Hydrogel microspheres for capturing and storing free DNA as well as preparation method and application of hydrogel microspheres
By using a composite structure of polydopamine nanosheets and GelMA hydrogel microspheres to capture and store free DNA, the problem of cytotoxicity and low adsorption efficiency of cationic materials is solved, and rapid healing of diabetic wounds and effective regulation of inflammation are achieved.
Patent Information
- Application Number
- CN202410740240.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
AI Technical Summary
Existing cationic materials are highly cytotoxic when capturing free DNA (cfDNA) and are easily affected by serum, resulting in a decrease in adsorption efficiency, difficulty in effectively reducing cfDNA concentration, and affecting diabetic wound healing and inflammation regulation.
A composite structure of polydopamine nanosheets and gelatin-methacrylic anhydride (GelMA) hydrogel microspheres is used to capture and store cfDNA through π-π stacking and hydrogen bonding interactions, using the polymer network confinement of the hydrogel microspheres. The release of cfDNA reduces the production of ROS.
It achieves high-efficiency, low-toxicity capture and storage of cfDNA, reduces chronic inflammation of diabetic wounds, shortens wound healing time, and has good biocompatibility and anti-inflammatory effects.
Smart Images

Figure CN118743686A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomaterial preparation, and in particular relates to a hydrogel microsphere for capturing and storing free DNA, and a preparation method and application thereof. Background Art
[0002] Cell-free DNA (cfDNA) is a powerful damage-associated molecular pattern (DAMPs). They initiate a process similar to the cell signaling pathway in the body, that is, cfDNA is released by necrotic / apoptotic cells, neutrophil extracellular traps (NETs) or invasive microorganisms, contacts immune cells, and is recognized by pattern recognition receptors (PRRs) in immune cells, thereby initiating intracellular immune signaling cascades and releasing inflammatory factors. Although cfDNA may originate from the host, it always acts as a pro-inflammatory "information medium" and causes pro-inflammatory biological effects. Although in order to maintain tissue homeostasis, the body has established a variety of defense mechanisms to clear circulating cfDNA, such as liver uptake and kidney filtration, as well as the degradation of cfDNA by various nucleases inside and outside the cell. However, factors such as mutations in nucleic acid metabolism-related genes, reduced nuclease activity, and oxidized cfDNA escaping nuclease degradation lead to excessive accumulation of circulating cfDNA, which may lead to the occurrence of inflammatory diseases such as rheumatoid arthritis, systemic lupus erythematosus, chronic wounds that do not heal, and sepsis. Therefore, rational intervention of cfDNA concentration and blocking of signal transduction between cfDNA and immune cells are crucial for regulating chronic inflammation and may be a new strategy for the treatment of such diseases.
[0003] Tissue regeneration is usually a complex programmed process, in which the generation and resolution of inflammation are extremely important, requiring interaction and coordination between immune cells and biochemical mediators. For example, the healing process of diabetic wounds may be stuck in the stage of persistent inflammation, which may be due to an imbalance in communication between cfDNA and immune cells. In addition to the release of a large amount of cfDNA by damaged cells, hyperglycemia promotes the production of excessive NETs, and the release of DNA fragments is also one of the reasons why cfDNA in diabetic wound sites remains at a high level. cfDNA can be recognized by Toll-like receptors (TLRs) expressed in immune cells, activating their downstream NF-κB signaling pathway and inducing excessive release of inflammatory cytokines. In addition, many inflammatory cytokines can activate various oxidases, produce excessive reactive oxygen species (ROS), and then lead to cell death, release DAMPs including cfDNA, and form a vicious cycle. Worse, ROS not only cause oxidative damage to tissues, but also oxidize cfDNA, making it more susceptible to phagocytosis by immune cells. Restoring the balance of communication between cfDNA and immune cells may be a potential therapeutic strategy to promote regeneration of chronic wounds.
[0004] However, how to effectively and specifically reduce the concentration of cfDNA in pathological microenvironments remains a challenge. DNA molecules have a sophisticated double helix structure and are naturally "assigned" to carry genetic information. Although DNA nanotechnology is becoming an increasingly powerful force in materials science, which can manipulate DNA molecules and their derivatives using the base pairing properties of DNA, cfDNA molecules are highly degraded nucleic acid fragments without accurate base sequences and lengths, making them difficult to interact with or remove through base pairing.
[0005] Although the use of polycationic materials to absorb polyanionic cfDNA through electrostatic interactions is a feasible method, other electronegative molecules such as proteins can also be quickly adsorbed, thereby reducing the efficiency and specificity of cfDNA binding. For example, the cationic material PEI has a strong adsorption effect on serum proteins (negatively charged under physiological conditions), and its adsorption efficiency for cfDNA is significantly reduced in the presence of serum. On the other hand, cationic materials are highly cytotoxic, with an IC50 of around 100 micrograms per milliliter. Therefore, the problems of cationic materials' strong adsorption capacity for serum and potential cytotoxicity are not conducive to the subsequent in vivo application and clinical transformation of such materials.
[0006] Therefore, how to provide a biomaterial with good biosafety, low cytotoxicity, and no influence of serum, capable of efficiently and long-term capture and storage of cfDNA, and capable of shortening the wound healing time and having good anti-inflammatory effects in diabetic patients, has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] The present invention is to solve the above technical problems, thereby providing a hydrogel microsphere for capturing and storing free DNA and its preparation method and application. The technical purpose of the present invention is to provide a biomaterial that can capture and store excess cfDNA in the microenvironment in the body to prevent the pro-inflammatory signals caused by cfDNA, thereby reducing chronic inflammation, and has good biosafety, low cytotoxicity, short wound healing time for diabetic patients, and good anti-inflammatory effect, so as to solve the problems of existing cationic materials with high cytotoxicity, significantly reduced adsorption efficiency of cfDNA due to the influence of serum, and long wound healing time for diabetic patients.
[0008] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0009] The present invention first provides a method for preparing hydrogel microspheres for capturing and storing free DNA, comprising the following steps:
[0010] (1) preparing polydopamine nanosheets;
[0011] (2) Preparation of GelMA hydrogel microspheres using a microfluidic device;
[0012] (3) The freeze-dried GelMA hydrogel microspheres are swelled in a polydopamine nanosheet suspension to prepare GelMA hydrogel microspheres encapsulating polydopamine nanosheets.
