Wearable sweat integrated sensor based on laser-induced graphene and preparation method thereof

Through the method of laser-induced graphene and laser cutting of microfluidic channels, the problems of high cost and low detection efficiency of existing wearable sweat sensors are solved, low-cost, fast and accurate multi-index detection is achieved, and the manufacturing speed and Detection efficiency.

CN118743547APending Publication Date: 2024-10-08CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410808664.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing wearable sweat sensors are high in cost, complex to produce, and difficult to prepare on a large scale. They are also unable to detect multiple physiological indicators at the same time, which reduces detection efficiency.

Method used

Using the laser-induced graphene preparation method, cyclic voltammetry and galvanostatic deposition were performed on an electrochemical workstation to prepare a multifunctional graphene electrode, which was then combined with a polyethylene terephthalate film for laser cutting to prepare microfluidics. Control channel layer to realize the manufacturing of sweat integrated sensor.

Benefits of technology

It achieves low-cost, fast and accurate simultaneous detection of glucose, potassium ions and pH value in sweat, improves the manufacturing speed and detection efficiency, and is suitable for the field of wearable sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743547A_ABST
    Figure CN118743547A_ABST
Patent Text Reader

Abstract

The invention provides a wearable sweat sensor based on laser-induced graphene and a preparation method of the wearable sweat sensor. The invention relates to the technical field of micro-nano sensing and flexible electronics. The method comprises the following steps: performing laser firing on a polyimide film to prepare graphene; carrying out laser cutting on the polyethylene glycol terephthalate film to prepare a microfluidic channel layer; the sensor is prepared by electrochemical deposition and dispensing methods; assembling the sensor and a micro-fluidic channel layer to obtain the sweat integrated sensor; the sweat integrated sensor is attached to the skin surface to detect the marker. The invention provides a wearable integrated sweat sensor based on laser-induced graphene. The wearable integrated sweat sensor is used for detecting glucose, potassium ions and the PH value in sweat so as to explore the physiological state of a detected person.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of micro-nano sensing and flexible electronic technology, and in particular to a wearable sweat integrated sensor based on laser-induced graphene and a preparation method thereof. Background Art

[0002] Human sweat is one of the most important body fluids related to physiological conditions. Compared with other biological fluids, sweat contains a wealth of markers, including electrolytes, metabolites, and exogenous substances. The levels of these markers in sweat are closely related to those in blood and can convey relevant physiological information about the body. The collection, detection, and quantitative analysis of markers in sweat can assess the physiological state and health of the person being tested.

[0003] Wearable sensors need to be made of materials that can still have good performance under certain deformation conditions. Although metal electrodes have excellent electrical conductivity, electrocatalytic properties and stability, they are difficult to use in wearable sensors due to their high cost, poor bending resistance and some intermediates are toxic to the human body. Graphene has extremely high carrier mobility, ultra-large specific surface area, good electrical conductivity and outstanding mechanical properties, and is widely used in the field of wearable sensors. The common methods for making graphene currently include mechanical exfoliation, redox method and chemical gas deposition method, but the above methods all have disadvantages such as high cost and complex production process, making it difficult to prepare wearable sensors on a large scale.

[0004] In addition, most existing flexible wearable sweat sensors can only detect one substance, but judging the body's physiological state often requires detecting multiple substances, which requires the subject to wear multiple sensors, greatly reducing detection efficiency. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to propose a wearable sweat integrated sensor based on laser-induced graphene and a preparation method thereof, which can simultaneously and accurately detect glucose, potassium ions and pH value in sweat.

