
[0028] When the glass transition temperature Tg of the organic binder is 5° C. or less, the strength of the organic binder film formed by the organic binder can be increased, and the film elongation can be high and the resulting papermaking mat can have excellent flexibility.
[0029] In the papermaking mat of the present invention, the organic binder is preferably at least one selected from the group consisting of acrylic resins, acrylate latexes, rubber latexes, carboxymethyl cellulose and polyvinyl alcohol functioning as water-soluble organic polymers, styrene resins functioning as thermoplastic resins, and epoxy resins functioning as thermosetting resins.
[0030] In the papermaking mat of the present invention, the inorganic binder preferably includes at least one of alumina, silica, silicon carbide, zirconium oxide, boron nitride, diamond and pumice.
[0031] These organic binders and inorganic binders are suitable for bonding the inorganic fibers to each other and maintaining the shape of the paper-made mat.
[0032] In the paper-made mat of the present invention, the fiber bundle may include a straight fiber bundle.
[0033] The straight fiber bundle can be obtained by opening the first inorganic fiber molded body derived from the needle punched mat and the second inorganic fiber molded body derived from the papermaking mat in water.
[0034] The method for producing a paper-made mat of the present invention is a method for producing a mat comprising the following steps: a fiber-opening step of fiber-opening an inorganic fiber molded body in water to produce a slurry containing the fiber-opened inorganic fibers; and a paper-making step of paper-making the slurry to produce a paper-made mat, wherein the fiber-opening step is performed in such a manner that the slurry contains fiber bundles having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, which are formed by interweaving more than 10 inorganic fibers in a twisted manner, and the inorganic fibers that do not constitute the fiber bundles.
[0035] In the method for producing a paper-made mat of the present invention, an inorganic fiber molded body is opened in water, and the obtained inorganic fibers are paper-made.
[0036] When the inorganic fiber molded body is opened, the inorganic fibers may not be completely opened, and a fiber bundle in which a plurality of fibers are twisted and intertwined may be generated.
[0037] In the method for producing a paper mat of the present invention, such a fiber bundle is intentionally generated.
[0038] It should be noted that the number of inorganic fibers intertwined in a twisted manner in the fiber bundle, the average length of the fiber bundle, and the average width of the fiber bundle can be adjusted by adjusting the fiber-opening conditions.
[0039] The surface pressure of the paper mat produced by this method is increased.
[0040] In the method for producing a paper-made mat of the present invention, the inorganic fiber molded body preferably includes a first inorganic fiber molded body derived from a needle-punched mat and / or a second inorganic fiber molded body derived from a paper-made mat.
[0041] Regardless of whether the inorganic fiber molded body is derived from a needle punched mat or a paper-made mat, it is possible to form a fiber bundle in the fiber opening step.
[0042] Effects of the Invention
[0043] According to the present invention, a papermaking mat having a sufficiently high surface pressure can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1A This is a perspective view schematically showing an example of the papermaking mat of the present invention.
[0045] Figure 1B yes Figure 1A An enlarged view of the dotted line portion.
[0046] Figure 2 This is a schematic diagram of an example of a crimped fiber bundle included in the papermaking mat of the present invention.
[0047] Figure 3This is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention.
[0048] Figure 4A This is a photograph of one straight fiber bundle included in the papermaking mat of Example 1.
[0049] Figure 4B The diagram shows Figure 4A Photographs showing the orientation of the fiber bundles.
[0050] Figure 5A This is a photograph of one fiber bundle contained in the papermaking mat of Example 1 in a crimped state.
[0051] Figure 5B The diagram shows Figure 5A Photographs showing the orientation of the fiber bundles. DETAILED DESCRIPTION
[0052] The following is a detailed description of the paper-made mat of the present invention. However, the present invention is not limited to the following configurations, and can be appropriately changed and applied without changing the gist of the present invention. It should be noted that a configuration obtained by combining two or more of the preferred configurations of the present invention described below is also the present invention.
[0053] The copy mat of the present invention will be described with reference to the drawings.
[0054] Figure 1A This is a perspective view schematically showing an example of the papermaking mat of the present invention.
[0055] Figure 1B yes Figure 1A An enlarged view of the dotted line portion.
[0056] like Figure 1A As shown, the paper-made mat 10 is a paper-made mat composed of inorganic fibers.
[0057] The copying mat 10 has a rectangular shape in a plan view, with a convex portion 11 a provided at one end portion 11 and a concave portion 12 a provided at the other end portion 12 .
[0058] As will be described in detail later, the papermaking mat 10 is wound around an exhaust gas treating body and is disposed in an exhaust gas purifying device.
[0059] The convex portion 11a and the concave portion 12a are shaped so as to fit in with each other when the papermaking mat 10 is wound around an exhaust gas treating body.
[0060] If such convex portions 11 a and concave portions 12 a are provided, the sealing property is improved when the papermaking mat 10 is disposed in an exhaust gas purifying device described later.
[0061] It should be noted that the papermaking mat of the present invention may not have convex portions and concave portions at the end portions.
[0062] like Figure 1B As shown, the paper-made mat 10 includes a fiber bundle 21 in which ten or more inorganic fibers 20 are intertwined and twisted, and inorganic fibers 22 that do not constitute the fiber bundle 21 .
[0063] The fiber bundle 21 includes a straight state ( Figure 1B , the state represented by symbol "21a"), the curled state ( Figure 1B , the state represented by symbol "21b").
[0064] In addition, in the paper-made mat 10, the fiber bundle 21 includes the fiber bundle 21b in a crimped state as an essential component.