[0013] The present invention develops a composite hydrogel microsphere as an intervention medium between cfDNA and immune cells through the above method. The π-π stacking / hydrogen bonding interaction between DNA bases rich in π-conjugated structure and polydopamine nanosheets and the polymer network of the hydrogel microsphere are used to capture and store excess cfDNA in the microenvironment to prevent the pro-inflammatory signals caused by cfDNA, thereby alleviating chronic inflammation.
[0014] The above method of the present invention prepares polydopamine nanosheets (PDANSs) with orderly stacking of partial oligomers by self-polymerization and directional assembly of dopamine, and further embeds PDANSs in gelatin-methacrylic anhydride (GelMA) hydrogel microspheres prepared by microfluidic technology to obtain composite hydrogel microspheres. The internal PDA nanosheets provide a large specific surface area and π-conjugated binding sites, and capture cfDNA through π-π stacking interactions. The polymer network of GelMA microspheres forms a "cage-like" space to restrict cfDNA. In addition, the rich catechol groups on the surface of PDA help reduce ROS in the microenvironment and play a positive role in controlling the concentration of cfDNA. The hydrogel microspheres have good biocompatibility, can exclude nonspecific adsorption of biological molecules such as negatively charged proteins, and have the characteristics of good biosafety, low cytotoxicity, short wound healing time for diabetic patients (only 12 days), and good anti-inflammatory effect.
[0015] However, the existing method of using cationic polymer materials to capture cfDNA has the problems of high cytotoxicity, susceptibility to specific adsorption by biological molecules such as negatively charged proteins, which greatly reduces the capture efficiency, long wound healing time for diabetic patients (requires 14 days), and poor anti-inflammatory effect.
[0016] The present invention provides an efficient and low-toxic strategy for cfDNA signal transduction intervention, and can also be extended to other tissue trauma, autoimmune diseases, chronic inflammatory diseases, etc.
[0017] Furthermore, the preparation method of the polydopamine nanosheets in step (1) is: mixing the herring sperm DNA solution and the dopamine hydrochloride solution evenly, then adding the tris(hydroxymethyl)aminomethane solution, placing it on a rotary mixer to react at room temperature for 24 hours, centrifuging (11000 rpm, 10 min) and discarding the supernatant to obtain the nanosheet product.
[0018] Furthermore, the concentration ratio of the herring sperm DNA solution, dopamine hydrochloride solution and tris(hydroxymethyl)aminomethane solution is 2:4:3.
[0019] Furthermore, in step (2), the GelMA solution is used as the dispersed phase, and the liquid paraffin containing 10 wt % of Span 80 is used as the continuous phase, and then the GelMA hydrogel microspheres are prepared by photocrosslinking.
[0020] Furthermore, in step (3), the weight ratio of GelMA hydrogel microspheres to polydopamine nanosheets is 1:0.04 to 1:0.05.
[0021] Furthermore, the swelling time in step (3) is 10 minutes.
[0022] The second object of the present invention is to provide hydrogel microspheres prepared by the above method for capturing and storing free DNA.
[0023] The third object of the present invention is to provide the use of the above hydrogel microspheres in the preparation of a pharmaceutical preparation for reducing the concentration of free DNA.
[0024] A fourth object of the present invention is to provide the use of the above-mentioned hydrogel microspheres in the preparation of anti-inflammatory drugs.
[0025] The fifth object of the present invention is to provide the use of the above-mentioned hydrogel microspheres in the preparation of drugs for promoting the healing of diabetic wounds.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention couples GelMA hydrogel microspheres with polydopamine nanosheets to construct a composite hydrogel microsphere. The π-π stacking / hydrogen bond interaction between the polydopamine nanosheets and the cfDNA bases rich in π-conjugated structure realizes the capture of cfDNA, and the cage-like confined space formed by the methacrylylated gelatin (GelMA) hydrogel polymer network is used to realize the storage of cfDNA. By capturing and storing cfDNA inside the hydrogel microspheres, the cfDNA concentration in the lesion site (diabetic wound) is reduced, thereby specifically blocking the abnormal activation of cfDNA-related Toll-like receptor 9 (TLR9) and its downstream NF-κB signaling pathway in macrophages, reducing the release of inflammatory cytokines and ROS, and then alleviating chronic inflammation of diabetic wounds and promoting wound healing. The composite hydrogel microsphere has excellent biocompatibility, and its cfDNA binding efficiency is not affected by serum proteins. The microspheres can serve as intervention mediators for cfDNA-related proinflammatory signaling pathways, providing a new strategy for cfDNA capture and storage to intervene in cell signal transduction, and providing new insights into the regulatory mechanism between inflammatory mediators and biomaterials in inflammation-related diseases. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the microfluidic preparation of PDA@GM MSs (A) and the capture and storage of cfDNA and the intervention mechanism of pro-inflammatory signals in the diabetic wound model (B).
[0029] Figure 2 Preparation and characterization of PDANSs, GM and PDA@GM MSs; TEM (A) and AFM (B) images of PDANSs; height distribution based on white lines on the selected nanosheets (C) and the corresponding three-dimensional image of image B (D), the inset in image A shows the Tyndall effect of the PDANSs suspension; GelMA solution was prepared into hydrogel microspheres using a microfluidic device, and PDANSs were encapsulated in GM MSs to obtain PDA@GM MSs (E); SEM images of GM MSs and PDA@GM MSs (F) and their corresponding diameter distribution data (G); CLSM image of Cy5-PEG-PDA@GM MSs (Hi), Z-stack layered scanning overlay image and enlarged area image (H-ii), and corresponding 3D image (H-iii); Raman spectra of GM MSs and PDA@GM MSs (I), changes in relative weight over time in a buffer containing collagenase (J) and their representative optical microscope images (K).
[0030] Figure 3 Optical microscope images of GelMA and PDA@GM hydrogel microspheres.
[0031] Figure 4 Characterization of cfDNA binding efficiency and biocompatibility; Binding efficiency of PDANSs to DNA (A), HDF DAMPs DNA (B), and HDF DAMPs RNA (C) at different PDANSs to DNA mass ratios, as well as nucleic acid binding efficiency of GM MSs and PDA@GM MSs (D); Binding efficiency of polyethyleneimine (PEI) to DNA (E), HDF DAMPs DNA (F), and HDF DAMPs RNA (G) at different PEI to DNA mass ratios; Protein adsorption of GM, PDA@GM, and PEI@GM MSs (H); Cytotoxicity of PEI to macrophages (I), proliferation data (J), and live / dead cell distribution of macrophages cultured with different samples for 1, 3, and 5 days (K); Schematic diagram showing the advantages of PDA@GM MSs in capturing cfDNA (L).