[0006] A method for preparing a wearable sweat integrated sensor based on laser-induced graphene of the present invention comprises the following steps:

[0007] S1, five laser-induced graphene electrodes are prepared on the surface of polyimide film from left to right;

[0008] S2, coating Ag / Agcl conductive silver paste on the reaction areas of the two graphene electrodes to obtain two reference electrodes;

[0009] S3, dissolving pyrrole and potassium chloride in deionized water, stirring until uniform, to obtain a mixed solution A; placing a graphene electrode in the mixed solution A; performing cyclic voltammetry on a graphene electrode using an electrochemical workstation, and obtaining a pH sensing electrode after drying;

[0010] S4, adding 3,4-ethylenedioxythiophene and poly (sodium 4-styrene sulfonate) to deionized water, stirring until uniform, to obtain a mixed solution B; placing graphene in the mixed solution B, using an electrochemical workstation to perform constant current deposition on a graphene electrode, and obtaining a poly (3,4-ethylenedioxythiophene) / graphene electrode after drying;

[0011] S5, dissolving hydrochloric acid, potassium chloride, potassium ferrocyanide and ferric chloride in deionized water, stirring until uniform, to obtain a mixed solution D; inserting graphene into the mixed solution D, and using an electrochemical workstation to perform a constant potential method and a cyclic voltammetry method on a graphene electrode to prepare a Prussian blue / graphene electrode;

[0012] S6, adding valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate mixture to cyclohexanone in proportion, stirring until uniform, to obtain a mixed solution C; dissolving acetic acid and chitosan in deionized water, stirring until uniform, adding multi-walled carbon nanotubes after no obvious precipitation, ultrasonic stirring, and adding glucose oxidase solution to the mixed solution in a certain proportion to obtain a mixed solution E;

[0013] S7, adding the mixed solution C dropwise onto the poly(3,4-ethylenedioxythiophene) / graphene electrode, and drying at room temperature to obtain a potassium ion sensing electrode; adding the mixed solution E dropwise onto the Prussian blue / graphene electrode, and drying at room temperature to obtain a glucose sensing electrode;

[0014] S8, placing the polyethylene terephthalate film in a laser cutting machine, setting corresponding parameters for cutting to obtain a microfluidic channel layer corresponding to the five graphene electrodes;

[0015] S9, laminating the microfluidic channel layer on the surface of the polyimide film to obtain a wearable sweat integrated sensor.

[0016] Furthermore, step S8 also includes placing the medical double-sided tape in a laser cutting machine, setting corresponding parameters for cutting to obtain a sensor connection layer, and the microfluidic channel layer is attached to the surface of the polyimide film through the sensor connection layer.

[0017] Furthermore, step S8 also includes placing the medical double-sided tape in a laser cutting machine, setting corresponding parameters for cutting to obtain a sweat inlet layer, and the sweat inlet layer is attached to the upper surface of the microfluidic channel layer.

[0018] Furthermore, in step S1, the power of the blue light laser engraving machine used is set to 1.35W, the laser speed is 1.8mm / S, and the reaction area of ​​the graphene electrode is circular with a diameter of 6mm.

[0019] Furthermore, in step S3, the concentrations of potassium chloride and pyrrole are both 0.1 mol / L, the cyclic voltammetry scanning interval is 0-4 V, the scanning speed is 0.05 V / S, and the number of scanning cycles is 3 times.

[0020] Further, in step S4, the concentration of 3,4-ethylenedioxythiophene is 0.01 mol / L, and the concentration of poly(sodium 4-styrene sulfonate) is 0.1 mol / L; the current size of the constant current deposition method is 56 uA, and the deposition time is 710 S;

[0021] In step S6, valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate are added in a mass ratio of 2:0.5:32.6:64.8; in step S6, acetic acid and chitosan are added at 1% of the volume and mass of deionized water respectively, multi-walled carbon nanotubes are added at 2 mg / mL, the content of glucose oxidase solution is 6 mg / mL, and the mixed solution and glucose oxidase solution are added in a ratio of 2:1 to form a mixed solution E.

[0022] Further, in step S5, the concentrations of hydrochloric acid, potassium chloride, potassium ferrocyanide and ferric chloride are 0.12 mol / L, 0.1 mol / L, 0.002 mol / L and 0.002 mol / L respectively;

[0023] In step S5, a constant potential method is first performed, with a potential of 0.4 V for 300 S, and a cyclic voltammetry method is performed, with a cycle interval of -0.05 V to 0.35 V, a cycle rate of 0.05 V / S, and a cycle number of 40 times.

[0024] Furthermore, the glucose sensing electrode is located at the left end or the right end of the polyimide film surface, and two reference electrodes are respectively arranged between the glucose sensing electrode, the pH sensing electrode, and the potassium ion sensing electrode.