[0065] It should be noted that, in this specification, "straight state" refers to the direction of the fiber bundle ( Figure 1B , the direction indicated by arrow D1) is a straight line.
[0066] In addition, in this specification, "crimped state" refers to the direction of the fiber bundle ( Figure 1B , a state in which the device is bent at least once in the direction indicated by arrow D2.
[0067] The average length of the fiber bundle 21 ( Figure 1B The average length of the fiber bundle 21 is preferably 7 to 13 mm, more preferably 8 to 10 mm.
[0068] The average width of the fiber bundle 21 ( Figure 1B The average value of the length represented by the symbol W is 0.2 to 1.0 mm. In addition, the average width of the fiber bundle 21 is preferably 0.2 to 0.8 mm.
[0069] It should be noted that if Figure 1B As shown, in the case where the fiber bundle 21 is a straight fiber bundle 21a and in the case where the fiber bundle 21 is a crimped fiber bundle 21b, the maximum width ( Figure 1B , the lengths represented by symbols Wa and Wb respectively are the widths of the fiber bundle 21.
[0070] The fiber bundle 21 is formed by interweaving 10 or more inorganic fibers 20 in a twisted manner, and supports each other, so it is not easy to be deformed by pressure. Therefore, when pressure is applied to the papermaking mat 10, the fiber bundle 21 acts as a core material, and the pressure on the inorganic fibers 22 that do not constitute the fiber bundle 21 can be alleviated. Therefore, the inorganic fibers 22 that do not constitute the fiber bundle 21 can be prevented from being broken by pressure. As a result, the surface pressure of the papermaking mat 10 increases.
[0071] In particular, when the fiber bundle 21 is the fiber bundle 21b in a crimped state, this effect is appropriately exerted, and the surface pressure of the papermaking mat 10 is further increased.
[0072] If the average length of the fiber bundle is less than 5 mm, the fiber bundle is too short and it is difficult for the fiber bundle to relieve pressure applied to the inorganic fibers that do not constitute the fiber bundle as a core material.
[0073] If the average length of the fiber bundle exceeds 15 mm, the fiber bundle is too long and is easily bent when the side surface of the fiber bundle is pressed, making it difficult for the fiber bundle to function as a core material.
[0074] When the average width of the fiber bundle is less than 0.2 mm, the strength of the fiber bundle decreases, the fiber bundle is easily bent, and it is difficult for the fiber bundle to function as a core material.
[0075] When the average width of the fiber bundle exceeds 1.0 mm, the strength of the fiber bundle becomes too high, and the flexibility of the entire paper-made mat decreases.
[0076] In addition, in this specification, "fiber bundle" means the part where inorganic fibers are concentrated in the papermaking mat and the density is higher than other parts.
[0077] In this specification, "a fiber bundle in which inorganic fibers are intertwined in a twisted manner" means the following fiber bundle.
[0078] The paper-made mat of the present invention is produced using inorganic fibers obtained by fibrillating a needle punched mat or a paper-made mat as a material, and the details will be described later.
[0079] When the needle punched mat or paper-made mat is opened, the inorganic fibers may not be completely opened, and a fiber bundle in which a plurality of fibers are twisted and intertwined may be generated.
[0080] That is, when the needle punch mat is produced, the inorganic fibers are intertwined with each other by needles, so that the inorganic fibers are strongly intertwined with each other in this portion.
[0081] In addition, when making a paper-made mat, inorganic fibers are bonded to each other with an organic binder, so that inorganic fibers are difficult to separate from each other. When making a paper-made mat by a paper-making method, the aggregation of inorganic fibers is uneven, and a high-density inorganic fiber aggregation is formed.
[0082] The portion where inorganic fibers are intertwined with needles in the needle punched mat and the aggregated portion of dense inorganic fibers in the papermaking mat are not easily opened and remain as twisted intertwined fiber bundles.
[0083] In this way, the fiber bundles remaining when the needle punched mat and the paper-made mat are opened are "fiber bundles formed by intertwining the inorganic fibers in a twisted manner" in this specification.
[0084] The papermaking mat of the present invention includes fiber bundles in which the inorganic fibers are twisted and intertwined.
[0085] The average length of the fiber bundle and the average width of the fiber bundle are values measured as follows.
[0086] Cut 150cm from the paper mat 3 of the test piece.
[0087] Thereafter, the test piece was fired at 600° C. for 1 hour to thermally decompose the binder component.
[0088] Next, the test piece is placed in a container, and the container is vibrated up and down and left and right to disentangle the inorganic fibers constituting the test piece.
[0089] The fiber bundle was taken out from the untied test piece, and the length and width of the fiber bundle were measured.
[0090] The same operation was repeated three times, and the average values of the length and width of the obtained fiber bundle were calculated.
[0091] In addition, when calculating the average length and average width of the fiber bundle, the calculation was performed excluding the fiber bundle consisting of less than 10 inorganic fibers.
[0092] It should be noted that the mat material of the present invention may contain fiber bundles with an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, and may contain fiber bundles with a length of less than 5 mm, fiber bundles with a length of more than 15 mm, fiber bundles with a width of less than 0.2 mm, and fiber bundles with a width of more than 1.0 mm.
[0093] As described above, the papermaking mat 10 includes the crimped fiber bundle 21b as an essential component.
[0094] The fiber bundle 21b in the crimped state will be described in detail below using the drawings.
[0095] Figure 2 This is a schematic diagram of an example of a crimped fiber bundle included in the papermaking mat of the present invention.