[0032] Figure 5 The cytotoxicity of PDANSs at different concentrations on macrophages.
[0033] Figure 6The proliferation of fibroblasts after co-culture with different samples for 1, 3, and 5 days.
[0034] Figure 7 Live / dead cell distribution of fibroblasts after 1, 3, and 5 days of co-culture with different samples.
[0035] Figure 8 Data for the interaction between PDANSs and DNA and the ROS scavenging mechanism; TEM images of PDANSs after interaction with ssDNA and dsDNA, respectively (A); DNA released from PDA NSs / DNA conjugates in urea solution (B); Molecular dynamics model showing typical snapshots of the interaction process between DNA and PDA nanosheets containing ordered and disordered domains, as well as the enlarged final binding conformation (C); The number of π-π stacking (D) and hydrogen bonds (E) between DNA and PDANSs changes with simulation time; DNA storage data (F), ROS scavenging efficiency (G) and cyclic voltammetry curves (H) of GM MSs and PDA@GelMAMSs, and a schematic diagram of cfDNA capture, storage and ROS scavenging mechanism (I).
[0036] Fig. 9 Top view of the initial and final binding configurations of DNA on the PDA nanosheet during the molecular dynamics simulation.
[0037] Fig.10 The effects of PDANSs on DPPH (A), hydroxyl radicals (B) and O2 - Reactive oxygen species scavenging data of free radicals (C).
[0038] Fig.11 DPPH, hydroxyl radicals and O2 - Total catechol contents of PDANSs before and after free radical treatment.
[0039] Fig.12 Capture and storage of free DNA, and intervention of pro-inflammatory signals; fluorescence images of cellular fluorescence signals of CpG DNA, lysosomes and Cy5.5-labeled PDANSs in RAW 264.7 cells (A) and corresponding flow cytometry data (B), scale bar 20μm; fluorescence images showing co-localization of CpG DNA and PDA@GM MSs (C), scale bar 50μm; activation of HEK-Blue hTLR9 (D), hTLR8 (E), and hTLR3 (F) reporter cells before and after FBS treatment, and schematic diagram of hydrogel microspheres inhibiting nucleic acid-induced TLR activation (G), changes in TNF-α (H), IL-6 (I) cytokine levels under different treatment conditions, and cellular ROS fluorescence signals (J), scale bar 200μm.
[0040] Fig.13 Activation of HEK-Blue hTLR4 reporter cells after PDANSs treatment.
[0041] Fig.14 Figure 3 Diabetic wound healing in vivo; Schematic diagram of PDA@GM MSs accelerating wound healing (A); Representative photos of wounds treated with different samples (B) and wound healing rates (C); H&E staining of wound tissue sections (D) and quantitative data of epidermal thickness on day 12 (E); The magnified image shows the interface between hydrogel microspheres and skin tissue (F), and semi-quantitative data of corresponding inflammatory cells in selected areas (G).
[0042] Fig.15 For the evaluation of in vivo anti-inflammatory efficiency; representative immunofluorescence images of macrophage phenotypes in regenerated skin tissue on day 7 (A), immunohistochemical staining of TNF-α, IL-6 (B), IL-10 and TGF-β (C) and corresponding semi-quantitative analysis (DF); macrophages were stained with F4 / 80 (macrophage marker fluorescent substance), iNOS (M1 marker, another fluorescent substance) and CD206 (M2 marker, another fluorescent substance), respectively, scale bar 100 μm. Fig.16 This is a semi-quantitative analysis of the ratio of M1 and M2 macrophages in the regenerated skin tissue on the 7th day.
[0043] Fig.17 Representative immunofluorescence images of DHE in regenerated skin tissue on day 3 (A) and corresponding semi-quantitative analysis (B); scale bar represents 100 μm.
[0044] Fig.18 Masson staining of wound skin tissue sections on days 3 and 7.
[0045] Fig.19 For tissue regeneration assessment; CD31 and α-SMA immunohistochemical staining (B) and quantitative data (CE) of wound skin tissue sections on day 12; the scale bar is 200μm in image A and 100μm in image B.
[0046] Fig. 20 These are histological images of major organs collected on day 12; the scale bar is 200 μm.
[0047] Fig.21 is the binding efficiency of different hydrogel microspheres to DNA in the absence of FBS or in the presence of 10wt% FBS; GMMSs represents GelMA hydrogel microspheres; PDA-GM MSs represents GelMA hydrogel microspheres loaded with PDA nanosheets; GM@PDAMSs represents GelMA hydrogel microspheres covered with a layer of dopamine self-polymerized coating on the surface. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the embodiments. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not used to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still belong to the protection scope of the present invention.
[0049] Example 1
[0050] 1. Experimental Materials and Methods
[0051] 1. Experimental Materials
[0052] Unless otherwise specified, all reagent-grade chemicals were used according to the instructions, and all aqueous solutions were prepared with distilled water. Herring sperm DNA, pig skin gelatin, and Folin phenol reagent were purchased from Sigma-Aldrich. Tris (hydroxymethyl)-aminomethane (Tris, 99.9%), dopamine hydrochloride (AR, 98%), Cy5-PEG-SH (M W =2000Da), urea (AR, 99%), 1,1-diphenyl-2-pyridine hydrazine (DPPH), nitro blue tetrazolium (NBT, 98%), and 2,2'-amino-bis(3-ethylbenzothiazole-6-sulfonic acid) diammonium salt (ABTS) were purchased from Aladdin Industries. Ferrous sulfate heptahydrate (AR), methionine (99%), and riboflavin (98%) were purchased from MACKLIN reagents. HEK-Blue hTLR3, hTLR4, hTLR8, and hTLR9 reporter gene cells, ODN1826FITC, CpG Bw006, Poly(I:C), ORN 06, and LPS were purchased from Invivo Gen. Lysotracker Red, DAPI, Quant-iT PicoGreen dsDNA detection kit, TNF-α, and IL-6 ELISA kits were purchased from Invitrogen. Calcein-AM / PI solution, reactive oxygen species assay kit, enhanced BCA protein assay kit, and cell counting kit-8 (CCK-8) were purchased from Beyotime Biotech (Shanghai, China).