[0025] Furthermore, the power of the laser cutting machine used was set to 4w, the laser speed was 80mm / s, the small circular diameter of the sweat inlet of the sweat inlet layer and the microfluidic channel layer was 1mm, the circular diameter of the injection port of the microfluidic channel layer was 6mm, and the microchannel width was 0.3mm.

[0026] A wearable sweat integrated sensor based on laser-induced graphene prepared by the above-mentioned preparation method.

[0027] In the present invention, since the entire sensor needs to be immersed in different solutions for multiple times, the preparation of the sensing electrode needs to be in a certain order. The polymer is highly stable and not easy to react, so in the preparation process of the present invention, polypyrrole and poly (3,4-ethylenedioxythiophene) are first electrodeposited on the graphene electrode, and finally Prussian blue is electrochemically deposited.

[0028] Beneficial effects of the present invention:

[0029] 1) A wearable sweat integrated sensor based on laser-induced graphene of the present invention can simultaneously and accurately detect glucose, potassium ions and pH value in sweat.

[0030] 2) The graphene prepared by the laser induction method of the present invention has extremely high carrier mobility, ultra-large specific surface area, good electrical conductivity and excellent mechanical properties. The graphene prepared by the laser induction method has the advantages of high precision, repeatability, controllable scale, industrial deployment, low cost, fast and energy saving.

[0031] 3) Polyethylene terephthalate film is a common plastic film, which is easy to purchase and can be customized in thickness. The present invention uses polyethylene terephthalate film to prepare the microfluidic channel layer, which greatly optimizes the microfluidic preparation process, reduces the preparation difficulty, and enables microfluidics to be prepared on a large scale. The method of preparing microfluidic channels by laser cutting is simple and low-cost.

[0032] 4) The method of using laser-induced graphene and laser cutting of microfluidic channels in the present invention can be widely used in the field of wearable sensors, further improving the manufacturing rate of sweat integrated sensors and reducing the manufacturing cost of sweat integrated sensors. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A diagram showing the structure of a sensor in an embodiment of the present invention;

[0034] Figure 2 A microfluidic structure diagram in an embodiment of the present invention;

[0035] Figure 3 This is a structural diagram of a sweat integrated sensor in an embodiment of the present invention;

[0036] Figure 4 is the sensitivity fitting curve of the pH sensor electrode in Example 1;

[0037] Figure 5 is the sensitivity fitting curve of the potassium ion sensing electrode in Example 1;

[0038] Figure 6 is the sensitivity fitting curve of the glucose sensor electrode in Example 1;

[0039] Figure 7 It is the sensitivity fitting curve of the pH sensing electrode in Comparative Example 1;

[0040] Figure 8 is the sensitivity fitting curve of the potassium ion sensing electrode in Comparative Example 1;

[0041] Fig. 9 This is the sensitivity fitting curve of the glucose sensor electrode in Comparative Example 1. DETAILED DESCRIPTION

[0042] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0043] Example 1

[0044] A method for preparing a wearable sweat integrated sensor based on laser-induced graphene of the present invention comprises the following steps:

[0045] Step 1: Place the polyimide film in a beaker filled with anhydrous ethanol, and then place it in an ultrasonic cleaner for 10 minutes. After the ultrasonic treatment, place the film in a beaker filled with deionized water, and then perform ultrasonic treatment for another 10 minutes. Then take it out and place it in a drying oven at 50°C for 5 minutes. After drying, enter the corresponding pattern in the software, and use a blue light laser engraver for laser induction to prepare five graphene electrodes.

[0046] The corresponding pattern in step 1 is composed of five circles and five rectangles, one circle (reaction area) and one rectangle constitute a graphene electrode, wherein the diameter of the circle is 6 mm;

[0047] The power of the blue light laser engraving machine used in step 1 is set to 1.35W, and the laser speed is 1.8mm / S.

[0048] Step 2: Coat the circular area of ​​graphene (reaction area) with Ag / Agcl conductive silver paste. After coating, place it in a drying oven at 50°C for 30 minutes to obtain an Ag / Agcl reference electrode.