[0096] exist Figure 2 In the crimped fiber bundle 21b shown in FIG. 1 , it is preferable that the drawing length L of the crimped fiber bundle 21b measured by the following drawing length measuring method is t It is longer than the length L of the fiber bundle 21b in the crimped state, more preferably 0.1 mm or more longer, and further preferably 0.2 to 0.6 mm longer.
[0097] (Method for measuring drawing length)
[0098] The crimped fiber bundle 21b is placed still on a flat surface.
[0099] Next, the crimped fiber bundle 21b after being left to stand is observed from above, and a line is drawn along the crimped fiber bundle 21b from one end P1 to the other end P2 of the crimped fiber bundle 21b, and the drawn distance L is t As "the drawing length of the fiber bundle in the crimped state".
[0100] When the drawing length L of the fiber bundle 21b in the crimped state t When it is longer than the length L of the crimped fiber bundle 21b, the elasticity of the crimped fiber bundle 21b becomes higher, and the surface pressure of the papermaking mat 10 increases.
[0101] The papermaking mat 10 preferably includes the following crimped fiber bundles 21b: Figure 2 In the crimped fiber bundle 21b shown, when measuring the “drawing length of the crimped fiber bundle”, the crimped fiber bundle 21b can be drawn by crossing the line segment S connecting the end P1 and the end P2 two or more times.
[0102] The degree of crimping of the fiber bundle 21b in such a crimped state is appropriate, the elasticity of the fiber bundle 21b in the crimped state is increased, and the surface pressure of the papermaking mat 10 is increased.
[0103] In the papermaking mat 10, it is preferable that the drawing length L of the crimped fiber bundle 21b is t The ratio of the length L of the fiber bundle 21b in the crimped state is L t / L=1.1~1.6.
[0104] In the paper-made mat 10, the value of the following formula (1) is preferably 0.1 or more, and more preferably 0.2 to 0.6.
[0105] (L t -L) / Wb...(1)
[0106] In the paper-made mat 10, the crimped fiber bundle 21b is placed on a flat surface, and the area of the crimped fiber bundle 21b viewed from above is preferably 2.6 to 8.3 mm. 2 .
[0107] In the papermaking mat 10, the ratio of the number of the crimped fiber bundles 21b contained in the fiber bundles 21 is preferably 85% or less, more preferably 60% or less, further preferably 30% or less, and further preferably 10% to 30%.
[0108] The inorganic fibers 20 constituting the papermaking mat 10 preferably include at least one selected from the group consisting of alumina fibers, silica fibers, alumina-silica fibers, mullite fibers, glass fibers, and biosoluble fibers.
[0109] When the papermaking mat 10 is composed of these inorganic fibers, the heat resistance is sufficient.
[0110] The inorganic fibers 20 constituting the paper-made mat 10 preferably have an average fiber diameter of 2 to 10 μm and an average fiber length of 0.01 to 5.0 mm.
[0111] The bulk density of the sheet mat 10 is preferably 0.05 to 0.30 g / cm 3 .
[0112] If the bulk density of the sheet mat 10 is less than 0.05 g / cm 3 , the inorganic fibers are weakly entangled with each other, and the inorganic fibers are easily peeled off, so it is difficult to maintain the shape of the papermaking mat in a predetermined shape.
[0113] If the bulk density of the sheet mat 10 exceeds 0.30 g / cm 3 , the papermaking mat becomes hard, the windability is reduced, and the mat is prone to rupture.
[0114] The paper-made mat 10 preferably contains 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, of an organic binder based on 100 parts by weight of the inorganic fibers 20 .
[0115] The inorganic binder is preferably contained in an amount of 0.1 to 10 parts by weight, more preferably 0.5 to 3.0 parts by weight, based on 100 parts by weight of the inorganic fibers 20 .
[0116] The organic binder and the inorganic binder bond the inorganic fibers to each other and maintain the shape of the paper-made mat.
[0117] When the content of the organic binder and the inorganic binder is within the above range, the inorganic fibers are appropriately bonded to each other, and both the flexibility and the shape retention of the paper-made mat can be achieved.
[0118] In addition, it is possible to suppress the inorganic fibers from falling off and scattering from the papermaking mat.
[0119] In the papermaking mat 10, the glass transition temperature Tg of the organic binder is preferably 5°C or less, more preferably -35 to 5°C.
[0120] When the glass transition temperature Tg of the organic binder is 5° C. or less, the strength of the organic binder film formed by the organic binder can be increased, and the film elongation can be high and the resulting papermaking mat can have excellent flexibility.
[0121] In addition, the mat 10 is less likely to break when it is wound around an exhaust gas treatment body, etc. In addition, since the organic binder film does not become too hard, it can connect the inorganic fibers to each other when the inorganic fibers break, and can suppress the scattering of the inorganic fibers.
[0122] When the glass transition temperature Tg of the organic binder exceeds 5° C., the flexibility of the papermaking mat may decrease and the elongation at break may decrease.
[0123] In the papermaking mat of the present invention, the organic binder may be a water-soluble organic polymer, a thermoplastic resin, or a thermosetting resin.
[0124] Examples of water-soluble organic polymers include acrylic resins, acrylate latex, rubber latex, carboxymethyl cellulose, and polyvinyl alcohol. Examples of thermoplastic resins include styrene resins. Examples of epoxy resins that function as thermosetting resins include.
[0125] In the copy mat 10 , the inorganic binder preferably contains at least one of alumina, silica, silicon carbide, zirconium oxide, boron nitride, diamond, and pumice.