[0053] 2. Characterization methods
[0054] Microstructural studies were performed by transmission electron microscopy (TEM, Talos F200S, ThermoFisher Scientific, The Netherlands), scanning electron microscopy (SEM, Sirion 200, FEI, USA) and atomic force microscopy (AFM, Oxford Instruments, MFP-3D, USA). Raman spectra were obtained using confocal Raman spectroscopy (Renishaw inVia Qontor, UK). UV-visible absorption spectra were obtained using a UV-2600 spectrophotometer (Shimadzu, Japan). Cyclic voltammetry curves were studied using a CHI660D electrochemical workstation. Fluorescence intensity was measured using a multimode microplate reader (BMG LABTECH, Germany). Fluorescence images of cells were obtained using a confocal laser scanning microscope (LSM800, Zeiss).
[0055] 3. Synthesis of hydrogel microspheres encapsulating PDA nanosheets ( Figure 1 A is a schematic diagram of the preparation process. Figure 1 (B) Its mechanism of capturing and storing cfDNA and intervening in pro-inflammatory signals in diabetic wound models
[0056] (1) Preparation of PDA nanosheets (PDANSs)
[0057] Herring sperm DNA (32 mg) and dopamine hydrochloride (32 mg) were added to 16 mL of deionized water, and then 12 mL of Tris solution (50 mM) was added. Stirring was carried out at room temperature for 24 h, and the product was obtained by centrifugation (11000 rpm, 12 min). After ultrasonication for 20 minutes using an ultrasonic cell disruptor (300 W, 50 Hz, working for 3 seconds, alternately pausing for 3 seconds), nano-PDANSs were obtained.
[0058] (2) Preparation of gelatin methacrylate (GelMA) hydrogel microspheres (GM MSs)
[0059] Gelatin (10 g) was dissolved in 100 mL of carbonate buffer solution (pH 9.0) at 50 °C using a microinjection pump at 0.25 mL min. -1 4 mL of methacrylic anhydride (MA) was added at a rate of 1.5 % and protected from light. 50 mL of phosphate buffered saline (PBS) was added to stop the reaction, and then dialyzed with distilled water (molecular weight cutoff: 12-14 kDa) for 3 days. The product was freeze-dried and used for later use.
[0060] Next, GelMA (5wt%) and photoinitiator (0.5wt%) were dissolved in PBS as the aqueous phase (inner layer), and paraffin oil containing 10wt% Span80 was used as the oil phase (outer layer). The aqueous phase and the oil phase were injected into the microfluidic device respectively, and the flow rate was controlled by a microinjection pump. After irradiation with 365nm ultraviolet light for 5min, the emulsion droplets were cross-linked into hydrogel microspheres (MSs). The MSs were collected in a centrifuge tube and the paraffin oil was removed. Wash with acetone and water three to five times to obtain purified hydrogel microspheres. The freeze-dried hydrogel microspheres were suspended in a PDANSs dispersion to prepare hydrogel microspheres encapsulating PDANSs (the final mass ratio of GM MSs to PDANSs was 20:1).
[0061] 4. Biodegradation of hydrogel microspheres
[0062] 10 mg of GM MSs or PDA@GM MSs were suspended in 1 mL of type I collagenase (1 U mL -1 ) in PBS buffer and placed in an incubator at 37°C. The microspheres were dried and weighed at predetermined time points on days 0, 1, 3, 5, 7, 10, and 14. The morphology was observed using an optical microscope, and the residual weight was calculated according to the formula 100×Wt / W0, where Wt is the weight on day t and W0 is the weight on day 0. Three independent experiments were performed for each group of experiments.
[0063] 5. DNA Binding Analysis
[0064] The DNA binding efficiency of the materials was determined according to the instructions of the Quant-iT PicoGreen DNA assay Kit. The repeated freeze-thaw method was used, freezing at -80 °C for 24 h, thawing at room temperature, and vortexing every 10 seconds for a total of 5 cycles. After incubation of different materials at 37 °C for 30 minutes, the cfDNA and cfRNA levels in DAMPs were detected using the Quant-iT PicoGreen DNA or RNA detection kit and the NGSTM RNAHS detection kit (ABP-Biosciences Co., Ltd, Wuhan, Hubei, China).
[0065] 6. Protein adsorption experiment
[0066] GM MSs, PDA@GM MSs and PEI@GM MSs were suspended in 1 mL of bovine serum albumin (BSA) solution and placed in an incubator shaker at 37°C for 30 min. The final concentration of the microspheres was 2 mg mL -1 The final concentration of BSA was 100 μg mL -1 After microsphere precipitation, the supernatant was collected and the protein concentration was determined using an enhanced BCA protein assay kit. MSsCalculate the amount of protein adsorption. Where C0 is the initial concentration of bovine serum albumin (100 μg mL -1 ), C1 is the residual bovine serum albumin concentration in the supernatant, C MSs is the initial concentration of microspheres (2 mg mL -1 ).
[0067] 7. Urea-induced DNA release
[0068] First, PDANSs were suspended in 1 ml of dsDNA (DNA standard) or ssDNA (FITC-CpG) solution (1 μg mL -1 ) and then placed the mixture in an incubator for 12 hours to prepare PDA / DNA conjugates. After centrifugation, the supernatant was collected and the fluorescence intensity of the sample was compared with the standard curve to quantify the DNA concentration in the supernatant. For dsDNA, 1×Picogreen was added and the fluorescence intensity was measured (Ex / Em=488 / 525nm). For ssDNA, the fluorescence intensity of the FITC conjugate was directly measured (Ex / Em=488 / 525nm). The amount of DNA captured by PDANSs was calculated by subtracting the supernatant mass from the total mass of DNA. The PDA / DNA conjugate was then resuspended in HEPES buffer (10mM, pH 7.4) containing 300mM NaCl and 6M urea, stirred at 37°C for 1 hour, and then the supernatant was centrifuged to quantify the released DNA in the supernatant.