[0049] Step 3: Prepare 50mL of deionized water and pour it into a beaker, weigh 0.372g of potassium chloride and dissolve it in the beaker, then use a pipette to extract 350uL of pyrrole and drip it into the beaker, and stir for 10 minutes to obtain a mixed solution A of 0.1mol / L pyrrole and potassium chloride. Graphene is used as the working electrode, platinum electrode as the counter electrode, and commercial Ag / Agcl electrode as the reference electrode. Place the three electrodes in the mixed solution A and perform cyclic voltammetry using an electrochemical workstation. After the cyclic voltammetry is completed, a polypyrrole / graphene sensing electrode, i.e., a pH sensing electrode, is obtained;

[0050] In step 3, the cyclic voltammetry scanning interval is 0-4V, the scanning speed is 0.05V / S, and the number of scanning cycles is 3 times.

[0051] Step 4: 0.07 g of 3,4-ethylenedioxythiophene and 1.03 g of poly(sodium 4-styrene sulfonate) were added to 50 mL of deionized water and stirred for 10 minutes to obtain a mixed solution B of 0.01 mol / L 3,4-ethylenedioxythiophene and 0.1 mol / L poly(sodium 4-styrene sulfonate). 200 mg of a mixture of valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate in a mass ratio of 2:0.5:32.6:64.8 was added to 700 uL of cyclohexanone and stirred until uniform to obtain a mixed solution C.

[0052] Step 5: Graphene is used as the working electrode, platinum electrode is used as the counter electrode, and commercial Ag / Agcl electrode is used as the reference electrode. The three electrodes are placed in the mixed solution B and constant current deposition is performed using an electrochemical workstation to obtain a poly(3,4-ethylenedioxythiophene) / graphene electrode;

[0053] In the step 5, the current of the constant current deposition method is 56uA, and the deposition time is 710S.

[0054] Step 6: Take 0.5mL concentrated hydrochloric acid (12mol / L), 0.372g potassium chloride, 0.032g potassium ferrocyanide and 0.016g ferric chloride, add 50mL deionized water, stir for 10 minutes, and obtain mixed solution D. Add 200uL acetic acid to 20mL deionized water, add 200mg chitosan, stir for 1 hour, add 40mg multi-walled carbon nanotubes after no obvious precipitation, and ultrasonicate for 30 minutes to obtain a mixed solution of acetic acid, chitosan and multi-walled carbon nanotubes. Add 6mg glucose oxidase to 1mL deionized water and stir for 5 minutes. Take 2mL of the mixed solution and add glucose oxidase solution, stir for 3 minutes to obtain mixed solution E.

[0055] Step 7: Graphene is used as the working electrode, platinum electrode is used as the counter electrode, and commercial Ag / Agcl electrode is used as the reference electrode. The three electrodes are placed in the mixed solution D, and the Prussian blue / graphene electrode is prepared by constant potential method and cyclic voltammetry using an electrochemical workstation;

[0056] In step 7, the constant current deposition potential is set to 0.4 V and lasts for 300 seconds;

[0057] In the step 7, the cyclic voltammetry method is set to have a cycle interval of -0.05V-0.35V, a cycle rate of 0.05V / s, and a cycle number of 40 times.

[0058] Step 8: Use a pipette to take 6ul of mixed solution C and 6ul of mixed solution E respectively, drop 6uL of mixed solution C onto the poly(3,4-ethylenedioxythiophene) / graphene electrode, and drop 6uL of mixed solution E onto the Prussian blue / graphene electrode. Dry at room temperature to obtain a potassium ion sensing electrode and a glucose sensing electrode.

[0059] Figure 1 Schematic diagram of the sensor prepared in this embodiment, the sensor contains a total of 5 electrodes, from left to right, respectively, pH sensing electrode, Ag / Agcl reference electrode, potassium ion sensing electrode, Ag / Agcl reference electrode and glucose sensing electrode, wherein the circular area is the reaction area. Since the pH sensing electrode and the potassium ion sensing electrode are potentiometric sensors, the pH sensing electrode and the potassium ion sensing electrode share a Ag / Agcl reference electrode. The glucose sensing electrode is an amperometric sensing electrode, so a single Ag / Agcl reference electrode is used.