[0126] These organic binders and inorganic binders are suitable for bonding the inorganic fibers to each other and maintaining the shape of the paper-made mat.
[0127] Next, the method for producing the papermaking mat of the present invention will be described.
[0128] The method for producing a paper-made mat of the present invention comprises (1) a fiber-opening step and (2) a paper-making step.
[0129] It should be noted that in the following description, the case of using both the first inorganic fiber molded body from the needle-punched mat and the second inorganic fiber molded body from the paper-made mat as the inorganic fiber molded body is described, but in the method for manufacturing the paper-made mat of the present invention, any inorganic fiber molded body can be used.
[0130] Each step is described in detail below.
[0131] (1) Fiber opening process
[0132] In this step, the first inorganic fiber molded body derived from the needle punched mat and the second inorganic fiber molded body derived from the papermaking mat are opened in water to prepare a slurry containing the opened inorganic fibers.
[0133] In this step, the slurry is opened so that fiber bundles having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm formed by entanglement of 10 or more of the inorganic fibers twisted together and the inorganic fibers not forming a fiber bundle are included.
[0134] It should be noted that in this step, dry fiber opening is preferably not performed.
[0135] When the needle punched mat or paper-made mat is opened, the inorganic fibers may not be completely opened, and a fiber bundle in which a plurality of fibers are twisted and intertwined may be generated.
[0136] More specifically, it is as follows.
[0137] When the needle punch mat is produced, the inorganic fibers are intertwined with each other by needles, so that the inorganic fibers are strongly intertwined with each other in this portion.
[0138] In addition, when making a paper-made mat, inorganic fibers are bonded to each other with an organic binder, so that inorganic fibers are difficult to separate from each other. When making a paper-made mat by a paper-making method, the aggregation of inorganic fibers is uneven, and a high-density inorganic fiber aggregation is formed.
[0139] The portion where inorganic fibers are intertwined with needles in the needle punched mat and the aggregated portion of dense inorganic fibers in the papermaking mat are not easily opened and remain as twisted intertwined fiber bundles.
[0140] In the method for producing a paper mat of the present invention, such a fiber bundle is intentionally generated.
[0141] It should be noted that the number of inorganic fibers intertwined in a twisted manner in the fiber bundle, the average length of the fiber bundle, and the average width of the fiber bundle can be adjusted by adjusting the fiber-opening conditions.
[0142] The fiber opening conditions are not particularly limited. For example, when fiber opening is performed using a stirrer in water, the number of inorganic fibers intertwined in a twisted manner in the fiber bundle, the average length of the fiber bundle, and the average width of the fiber bundle can be adjusted by adjusting the rotation speed and time of the stirrer.
[0143] It should be noted that when dry fiber opening is performed in this step, the inorganic fibers are easily broken and the length of the fiber bundle becomes shorter. As a result, the length of the obtained fiber bundle becomes shorter and a fiber bundle having a desired shape cannot be obtained.
[0144] Therefore, in this step, it is preferred not to perform dry fiber opening.
[0145] In addition, the fiber bundle produced in this step may be derived from the first inorganic fiber molded body or the second inorganic fiber molded body.
[0146] Regardless of whether the inorganic fiber molded body is derived from the first inorganic fiber molded body (derived from the needle punched mat) or the second inorganic fiber molded body (derived from the papermaking mat), a fiber bundle can be formed in the fiber opening step.
[0147] As an example of fiber opening, for example, the following method can be cited.
[0148] First, the first inorganic fiber molded body and the second inorganic fiber molded body are fired at 700 to 1000°C for 1.0 to 8.0 hours. The preferred firing temperature is 800 to 950°C.
[0149] This makes it possible to thermally decompose the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body, and to easily open the first inorganic fiber molded body and the second inorganic fiber molded body.
[0150] Next, the fired first inorganic fiber molded body and the second inorganic fiber molded body are left to stand until they reach room temperature, and then the first inorganic fiber molded body and the second inorganic fiber molded body are untied by hand.
[0151] Next, the first inorganic fiber molded body and the second inorganic fiber molded body are added to water in an amount of 50 to 400 times by weight, and stirred to open the fibers, thereby preparing a slurry containing inorganic fibers. The weight ratio is preferably 100 to 200 times.
[0152] In addition, the stirring conditions are preferably set appropriately. For example, when making 10L of slurry, it is preferred to use (product name: SMT-101, manufacturer: AS ONE) as a stirrer, and stir at a rotation speed of 500 to 1000 rpm and a stirring time of 200 to 900 seconds. Preferably, the rotation speed is 650 to 850 rpm and the stirring time is 500 to 700 seconds, and more preferably the rotation speed is 700 to 800 rpm and the stirring time is 500 to 650 seconds.
[0153] In this case, when the slurry is dried, it is opened so as to form a fiber bundle having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm in which 10 or more inorganic fibers are intertwined in a twisted manner.
[0154] Next, an organic binder and an inorganic binder are added to the slurry.
[0155] The organic binder is preferably added in an amount of 0.1 to 20 parts by weight, more preferably 0.5 to 15.0 parts by weight, based on 100 parts by weight of the inorganic fibers in the produced papermaking mat.
[0156] The inorganic binder is preferably added in an amount of 0.1 to 15.0 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the inorganic fibers in the produced papermaking mat.
[0157] The types of preferred organic binders and inorganic binders have already been described, and thus their description is omitted here.
[0158] (2) Copying process
[0159] Next, the slurry is poured into a molding machine having a filter net formed on the bottom surface, and the solvent in the slurry is removed to obtain an inorganic fiber aggregate. Then, the inorganic fiber aggregate is dehydrated and dried to obtain the papermaking mat of the present invention.