[0069] 8. Molecular dynamics simulation
[0070] Atomistic molecular dynamics simulations were performed in the GROMACS (version 2020.6) simulation package. Nucleic acids were modeled using the Amber14SB (OL15) force field refined for DNA, and small molecule (dopamine tetramer) parameters were modeled using the GeneralAmber force field (GAFF2). Water molecules were modeled using the TIP3P water model. The assembly of 800 planar tetramers was first arranged in 2 layers of 14 lines on a surface of about 13×13nm and balanced for 10ns. The equilibrated surface was extended to 9nm along the surface canon to allow the incorporation of core molecules. After inserting 23-base single-stranded DNA and 20-base double-helical DNA molecules about 1.5nm above the surface, more than 65,000 water molecules were added to solvate the entire system, and thousands of steps of energy minimization were performed to remove close contacts. At a concentration of 0.1M, 235 sodium ions and 156 chloride ions were added to neutralize the charge of the entire system by randomly replacing water molecules. After 20 ns of equilibration under the NPT system, it was extended for another 100 ns under the conventional system. The temperature was coupled to 310 K using the Nose-Hoover method, and the pressure was coupled to 1 atm using the Parrinello-Rahman method. A cutoff of 1.2 nm was used for non-bonded interactions, and the Particle Mesh Ewald method with a Fourier spacing of 0.1 nm was used for long-range electrostatic interactions. All covalent bonds to hydrogen atoms were constrained using the LINCS algorithm.
[0071] 9. DNA storage capacity
[0072] Similar to the urea-induced DNA release experiment, GM / DNA or PDA@GM / DNA conjugates were first prepared and the captured DNA concentration was determined. Afterwards, the GM / DNA or PDA@GM / DNA conjugates were resuspended in fresh TE buffer and 100 μL of the supernatant was taken on day 14 to determine the released DNA. The amount of stored DNA was calculated by subtracting the mass in the supernatant from the captured DNA.
[0073] 10. Active oxygen scavenging ability
[0074] Evaluate the samples' resistance to DPPH free radicals, superoxide anions (O2 - ) and hydroxyl radical (·OH) scavenging ability. In the experiment of scavenging DPPH free radicals, different concentrations of PDANSs or microspheres were suspended in DPPH solution (50 μg·mL -1 , anhydrous ethanol) and incubated on a shaker for 20 minutes in the dark. After centrifugation for 5 minutes, the UV-Vis absorbance of the supernatant was measured at 515 nm. The photoreduction inhibition rate of NBT was recorded to investigate its ability to scavenge O2 -activity. First, methionine (12.5mM), NBT (75μM) and riboflavin (20μM) solutions were prepared respectively. PDANSs or microspheres of different concentrations were suspended in 800μL PBS buffer, and methionine (70μL), NBT (70μL) and riboflavin (70μL) were added in sequence. After ultraviolet irradiation for 10min, the UV-visible absorbance at 560nm was measured to evaluate its antioxidant activity. The mixture without material was used as a positive control, and the mixture without material and ultraviolet irradiation was used as a negative control. ABTs were used to detect the ·OH free radical scavenging activity of the samples. First, 10 μL H2O2 (200 μM) and 20 μL FeSO4·7H2O (18 mM) were added to 920 μL PDANSs or microsphere suspensions of different concentrations in sequence; ultrasonic treatment was performed for 5 min, and the supernatant collected by centrifugation was incubated with 50 μL ABTs (10 μM) for 3 to 5 min, and the UV-visible absorbance at 800 nm was recorded. ABTs solution was used as a negative control.
[0075] 11. Electrochemical measurement
[0076] The electrochemical properties of the samples were studied using a three-electrode cell consisting of a working electrode, a platinum counter electrode, and a silver / silver chloride reference electrode. The PDANSs dispersion before and after the reaction with active oxygen was dropped onto a glassy carbon electrode (GCE) and dried at room temperature as the working electrode. The CHI760E electrochemical workstation was used at a scan rate of 0.05 V s -1 The cyclic voltammetry curves were measured.
[0077] 12. Determination of Catechol Content
[0078] The catechol content of PDANSs before and after the reaction with ROS was determined by Folin-Ciocalteu colorimetry. 0.125 mL of Folin-Ciocalteu reagent was added to 1.5 mL of the suspension containing PDANSs. After incubation for 4 min, 0.875 mL of anhydrous sodium carbonate solution (20.0% w / v) was added and incubated in the dark at room temperature for 1 h. The solution was then analyzed for absorbance spectroscopy using a UV-visible spectrometer. A calibration curve was generated using gallic acid as the standard molecule.
[0079] 13. Cell culture
[0080] Raw 264.7, HEK-BlueTM hTLR reporter cells and human dermal fibroblast (HDF) cells purchased from ATCC were cultured in medium containing 10 wt% FBS, streptomycin (100 units mL -1 ) and penicillin (100 units mL -1 ) in growth medium (DMEM high glucose) at 37°C in a humidified atmosphere containing 5% CO2 in the air.
[0081] 14. Biocompatibility
[0082] The cell counting kit-8 (CCK-8) assay method was as follows: RAW 264.7 cells were seeded in a 96-well plate at a density of 5000 cells per well and cultured for 24 h. -1 ) or PEI (0-12 μg mL -1 ) was replaced with fresh medium. After incubation for 24 h, the cells were incubated with fresh medium containing 10% CCK-8 for 1-2 h. The OD value at 450 nm was recorded using a microplate reader. The cell proliferation experiment was similar to the CCK-8 experiment. RAW 264.7 or L929 cells were seeded in a 96-well plate at a density of 1000 cells per well and cultured overnight. The culture medium was carefully replaced with a medium containing PDANSs (100 μg mL -1 )、GM MSs(2mg·mL -1 ) or PDA@GM MSs (2 mg mL -1 ,PDANSs equivalent concentration is 100 μg·mL -1 ) fresh medium, after incubation for 1, 3, and 5 days, the cells were incubated with medium containing 10% fresh CCK-8 for 1-2 h, and the OD value at 450 nm was recorded using a microplate reader. Live / dead staining was performed as follows: RAW 264.7 or L929 were seeded in 96-well plates at a density of 10,000 cells per well and cultured overnight. The culture medium was carefully replaced with PDANSs (100 μg mL -1 )、GM MSs(2mg·mL -1 ) or PDA@GM MSs (2 mg mL -1 ,PDANSs equivalent concentration is 100 μg·mL -1 ) in fresh culture medium, incubated for 1, 3, and 5 days, and then incubated with calcein-AM and propidium iodide solution for 10 min and observed under a fluorescence microscope.