[0060] Step 9: Place two pieces of medical double-sided tape and a piece of polyethylene terephthalate film in the laser cutting machine, set the parameters, power to 4w, laser speed to 80mm / s, and cut them.

[0061] Figure 2 The microfluidic structure diagram shows the sweat inlet layer, microfluidic channel layer and sensor connection layer from top to bottom. The small circle in the sweat inlet layer is the sweat inlet, with a total of 8, a diameter of 1mm, used to collect sweat on the skin surface. The microfluidic channel layer has small circles (sweat inlets), large circles (sweat collection areas) and microfluidic channels between the circles. There are 3 sweat collection areas with a diameter of 6mm. The width of the microfluidic channel is 0.5mm. The sensor connection layer has three sweat collection areas for collecting sweat.

[0062] Step 10: Untie the backing paper on the double-sided adhesive surface of the sweat inlet layer and the sensor connection layer, align the sweat inlet in the sweat inlet layer with the sweat inlet of the microfluidic channel layer, align the sweat collection area of ​​the microfluidic channel layer with the sweat collection area of ​​the sensor connection layer, and align the sweat collection area of ​​the sensor connection layer with the reaction area of ​​the sensor, as shown in FIG. Figure 3 As shown, the preparation of the sweat integrated sensor is completed.

[0063] Test Example 1

[0064] Experimental plan 1: Prepare a solution with a pH value of 4-9 to simulate the pH detection in sweat. Use an electrochemical workstation to connect the pH sensing electrode and the Ag / Agcl reference electrode, where the pH sensing electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a dual-electrode system. Put the dual electrodes into a solution with a pH of 4 for an open circuit voltage test. After the test, wash with deionized water and then test in a solution with a pH of 5. Repeat the above process until the pH of 9 solution test is completed.

[0065] After testing, the fitting results are as follows Figure 4 As shown, the curve equation is Y = -73.736X + 762.51, and its curve R 2 It is 0.996 and the sensitivity is 73.736mV / dec, which shows that the pH sensing electrode has a good response to different pH values.

[0066] Experimental plan 2: Prepare solutions with potassium chloride concentrations of 2mM, 4mM, 8mM, 16mM and 32mM to simulate potassium ion detection in sweat. Use an electrochemical workstation to connect the potassium ion sensing electrode and the Ag / Agcl reference electrode, where the potassium ion sensing electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a two-electrode system. Place the two electrodes in a 2mM potassium chloride solution for an open circuit voltage test. After the test, wash with deionized water and then place in a 4mM potassium chloride solution for testing. Repeat the above process until the 32mM potassium chloride solution test is completed.

[0067] After testing, the fitting results are as follows Figure 5 As shown, the curve equation is Y = 57.3X-76.49, and its curve R 2 It is 0.995 and the sensitivity is 57.3mV / dec, which shows that the potassium ion sensing electrode has a good response to potassium ions at different potassium ion concentrations.

[0068] Experimental plan 3: Prepare solutions with glucose concentrations of 0.1M, 0.25M, 0.5M, 1M and 2.5M, use an electrochemical workstation to connect the glucose sensor electrode and the Ag / Agcl reference electrode to simulate the detection of glucose in sweat, where the glucose sensor electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a two-electrode system, which is placed in deionized water for detection. During the test, 10uL is added with a pipette for each concentration, and one more drop is added when testing 2.5M.

[0069] After testing, the fitting results are as follows Figure 6 As shown, the curve equation is Y = -0.0471X-4.32, and its curve R 2 It is 0.981 and the sensitivity is 0.0471uA / uM, which shows that the glucose sensing electrode has a good response to glucose.

[0070] Comparative Example 1

[0071] A method for preparing a wearable sweat integrated sensor based on laser-induced graphene comprises the following steps:

[0072] Step 1: Place the polyimide film in a beaker filled with anhydrous ethanol, and then place it in an ultrasonic cleaner for 10 minutes. After the ultrasonic treatment, place the film in a beaker filled with deionized water, and then perform ultrasonic treatment for another 10 minutes. Then take it out and place it in a drying oven at 50°C for 5 minutes. After drying, enter the corresponding pattern in the software, and use a blue light laser engraver for laser induction to prepare five graphene electrodes.