[0160] It should be noted that in the papermaking process, the inorganic fiber aggregate may be dried by heating and pressurizing. During heating and pressurizing, the inorganic fiber aggregate may be heat-treated by blowing hot air through it to dry it, or it may be kept wet without heat treatment.
[0161] When heat treatment is performed, the heating temperature or hot air temperature is preferably 150 to 210° C. in order to prevent the organic binder from being deteriorated by heat.
[0162] In the range of 150-210°C, the deterioration of the organic binder can be suppressed, and at the same time, the moisture can be dispersed from the inorganic fiber aggregate. When the heating temperature and the hot air temperature are less than 150°C, the temperature is not transmitted to the central part of the inorganic fiber aggregate, and the drying time becomes longer. In addition, if it exceeds 210°C, the organic binder is deteriorated, and the restraint force between the fibers is reduced, so the thickness of the inorganic fiber aggregate becomes difficult to control.
[0163] In the method for producing a paper-made mat of the present invention, it is preferred that batch paper-making or continuous paper-making be performed in the paper-making step.
[0164] The paper-made mat of the present invention can be easily obtained by batch paper-making or continuous paper-making.
[0165] It should be noted that a paper-made mat according to one embodiment of the present invention is produced through a fiber-opening process and a paper-making process, wherein the fiber-opening process is a process of fiber-opening an inorganic fiber molded body in water and producing a slurry containing the fiber-opened inorganic fibers, and the paper-making process is a process of paper-making the slurry to produce a paper-made mat, wherein in the fiber-opening process, the slurry is fiber-opened so that the slurry contains fiber bundles with an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm formed by interweaving more than 10 of the above-mentioned inorganic fibers in a twisted manner, and the above-mentioned inorganic fibers that do not constitute the above-mentioned fiber bundles.
[0166] It should be noted that in the above-mentioned fiber opening step, it is preferred that the slurry contains a crimped fiber bundle, and the drawn length of the crimped fiber bundle measured by the above-mentioned drawn length measuring method is longer than the length of the crimped fiber bundle by 0.1 mm or more.
[0167] Next, a method of using the papermaking mat of the present invention will be described.
[0168] Figure 3 This is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention.
[0169] like Figure 3 As shown, the exhaust gas purification device 100 includes a metal casing 30, an exhaust gas treatment body 40 accommodated in the metal casing 30, and a papermaking mat 10 disposed between the exhaust gas treatment body 40 and the metal casing 30. The papermaking mat 10 is the papermaking mat of the present invention.
[0170] The exhaust gas treatment body 40 is a columnar body having a plurality of cells 41 arranged in parallel along the length direction with a groove wall 42 therebetween. It should be noted that, at the end of the metal shell 30, an inlet pipe for introducing exhaust gas discharged from the internal combustion engine and an exhaust pipe for discharging the exhaust gas after passing through the exhaust gas purification device to the outside are connected as needed.
[0171] exist Figure 3 In the exhaust gas purification device 100 shown, an exhaust gas filter (honeycomb filter) in which any end of each groove is sealed with a sealing material 43 is used as the exhaust gas treatment body 40, but a catalyst carrier in which any end surface is not sealed with a sealing material may also be used.
[0172] like Figure 3 As shown, the exhaust gas ( Figure 3 In the figure, G represents exhaust gas and arrows represent the flow of exhaust gas) flows into a groove 41 opened at the exhaust gas inlet side end surface 40a of the exhaust gas treatment body (honeycomb filter) 40, and passes through the groove wall 42 separating the groove 41. At this time, PM in the exhaust gas is captured by the groove wall 42, and the exhaust gas is purified. The purified exhaust gas flows out from the other grooves 41 opened at the exhaust gas outlet side end surface 40b and is discharged to the outside.
[0173] As described above, the surface pressure of the papermaking mat 10 is high. Therefore, in the exhaust gas purifying device 100, even if the exhaust gas treating body 40 is subjected to high pressure from the exhaust gas, it is possible to prevent the exhaust gas treating body 40 from falling off from the metal casing 30.
[0174] The exhaust gas treating body 40 may be made of non-oxidizing porous ceramics such as silicon carbide and silicon nitride, or may be made of oxidizing porous ceramics such as sialon, alumina, cordierite, and mullite. Among them, silicon carbide is preferred.
[0175] When the exhaust gas treating body 40 is a silicon carbide porous ceramic, the porosity of the porous ceramic is not particularly limited, but is preferably 35 to 60%.
[0176] If the porosity is less than 35%, the exhaust gas treatment body may be immediately clogged. On the other hand, if the porosity exceeds 60%, the strength of the exhaust gas treatment body decreases and the exhaust gas treatment body may be easily broken.
[0177] In addition, the average pore diameter of the porous ceramic is preferably 5 to 30 μm.
[0178] When the average pore size is less than 5 μm, PM may easily cause clogging.
[0179] If the average pore size exceeds 30 μm, PM may pass through the pores, making it impossible to capture PM and thus failing to function as a filter.
[0180] In addition, the said porosity and pore diameter can be measured by the conventionally well-known method, such as measurement using a scanning electron microscope (SEM).
[0181] The groove density in the cross section of the exhaust gas treatment body 40 is not particularly limited, but the preferred lower limit is 31.0 grooves / cm 2 (200 pcs / inch 2 ), the preferred upper limit is 93.0 pcs / cm 2 (600 pcs / inch 2 ). In addition, the more preferred lower limit is 38.8 pieces / cm 2 (250pcs / inch 2 ), and the more preferred upper limit is 77.5 pieces / cm 2 (500 pcs / inch 2 ).