[0083] 15. In vitro TLR activation assay
[0084] HEK-Blue TM hTLR3, hTLR4, hTLR8, and hTLR9 reporter cell lines were cultured in DMEM supplemented with 10 wt% bovine serum and 1 wt% penicillin-streptomycin. To inhibit the activation of TLR9, 8, 3, and 4 by the materials, 8 × 10 4 , 4×10 4 , 5×10 4 and 2.5×10 4HEK-Blue hTLRs reporter cells were seeded in 96-well plates in DMEM with or without 10 wt% FBS for 30 min, and then 2 μL of 1 μg mL -1 CpGBW006, ORN 06 and Poly(I:C)(LMW) or 10 μg mL -1 lipopolysaccharide (LPS) was added to the cells, and then the materials (PDANSs, GM MSs or PDA@GM MSs) were added in a final volume of 200 μL. After incubation for 24 h, 50 μL of the supernatant was collected and incubated with 150 μL of QUANTI-Blue solution. The OD value at 620 nm was measured using a microplate reader to determine the embryonic alkaline phosphatase (SEAP) activity in each well.
[0085] 16. Cellular localization of cfDNA
[0086] RAW 264.7 cells were initially cultured on 24-well confocal slides at a density of 2 × 10 4 After 24 h, FITC-labeled CpG (1 μg mL -1 ) and Cy5-PDANSs (100 μg mL -1 )、GM MSs(2mg·mL -1 ) or Cy5-PDA@GM MSs (2 mg mL -1 , the equivalent concentration of Cy5-PDANSs is 100 μg·mL -1 After 24 h of incubation, the supernatant was discarded and the cells were washed three times with PBS. TM Red medium and incubated for 15 minutes. The cells were then washed and fixed with 4wt% paraformaldehyde for 30 minutes at room temperature. The nuclei were stained with 1×DAPI and the membrane was then sealed with neutral glue. Images were taken using a confocal laser scanning microscope.
[0087] 17. Flow cytometry
[0088] RAW 264.7 cells were used to detect the inhibitory effect of materials (PDANSs, GM MSs or PDA@GM MSs) on CpG DNA endocytosis. Briefly, cells were seeded in 24-well plates, and after the cells grew to 70-80%, FITC-labeled CpG DNA (1 μg mL -1 ), and PDANSs (100 μg mL -1 )、GM MSs(2mg·mL -1 ) or Cy5-PDA@GM MSs (2 mg mL -1, the equivalent concentration of Cy5-PDANSs is 100 μg·mL -1 After incubation for 24 h, the cells were harvested and the cell fluorescence intensity of FITC-CpG was detected by flow cytometry (MoFlo XDP, Beckman, USA).
[0089] 18. Intracellular ROS detection
[0090] RAW 264.7 cells were plated at 1.5 × 10 5 The cells were inoculated at a density of 1000 cells / mL in a 6-well plate and left overnight. 1.5 mL of the cell culture medium was replaced with fresh DMEM high glucose containing Rosup or Rosup containing materials (PDANSs, GM MSs or PDA@GM MSs). After incubation for another 6 h, the culture medium was completely removed and the fluorescent probe DCFH-DA was added. The fluorescence signal (Ex / Em=488 / 525 nm) was detected using a confocal laser scanning microscope to evaluate the intracellular ROS level.
[0091] 19. Expression of inflammatory factors in vitro
[0092] In order to study the inhibitory effect of materials (PDANSs, GM MSs or PDA@GM MSs) on the immunostimulatory effect induced by CpG DNA, 2×10 5 RAW 264.7 cells were seeded in 24-well plates and 1 μg mL -1 CpG DNA and different concentrations of materials (PDANSs, GM MSs or PDA@GM MSs) were added. After 24 h of incubation, the supernatant was collected and the concentrations of TNF-α and IL-6 were detected using the corresponding ELISA kits.
[0093] 20. Establishment of diabetic wound and in vivo experiments
[0094] All animal operations were approved by the Animal Ethics Committee of Ruijin Hospital, Shanghai Jiao Tong University School of Medicine (SYXK 018-0027). Eight-week-old male C57 rats were selected for the experiment. 1 wt% streptozotocin (STZ, 55 mg kg -1) was injected intravenously to establish a type Ⅰ diabetes model. Blood glucose levels were detected one week later, and rats with blood glucose levels higher than 16.7 mM, weight loss, polyuria, and polydipsia were considered diabetic rats. Two circular full-thickness skin defects with a diameter of 6 mm were made on the back of each diabetic rat, and the rats were randomly divided into 4 groups and treated with PDA NSs, GM MSs, PDA@GM MSs, and saline (control group). The wound healing was observed and recorded with a digital camera at 0, 3, 7, and 12 days after surgery. The formula for calculating the wound healing rate was: (A0-At) / A0×100%, where A0 and At represent the initial wound area and residual wound area at each time point, respectively.
[0095] 21. Evaluation of Inflammation Regulation and Wound Healing in Vivo
[0096] The harvested specimens were fixed in 4wt% PFA for 24h and then embedded in paraffin sections for histological and immunohistochemical staining, including H&E and Masson trichrome staining, immunofluorescence staining of iNOS, CD206 and DHE, and immunohistochemical staining of TNF-α, IL-6, CD31, α-SMA, IL-10 and TGF-β. Detailed operations were performed according to the manufacturer's instructions.
[0097] 22. Statistical analysis
[0098] Quantitative data were expressed as mean ± SD and analyzed by independent sample t test or one-way ANOVA with Tukey post hoc test; p value < 0.05 was considered statistically significant (*P < 0.05, **P < 0.01, ***P < 0.001, ****P < 0.0001).
[0099] 2. Experimental Results
[0100] 1. Preparation and characterization of composite hydrogel microspheres
[0101] The composite hydrogel microspheres are encapsulated by two-dimensional polydopamine nanosheets, and porous hydrogel microspheres (GelMAMSs) serve as capture and storage modules, respectively. Polydopamine nanosheets (PDANSs) are prepared by DNA-directed polymerization and assembly of dopamine.