[0073] The corresponding pattern in step 1 is composed of five circles and five rectangles, one circle (reaction area) and one rectangle constitute a graphene electrode, wherein the diameter of the circle is 6 mm;

[0074] The power of the blue light laser engraving machine used in step 1 is set to 1.2w, and the laser speed is 1.8mm / s.

[0075] Step 2: Coat the circular area of ​​graphene (reaction area) with Ag / Agcl conductive silver paste. After coating, place it in a drying oven at 50°C for 30 minutes to obtain an Ag / Agcl reference electrode.

[0076] Step 3: Prepare 50mL of deionized water and pour it into a beaker, weigh 0.372g of potassium chloride and dissolve it in the beaker, then use a pipette to extract 350uL of pyrrole and drip it into the beaker, and stir for 10 minutes to obtain a mixed solution F of 0.1mol / L pyrrole and potassium chloride. Graphene is used as the working electrode, platinum electrode as the counter electrode, and commercial Ag / Agcl electrode as the reference electrode. Place the three electrodes in the mixed solution F and perform cyclic voltammetry using an electrochemical workstation. After the cyclic voltammetry is completed, a polypyrrole / graphene sensing electrode, i.e., a pH sensing electrode, is obtained;

[0077] In step 3, the cyclic voltammetry scanning interval is 0-3V, the scanning speed is 0.1V / S, and the number of scanning cycles is 3 times.

[0078] Step 4: Add 700uL of cyclohexanone to a mixture of 200mg of valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate in a mass ratio of 2:0.5:32.6:64.8, and stir until uniform to obtain a mixed solution G.

[0079] Step 5: Take 0.5mL concentrated hydrochloric acid (12mol / L), 0.372g potassium chloride, 0.032g potassium ferrocyanide and 0.016g ferric chloride, add 50mL deionized water, stir for 10 minutes, and obtain mixed solution H. Add 200uL acetic acid to 20mL deionized water, add 200mg chitosan, stir for 1 hour, add 40mg multi-walled carbon nanotubes after no obvious precipitation, and ultrasonicate for 30 minutes to obtain a mixed solution of acetic acid, chitosan and multi-walled carbon nanotubes. Add 6mg glucose oxidase to 1mL deionized water and stir for 5 minutes. Take 2mL of the mixed solution and add glucose oxidase solution, stir for 3 minutes to obtain mixed solution I.

[0080] Step 6: Graphene was used as the working electrode, platinum electrode as the counter electrode, and commercial Ag / Agcl electrode as the reference electrode. The three electrodes were placed in the mixed solution H, and the Prussian blue / graphene electrode was prepared by constant potential method and cyclic voltammetry using an electrochemical workstation;

[0081] In step 6, the constant current deposition potential is set to 0.4V and lasts for 240S;

[0082] In the step 6, the cyclic voltammetry method is set to have a cycle interval of -0.05V-0.35V, a cycle rate of 0.05V / s, and a cycle number of 40 times.

[0083] Step 7: Use a pipette to take 6ul of mixed solution G and 6ul of mixed solution I respectively, drop 6uL of mixed solution G onto the graphene electrode, and drop 6uL of mixed solution I onto the Prussian blue / graphene electrode. Dry at room temperature to obtain a potassium ion sensing electrode and a glucose sensing electrode.

[0084] Step 8: Place two pieces of medical double-sided tape and a piece of polyethylene terephthalate film in the laser cutting machine, set the parameters, power to 4w, laser speed to 80mm / s, and cut them.

[0085] Step 9: Untie the backing paper on the double-sided adhesive surface of the sweat inlet layer and the sensor connection layer, align the sweat inlet in the sweat inlet layer with the sweat inlet of the microfluidic channel layer, align the sweat collection area of ​​the microfluidic channel layer with the sweat collection area of ​​the sensor connection layer, and align the sweat collection area of ​​the sensor connection layer with the reaction area of ​​the sensor, as shown in FIG. Figure 3 As shown, the preparation of the sweat integrated sensor is completed.