[0182] The exhaust gas treatment body 40 may also be loaded with a catalyst for purifying the exhaust gas. As the loaded catalyst, a noble metal such as platinum, palladium, or rhodium is preferred, and platinum is more preferred. In addition, as other catalysts, alkali metals such as potassium and sodium, and alkaline earth metals such as barium may also be used. These catalysts may be used alone or in combination of two or more.
[0183] If these catalysts are loaded, PM can be easily burned and removed, and toxic exhaust gas can also be purified.
[0184] (Metal Housing)
[0185] The metal housing 30 is approximately cylindrical.
[0186] The inner diameter of the metal casing 30 (the inner diameter of the portion accommodating the exhaust gas treating body) is preferably slightly shorter than the diameter of the exhaust gas treating body 40 around which the papermaking mat 10 is wound.
[0187] The metal case 30 is not particularly limited, but is preferably made of stainless steel.
[0188] Example
[0189] The following are examples that more specifically disclose the present invention, but it should be noted that the present invention is not limited to these examples.
[0190] (Example 1)
[0191] A first inorganic fiber molded body was prepared from a needle-punched mat, which was composed of alumina-silica fibers with a weight ratio of Al2O3:SiO2=72:28 and a bulk density of 0.17 g / cm 3 , the density of stitches is 21 / cm 2 density.
[0192] In addition, a second inorganic fiber molded body was prepared from the papermaking mat, which was composed of alumina-silica fibers with Al2O3:SiO2=72:28 (weight ratio) and a bulk density of 0.12 g / cm 3 .
[0193] Next, the first inorganic fiber molded body and the second inorganic fiber molded body were fired at 800° C. for 1 hour to thermally decompose the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body.
[0194] Next, the fired first inorganic fiber molded body and the second inorganic fiber molded body are left to stand until they reach room temperature, and then the first inorganic fiber molded body and the second inorganic fiber molded body are untied by hand.
[0195] Next, 5.0 g of the first inorganic fiber molded body and 5.0 g of the second inorganic fiber molded body were taken out and added to 0.4 L of water. Thereafter, the mixture was stirred at a rotation speed of 1000 rpm and a stirring time of 10 minutes using a stirrer (product name: SMT-101, manufacturer: AS ONE) to open the fibers, thereby preparing an inorganic fiber slurry.
[0196] In order to confirm whether a fiber bundle was formed in the slurry, a part of the slurry was taken out and dried. As a result, it was confirmed that a fiber bundle was formed in which 10 or more inorganic fibers were twisted together.
[0197] Next, an organic binder is added to the slurry in an amount of 0.5 to 10 parts by weight based on 100 parts by weight of the inorganic fibers.
[0198] Furthermore, an inorganic binder is added to the slurry in an amount of 0.5 to 3.0 parts by weight based on 100 parts by weight of the inorganic fibers.
[0199] Next, the slurry was poured into a molding machine having a filter mesh formed on the bottom surface, and the solvent in the slurry was desolvated to obtain an inorganic fiber aggregate. Thereafter, the inorganic fiber aggregate was dehydrated and dried at 150 to 210° C. for 5 minutes to 1 hour to produce the paper-made mat of Example 1.
[0200] (Observation of fiber bundles 1)
[0201] 150 cm thick pieces were cut from the sheet mat prepared in Example 1.3 of the test piece.
[0202] Then, the test piece was fired at 600° C. for 1 hour to thermally decompose the binder component.
[0203] Next, the test piece is placed in a container, and the container is vibrated up and down and left and right to disentangle the inorganic fibers constituting the test piece.
[0204] Fiber bundles were randomly taken out from the untied test piece, and the length and width of the fiber bundles were measured.
[0205] The same operation was repeated three times, and the average values of the fiber bundle length and the fiber bundle width were calculated.
[0206] As a result, the average length of the fiber bundle was 8 mm, and the average width of the fiber bundle was 0.393 mm.
[0207] In addition, a photograph of the fiber bundle contained in the sheet-made mat of Example 1 is shown in Figure 4A and Figure 5A In addition, the direction of each fiber bundle is shown in Figure 4B and Figure 5B .
[0208] Figure 4A This is a photograph of a straight fiber bundle included in the papermaking mat of Example 1.
[0209] Figure 4B The diagram shows Figure 4A Photographs showing the orientation of the fiber bundles.
[0210] Figure 5A This is a photograph of the crimped fiber bundle contained in the papermaking mat of Example 1.
[0211] Figure 5B The diagram shows Figure 5A Photographs showing the orientation of the fiber bundles.
[0212] Figure 4B The fiber bundle is shown in a straight state, and the direction of the fiber bundle is along the arrow D1.
[0213] Figure 5B The fiber bundle is shown in a crimped state, with the direction of the fiber bundle being along arrow D2.
[0214] (Example 2) and (Comparative Example 1) and (Comparative Example 2))
[0215] When each inorganic fiber molded body was opened with a mixer to prepare an inorganic fiber slurry, the stirring time was changed and the average length of the fiber bundles contained in the manufactured paper mat was adjusted to the length shown in Table 1. The paper mats of Example 2 and Comparative Examples 1 and 2 were manufactured in the same manner as Example 1.