[0102] By transmission electron microscopy (TEM, Figure 2 AFM (center A) and atomic force microscopy (AFM, Figure 2 (B) The morphology of PDANSs was characterized and it was found that their lateral dimensions were mainly within 500 nm, which is nanoscale. The typical Tyndall light scattering effect also shows that the nanoscale size ( Figure 2 AFM images, height distribution analysis, and corresponding 3D images also observed that the thickness was in the range of 5-25 nm, and the surface was rough with small protrusions ( Figure 2(in BD).
[0103] Although PDANSs may have the ability to capture cfDNA, the subsequent fate of cfDNA remains uncontrollable. Therefore, it may be a reasonable choice to use polymer networks to limit the uncontrollable shedding of cfDNA captured from PDANSs. Although this can also be achieved by using bulk hydrogels, spherical hydrogel microspheres with macroporous structures have larger active areas, allowing cfDNA to enter the hydrogel microspheres more efficiently. GelMA hydrogel microspheres were prepared using a microfluidic device ( Figure 2 (E) GelMA solution was used as the dispersed phase (inner channel) and 10% Span 80 in paraffin oil was used as the continuous phase (outer channel). Emulsion droplets were formed under the shearing action of the continuous phase, and cross-linked microspheres were obtained under subsequent UV irradiation. Freeze-dried GelMAMSs were swollen in the PDANSs suspension to encapsulate PDANSs (PDA@GM MSs). Figure 2 F, G and Figure 3 In the 2D images, a uniformly sized monodisperse sphere was observed. The average diameter of PDA@GM MSs was slightly reduced to 218 μm compared to the diameter of GelMA (228 μm), which may be due to the hydrogen bonding interaction between PDA NSs and GelMA. Scanning electron microscopy (SEM) showed that both GM MSs and PDA@GM MSs clearly had macroporous structures with diameters of tens of microns, which may be beneficial to improve the capture of cfDNA.
[0104] In addition, some flake structures were observed on the surface of PDA@GM MSs ( Figure 2 F), the microspheres clearly show the punctate fluorescence signals of Cy5-PEG-labeled PDANSs ( Figure 2 H), indicating that PDANSs were encapsulated. The encapsulated PDANSs hydrogel microspheres maintained a spherical shape, and the nanosheets were mainly gathered on the surface of the hydrogel microspheres, with a depth of up to 47.2 μm ( Figure 2 Middle H). Figure 2 Figure I shows the Raman spectra collected by PDA@GM MSs, PDANSs, and GM MSs. Typical D (disordered carbon, 1350-1534 cm -1 ) and G (graphite carbon, 1540~1833cm -1 ) peak, and a broad 2D (2580-3200cm -1 ) peaks, which are common in PDA materials or other carbonaceous materials. In addition, it was observed that the ID / IG ratio of PDANSs was very low, about 0.81, indicating the presence of short-range order and graphite-like carbon structure. Unlike GM MSs, which have no obvious characteristic peaks, D and G peaks appeared in the Raman spectrum of PDA@GM MSs, which also indicated that PDANSs were successfully encapsulated.
[0105] like Figure 2 As shown in Figure 1, on the 14th day, the degradation rate of GM MSs was slightly faster than that of PDA@GM MSs (relative weight retention was greater than 60% at 14 days). The structure and morphology of PDA@GM MSs were also maintained for at least 14 days ( Figure 2 Middle K). The interaction between PDANSs and the GelMA polymer network can retard the degradation of PDA@GM MSs, which may help maintain the structure of the hydrogel microspheres and the sustained efficiency of cfDNA capture and storage.
[0106] 2. cfDNA capture efficiency and biocompatibility
[0107] To explore whether nanosheets and hydrogel microspheres can capture cfDNA, a competitive binding experiment was first performed. PDANSs showed excellent DNA binding ability, which was positively correlated with the mass ratio of nanosheets to DNA ( Figure 4 Similar trends were observed in the data from HDFDAMPs DNA and RNA binding experiments ( Figure 4 In addition, the PDA@GM MSs group has a higher DNA binding efficiency compared with the original GM MSs, while the DNA binding ability of the original GM MSs is negligible ( Figure 4 (middle D).
[0108] Studies have shown that positively charged cationic polymers can effectively bind cfDNA with polyanionic characteristics through electrostatic interactions. W =10,000). Even at low PEI / DNA mass ratios of 1.5-12, good nucleic acid binding affinity was observed ( Figure 4 However, in the presence of 10wt% FBS, the nucleic acid binding ability of PEI decreased significantly, which may be related to the electrostatic adsorption of negatively charged serum proteins. In contrast, the difference in nucleic acid binding ability of PDANSs or PDA@GM MSs with or without FBS was negligible. In addition, protein adsorption experiments showed that PDA@GM MSs (17.7%) and GM MSs (22.6%) had protein resistance-like characteristics, while PEI-loaded hydrogel microspheres had a higher adsorption of bovine serum albumin (94.1%) ( Figure 4 Middle H).
[0109] In most cases, negatively charged materials are considered to be less cytotoxic than positively charged materials, and the micrometer-sized hydrogel microspheres may hinder cellular uptake, which may help biocompatibility.-1 When , significant cytotoxicity was observed, with cell viability inhibited by 44.8%, which may hinder further applications ( Figure 4 In contrast, even at 200 μg mL -1 Even at high concentrations, PDANSs had no significant in vitro toxicity to macrophages ( Figure 5 ).
[0110] Macrophages and fibroblasts were co-cultured with PDANSs, GM MSs, and PDA@GM MSs, respectively. Over time, macrophages and fibroblasts proliferated rapidly, as confirmed by CCK-8 data and fluorescent images of cells stained with Calcein-AM / PI solution ( Figure 4 J, K and Figure 6 , Figure 7 ). The number of cells in each group increased, and the number of dead cells was negligible, indicating high biocompatibility.
[0111] These findings suggest that PDA@GM MSs have certain advantages in cfDNA capture, namely, efficient DNA binding ability, negligible nonspecific protein adsorption, and high biocompatibility ( Figure 4 This suggests that it has the potential for further clinical application.