[0086] Test Example 2

[0087] Experimental plan 1: Prepare a solution with a pH value of 4-9 to simulate the pH detection in sweat. Use an electrochemical workstation to connect the pH sensing electrode and the Ag / Agcl reference electrode, where the pH sensing electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a dual-electrode system. Put the dual electrodes into a solution with a pH of 4 for an open circuit voltage test. After the test, wash with deionized water and then test in a solution with a pH of 5. Repeat the above process until the pH of 9 solution test is completed.

[0088] After testing, the fitting results are as follows Figure 7 As shown, the curve equation is Y = -33.95X + 457.66, and its curve R 2 The value is 0.991 and the sensitivity is 33.95mV / dec.

[0089] Experimental plan 2: Prepare solutions with potassium chloride concentrations of 2mM, 4mM, 8mM, 16mM and 32mM to simulate potassium ion detection in sweat. Use an electrochemical workstation to connect the potassium ion sensing electrode and the Ag / Agcl reference electrode, where the potassium ion sensing electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a two-electrode system. Place the two electrodes in a 2mM potassium chloride solution for an open circuit voltage test. After the test, wash with deionized water and then place in a 4mM potassium chloride solution for testing. Repeat the above process until the 32mM potassium chloride solution test is completed.

[0090] After testing, the fitting results are as follows Figure 8 As shown, the curve equation is Y = 42.96X + 24.17, and its curve R 2 The value is 0.998 and the sensitivity is 42.96mV / dec.

[0091] Experimental plan 3: Prepare solutions with glucose concentrations of 0.1M, 0.25M, 0.5M, 1M and 2.5M, use an electrochemical workstation to connect the glucose sensor electrode and the Ag / Agcl reference electrode to simulate the detection of glucose in sweat, where the glucose sensor electrode is used as the working electrode and the Ag / Agcl electrode is used as the reference electrode to form a two-electrode system, which is placed in deionized water for detection. During the test, 10uL is added with a pipette for each concentration, and one more drop is added when testing 2.5M.

[0092] After testing, the fitting results are as follows Fig. 9 As shown, the curve equation is Y = -0.0325X-85.22, and its curve R 2 It is 0.997 and the sensitivity is 0.0325uA / uM.

[0093] Compared with Example 1, Comparative Example 1 adjusted the laser power of laser-induced graphene, the cycle range and cycle speed of the subsequent pH sensor cyclic voltammetry, and the Prussian deposition time, and did not include step 5 in Example 1, so the sensitivity of the obtained sensor was greatly reduced.

[0094] For matters not mentioned above, the prior art applies.

[0095] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a wearable sweat integrated sensor based on laser-induced graphene, characterized in that: The following steps are involved: S1, five laser-induced graphene electrodes are prepared on the surface of polyimide film from left to right; S2, coating Ag / Agcl conductive silver paste on the reaction areas of the two graphene electrodes to obtain two reference electrodes; S3, dissolving pyrrole and potassium chloride in deionized water, stirring until uniform, to obtain a mixed solution A; placing a graphene electrode in the mixed solution A; performing cyclic voltammetry on a graphene electrode using an electrochemical workstation, and obtaining a pH sensing electrode after drying; S4, adding 3,4-ethylenedioxythiophene and poly (sodium 4-styrene sulfonate) to deionized water, stirring until uniform, to obtain a mixed solution B; placing graphene in the mixed solution B, using an electrochemical workstation to perform constant current deposition on a graphene electrode, and obtaining a poly (3,4-ethylenedioxythiophene) / graphene electrode after drying; S5, dissolving hydrochloric acid, potassium chloride, potassium ferrocyanide and ferric chloride in deionized water, stirring until uniform, to obtain a mixed solution D; inserting graphene into the mixed solution D, and using an electrochemical workstation to perform a constant potential method and a cyclic voltammetry method on a graphene electrode to prepare a Prussian blue / graphene electrode; S6, adding valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate mixture to cyclohexanone in proportion, stirring until uniform, to obtain a mixed solution C; dissolving acetic acid and chitosan in deionized water, stirring until uniform, adding multi-walled carbon nanotubes after no obvious precipitation, ultrasonic stirring, and adding glucose oxidase solution to the mixed solution in a certain proportion to obtain a mixed solution E; S7, dropping the mixed solution C onto the poly(3,4-ethylenedioxythiophene) / graphene electrode, and drying at room temperature to obtain a potassium ion sensing electrode; dropping the mixed solution E onto the Prussian blue / graphene electrode, and drying at room temperature to obtain a glucose sensing electrode; S8, placing the polyethylene terephthalate film in a laser cutting machine, setting corresponding parameters for cutting to obtain a microfluidic channel layer corresponding to the five graphene electrodes; S9, laminating the microfluidic channel layer on the surface of the polyimide film to obtain a wearable sweat integrated sensor.