[0216] [Table 1]
[0217] Average length of fiber bundle (mm) Surface pressure(kPa) Comparative Example 1 4 88.6 Example 1 8 97.0 Example 2 10 104.8 Comparative Example 2 18 92.2 Comparative Example 3 20 87.4
[0218] (Comparative Example 3)
[0219] The alkaline aluminum chloride aqueous solution was mixed with silica sol so that the composition ratio of the inorganic fibers after firing was Al2O3:SiO2=72:28 (weight ratio), and an appropriate amount of an organic polymer (polyvinyl alcohol) was added to prepare a mixed solution.
[0220] The obtained mixed solution was concentrated to form a spinning mixture, and the spinning mixture was spun by a spray spinning method (spinning atmosphere temperature: 120° C.) to produce an alumina fiber precursor.
[0221] Next, the obtained inorganic fiber precursor is compressed to produce a continuous sheet, and then the sheet is placed in a heating furnace and fired to produce an inorganic fiber aggregate.
[0222] Next, the inorganic fiber aggregate was opened by stirring using a stirrer (product name: SMT-101, manufacturer: AS ONE Co., Ltd.) at a rotation speed of 1000 rpm and a stirring time of 10 minutes.
[0223] In order to confirm whether or not a fiber bundle was formed in the slurry, a portion of the slurry was taken out and dried. As a result, it was confirmed that a fiber bundle was formed, but the fiber bundle was not twisted.
[0224] Next, the slurry was poured into a molding machine having a filter mesh formed on the bottom surface, and the solvent in the slurry was desolvated to obtain an inorganic fiber aggregate. Thereafter, the inorganic fiber aggregate was dehydrated and dried at 150 to 210° C. for 5 minutes to 1 hour to produce a paper-made mat of Comparative Example 3.
[0225] The sheet mat of Comparative Example 3 was observed in the same manner as in the above "(Observation of Fiber Bundles 1)". The mat contained untwisted fiber bundles, and the average length of the fiber bundles was 20 mm and the average width of the fiber bundles was 0.37 mm.
[0226] (Measurement of surface pressure)
[0227] The sheet mats of Examples 1 and 2 and Comparative Examples 1 to 3 were placed in a testing machine (product name: SMT-101, manufacturer: ASONE Co., Ltd.) and compressed at a rate of 25.4 mm / min until the gap bulk density (GBD) was 0.40 mm. 3 / g. With a void bulk density (GBD) of 0.40mm 3 The / g state is maintained for 10 minutes.
[0228] Thereafter, the surface pressure of each paper-made mat was measured. The results are shown in Table 1.
[0229] As shown in Table 1, it is clear that the surface pressure of the paper-made mat of each example is high.
[0230] (Comparative Example 4)
[0231] In an alkaline aluminum chloride aqueous solution with an aluminum content of 70 g / l and Al / Cl=1.8 (atomic ratio), a silica sol is mixed in such a way that the composition of the alumina fiber is Al2O3:SiO2=72:28, thereby forming a precursor of the alumina fiber. Next, an organic polymer such as polyvinyl alcohol is added to the precursor of the alumina fiber. Furthermore, the liquid is concentrated to form a spinning solution, and the spinning solution is used to perform spinning by a blowing method. Then, the material obtained by folding the precursor of the alumina fiber is layered to produce a layered sheet of the alumina fiber. Next, the layered sheet is subjected to a needle punching treatment. 50 pieces / 100 cm 2 Two sets of needle plates with needles are arranged on the front and back sides of the laminated sheet, and needle punching is performed from both sides of the laminated sheet. 2 The density of the interlaced dots on the left and right is a laminated sheet.
[0232] Then, the obtained laminated sheet was continuously fired from room temperature to a maximum temperature of 1250° C. to obtain a needle-punched sheet having a thickness of about 7 mm.
[0233] Next, the needle punched sheet was roughly cut into a size of 200 mm×200 mm or less, and then placed in a feather mill (FM-1, manufactured by Hosokawa Micron Co., Ltd.) for dry fiber opening to obtain cotton-like fiber having a diameter of about 150 mm.
[0234] Next, in order to prepare the raw material slurry, 1200 g of the obtained opened fiber and 120,000 g of water were placed in a stirrer and stirred for 1 minute. Next, 60 g of an organic binder (latex) was added to the solution and further stirred for 1 minute. Next, 12 g of an inorganic binder (alumina sol) was added to the solution and further stirred for 1 minute. Finally, 6 g of a coagulant (Percol 292) was added and stirred for 1 minute to obtain a raw material slurry.
[0235] Next, in order to form a molded body, the raw material slurry prepared in this way was transferred to a molding machine having a length of 930 mm, a width of 515 mm, and a depth of 400 mm and a metal mesh (30 mesh) for filtering at the bottom, and dehydrated. The dehydration was performed by forcibly sucking the water of the raw material slurry from the bottom side of the molding machine through the metal mesh for filtering using a suction pump.
[0236] Next, the molded body was taken out of the molding machine and compressed and dried at 120°C and 70 kPa for 30 minutes. 3 The sheet-made mat of Comparative Example 4.
[0237] The sheet mat of Comparative Example 4 was observed in the same manner as in the above "(Observation of Fiber Bundles 1)". The observation revealed that the sheet mat contained untwisted fiber bundles, and the average length of the fiber bundles was 3 mm and the average width of the fiber bundles was 1.43 mm.
[0238] (Observation of fiber bundles 2)
[0239] 150 cm thick pieces were cut out from the paper-made mat of Example 1 and the paper-made mat of Comparative Example 4. 3 of the test piece.
[0240] Then, the test piece was fired at 600° C. for 1 hour to thermally decompose the binder component.
[0241] Next, the test piece is placed in a container, and the container is vibrated up and down and left and right to disentangle the inorganic fibers constituting the test piece.
[0242] Thirteen fiber bundles were randomly taken out from the test piece of the paper-made mat of Example 1, and four fiber bundles were randomly taken out from the test piece of the paper-made mat of Comparative Example 4.
[0243] The fiber bundles taken out from the test piece of the paper-made mat of Example 1 contained 9 fiber bundles in a crimped state and 4 fiber bundles in a straight state.
[0244] The average length L of these crimped fiber bundles is 6.78 mm. The average area is 4.95 mm. 2 .
[0245] The average length L of these straight fiber bundles is 7.97 mm. The average area is 2.83 mm. 2 .
[0246] All the fiber bundles taken out from the test piece of the paper-made mat of Comparative Example 4 were in a straight state.
[0247] The average length L of these straight fiber bundles is 3.23 mm. The average area is 3.41 mm. 2 .
[0248] Each crimped fiber bundle of Example 1 was placed on a flat surface and observed from above to measure the drawn length L of the fiber bundle. t , calculate its average value.
[0249] Then, the length L of the fiber bundle and the drawing length L of the fiber bundle are calculated. t The difference (L t -L) and ratio (L t The results are shown in Table 2.
[0250] [Table 2]
[0251] Fiber bundle shape L(mm) <![CDATA[L t (mm)]]> <![CDATA[L t -L(mm)]]> <![CDATA[L t / L]]> Example 1 Curled state 6.78 7.89 1.11 1.16
[0252] Explanation of symbols
[0253] 10 Copy pad
[0254] 11 One end
[0255] 11a convex part
[0256] 12 The other end
[0257] 12a recess
[0258] 20 Inorganic fiber
[0259] 21 Fiber bundle
[0260] 21a Fiber bundle in a straight state
[0261] 21b Fiber bundle in curled state
[0262] 22Inorganic fibers not forming fiber bundles
[0263] 30 Metal housing
[0264] 40 Exhaust gas treatment body
[0265] 40a Exhaust gas inflow side end
[0266] 40b Exhaust gas discharge side end
[0267] 41 slots
[0268] 42 groove wall
[0269] 43 Sealing material
[0270] 100 Exhaust gas purification device
Claims
1. A papermaking mat, which is a papermaking mat composed of inorganic fibers, It is characterized in that The paper-made mat includes a fiber bundle formed by entwining 10 or more of the inorganic fibers in a twisted manner and the inorganic fibers that do not constitute the fiber bundle. The average length of the fiber bundle is 5 mm to 15 mm. The average width of the fiber bundle is 0.2 mm to 1.0 mm, The fiber bundle includes a fiber bundle in a crimped state, and a drawn length of the fiber bundle in the crimped state measured by the following drawn length measuring method is longer than the length of the fiber bundle in the crimped state by 0.1 mm or more, Method for measuring drawing length: The fiber bundle in a curled state is placed on a flat surface; Observe the curled fiber bundle after standing still from above, trace along the curled fiber bundle from one end to the other end of the curled fiber bundle, and define the traced distance as "the traced length of the curled fiber bundle".
2. The copying mat according to claim 1, in, The organic binder is contained in an amount of 0.1 to 20 parts by weight and the inorganic binder is contained in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the inorganic fibers.
3. The copying mat according to claim 2, in, The glass transition temperature Tg of the organic binder is 5° C. or less.
4. The copying mat according to claim 2 or 3, in, The organic binder is at least one selected from the group consisting of acrylic resin, acrylate latex, rubber latex, carboxymethyl cellulose and polyvinyl alcohol functioning as water-soluble organic polymers, styrene resin functioning as thermoplastic resins, and epoxy resin functioning as thermosetting resins.
5. The copying mat according to any one of claims 2 to 4, in, The inorganic binder includes at least one of alumina, silicon dioxide, silicon carbide, zirconium oxide, boron nitride, diamond and pumice.
6. The copy mat according to any one of claims 1 to 5, in, The fiber bundle includes a straight fiber bundle.
7. A method for making a pad, wherein include: A fiber opening step of opening the inorganic fiber molded body in water to prepare a slurry containing the opened inorganic fibers; and a papermaking step of papermaking the slurry to form a papermaking mat, The method for producing the paper-made mat is characterized in that: In the fiber-opening step, the fiber-opening is performed so that the slurry contains a fiber bundle having an average length of 5 mm to 15 mm and an average width of 0.2 mm to 1.0 mm, which is formed by entwining 10 or more of the inorganic fibers in a twisted manner, and the inorganic fibers that do not constitute the fiber bundle.
8. The method for producing a sheet-made mat according to claim 7, in, The inorganic fiber molded body includes a first inorganic fiber molded body derived from a needle punched mat and / or a second inorganic fiber molded body derived from a papermaking mat.
Citation Information
Patent Citations
Fiber tow crimping device and method for manufacturing crimped fiber tow
CN104968844A
Synthetic fiber, fiber treatment agent, and use thereof
CN112601856A
Leather like sheet-formed material and method for producing the same
JP2007224481A
Sheet member, manufacturing method of the same, and exhaust gas processing device
JP2008082310A
Method and apparatus for detecting width abnormality of crimped fiber bundle
JP2008280637A
Cited By
Pad and method for manufacturing same
CN120083588A
A cast sheet and a method for manufacturing a cast sheet
CN120083588B
Inorganic fiber sheet with shots distributed on the side surface
US12540437B2
Inorganic fiber sheet
US20240175210A1