2. The preparation method according to claim 1, characterized in that: Step S8 also includes placing the medical double-sided tape in a laser cutting machine, setting corresponding parameters for cutting to obtain a sensor connection layer, and laminating the microfluidic channel layer on the surface of the polyimide film through the sensor connection layer.

3. The preparation method according to claim 2, characterized in that: Step S8 also includes placing the medical double-sided tape in a laser cutting machine, setting corresponding parameters for cutting to obtain a sweat inlet layer, and the sweat inlet layer is attached to the upper surface of the microfluidic channel layer.

4. The preparation method according to any one of claims 1 to 3, characterized in that: In step S1, the power of the blue light laser engraving machine used is set to 1.35W, the laser speed is 1.8mm / S, and the reaction area of ​​the graphene electrode is circular with a diameter of 6mm.

5. The preparation method according to any one of claims 1 to 3, characterized in that: In step S3, the concentrations of potassium chloride and pyrrole are both 0.1 mol / L, the cyclic voltammetry scanning interval is 0-4 V, the scanning speed is 0.05 V / S, and the number of scanning cycles is 3 times.

6. The preparation method according to any one of claims 1 to 3, characterized in that: In step S4, the concentration of 3,4-ethylenedioxythiophene is 0.01 mol / L, and the concentration of poly(sodium 4-styrene sulfonate) is 0.1 mol / L; the current size of the constant current deposition method is 56 uA, and the deposition time is 710 s; In step S6, valinomycin, sodium tetraphenylborate, polyvinyl chloride and bis(2-ethylhexyl) sebacate are added in a mass ratio of 2:0.5:32.6:64.8; acetic acid and chitosan are added at 1% of the volume and mass of deionized water, respectively, multi-walled carbon nanotubes are added at 2 mg / mL, the content of glucose oxidase solution is 6 mg / mL, and the mixed solution and glucose oxidase solution are added in a ratio of 2:1 to form a mixed solution E.

7. The preparation method according to any one of claims 1 to 3, characterized in that: In step S5, the concentrations of hydrochloric acid, potassium chloride, potassium ferrocyanide and ferric chloride are 0.12 mol / L, 0.1 mol / L, 0.002 mol / L and 0.002 mol / L respectively; In step S5, a constant potential method is first performed, with a potential of 0.4 V for 300 S, and a cyclic voltammetry method is performed, with a cycle interval of -0.05 V to 0.35 V, a cycle rate of 0.05 V / S, and a cycle number of 40 times.

8. The preparation method according to any one of claims 1 to 3, characterized in that: The glucose sensing electrode is located at the left end or the right end of the surface of the polyimide film, and two reference electrodes are respectively arranged between the glucose sensing electrode, the pH sensing electrode and the potassium ion sensing electrode.

9. The preparation method according to claim 3, characterized in that: The power of the laser cutting machine used was set to 4w, the laser speed was 80mm / s, the small circular diameter of the sweat inlet of the sweat inlet layer and the microfluidic channel layer was 1mm, the circular diameter of the injection port of the microfluidic channel layer was 6mm, and the microchannel width was 0.3mm.

10. A wearable sweat integrated sensor based on laser-induced graphene prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Ion sensor, preparation method thereof and wearable electronic equipment

    CN119666964A

  • Sweat sensor and preparation method and application thereof

    CN119881034A

  • Preparation method of micro-fluidic chip of multifunctional sensing system

    CN120227902A