[0112] 3. Mechanisms of cfDNA capture and storage, and reactive oxygen species scavenging properties
[0113] In order to better understand the mechanism of cfDNA capture, we first observed the morphology of PDANSs after binding to cfDNA using single-stranded DNA (ssDNA, CpG1826) and double-stranded DNA (dsDNA, λDNA). There was no obvious change in the two-dimensional morphology, suggesting that DNA molecules may be adsorbed on the surface of PDANSs, rather than PDANSs embedding DNA inside in the form of folding and wrinkling ( Figure 8 (A).
[0114] Next, urea, which can destroy hydrogen bonds, was used to explore the interaction between PDANSs and DNA molecules. PDANSs / ssDNA or PDANSs / dsDNA conjugates were suspended in urea solution for 60 minutes, releasing about 17.5% of ssDNA and 4.4% of dsDNA, respectively. Figure 8 These results suggest that the hydrogen bonding ratio in PDA NSs / ssDNA may be higher than that in PDANSs / dsDNA conjugates. We then proposed a hypothesis that dsDNA molecules rely more on π-π interactions on the surface of PDANSs than ssDNA molecules.
[0115] To further confirm this hypothesis, all-atom molecular dynamics (MD) simulations were performed to explore the interaction between DNA and PDANSs. A model of a PDA nanosheet was built by assembling the tetramers 13 × 13 nm above the surface and then inserting model ssDNA and dsDNA molecules approximately 1.5 nm above the surface. The interaction was tested for 100 ns after equilibration for 20 ns. Figure 8 Middle C and Fig. 9 The side view of the DNA molecule at 0, 10, 40, and 100 ns, the top view of the initial and final binding configurations, and the zoomed-in configuration (100 ns) are shown. The number of hydrogen bonds and π-π stacking interactions during the process was further counted. For ssDNA, less than 10 hydrogen bonds were initially formed. After 60 ns, the number of hydrogen bonds increased to 5 to 15 ( Figure 8 At the same time, the number of π-π stacking interactions increases steadily, reaching about 10 ( Figure 8 For dsDNA, less than five π-π stacking interactions were initially observed, which rapidly increased to 6 to 7 after 40 ns ( Figure 8 D). However, the hydrogen bonding that occurs is negligible ( Figure 8 (E) This simple model shows that the way and main driving force of PDANS capturing ssDNA and dsDNA are different. ssDNA tends to interact with PDANS through hydrogen bonding and π-π stacking interactions, although it will bend and deform in the process. On the other hand, dsDNA utilizes the base pairs at the ends, and its main driving force is π-π stacking, which may be due to the fact that most base pairs are hidden in the middle of the double helix.
[0116] The cfDNA storage capacity of PDA@GM MSs was then studied. The cfDNA released into the buffer by PDA@GM MSs / DNA or GM MSs / DNA conjugates after 14 days was measured, and the cfDNA stored in the microspheres was further calculated. -1 ssDNA and 0.12 g mg -1 dsDNA, while GM MSs contain about 0.11 g·mg -1 of ssDNA and almost no dsDNA ( Figure 8 (F) These results indicate that PDA@GM MSs have the ability to capture and store cfDNA. It is worth noting that a certain amount of ssDNA is stored in GM MSs, which may be due to the long-term interaction between the side-exposed DNA base pairs and the polymer chains in GelMA through hydrogen bonds.
[0117] Next, a DPPH free radical scavenging assay was performed to evaluate the antioxidant activity of PDANSs. Fig.10 As shown, PDA nanosheets have a dose-dependent DPPH scavenging activity, 25 μg mL -1 In addition, PDANSs showed a high clearance of O2 - The ability to scavenge various ROS such as ·OH and ·OH indicates that it has excellent antioxidant capacity when applied in inflammatory microenvironments. In addition, encapsulation of PDANSs in hydrogel microspheres also showed excellent ROS scavenging ability ( Figure 8 In G, the equivalent concentration of PDANSs is 100 μg mL -1 ), indicating that the encapsulation of PDANSs in GelMA hydrogel microspheres had little effect on the ROS scavenging efficiency of PDANSs.
[0118] like Figure 8 As shown in H, with DPPH, ·OH and O2 - After the treatment, the oxidation potential of PDANSs shifted positively from 0.23 V to 0.72, 0.70, and 0.35 V, respectively, indicating a decrease in electron-donating ability. In addition, compared with the original PDANSs, the catechol concentrations after ROS removal were reduced by 73.9%, 18.8%, and 14.3%, respectively ( Fig.11 ), indicating that catechol consumption is required for scavenging ROS.
[0119] In summary, PDANSs play an important role in cfDNA capture based on hydrogen bonding and π-π stacking interactions and ROS scavenging based on H atom / electron transfer. The mechanism of cfDNA capture and storage and the antioxidant properties of PDA@GM MSs are shown in Figure 2. Figure 8 As shown in I.
[0120] 4. In vitro cfDNA binding and intervention of cfDNA pro-inflammatory signal transduction
[0121] After figuring out the mechanism of cfDNA capture and storage, we then studied how the microspheres functioned inside cells. We used RAW 264.7 cells for intracellular validation, co-cultured the cells with FITC-CpG DNA and three materials (Cy5-PDANSs, GM MSs, or Cy5-PDA@GM MSs), and observed the location of FITC-CpG DNA, Cy5-PDANSs, or Cy5-PDA@GM MSs, and lysosomes (labeled with lysosome-specific fluorescent dyes). Fig.12(A). When CpG DNA was co-cultured with cells alone, it was mainly distributed in lysosomes and nuclei. When CpG DNA and PDANSs were co-cultured with cells, co-localization signals of CpG DNA and PDANSs in lysosomes were observed. In addition, after the addition of PDA@GM MSs, the fluorescence signal of FITC-CpG DNA almost disappeared, which may be due to the capture of DNA molecules by PDA@GM MSs, while PDA@GM MSs cannot be taken up by cells, so the fluorescence signal in cells almost disappeared. The fluorescence signal of FITC-CpG DNA in the GM MSs treatment group was slightly weakened, which may be due to the physical adsorption of DNA by the polymer network of hydrogel microspheres.
[0122] Fig.12 Figure B shows the flow cytometry data of the cellular signal of endocytosed CpG DNA. The fluorescence intensity of the CpG DNA-treated group was the highest, indicating that the CpG DNA was effectively internalized. The GM MSs-treated group had a high fluorescence intensity, indicating that the DNA binding ability was negligible. In the PDA@GM MSs-treated group, the fluorescence intensity was significantly reduced, indicating a high DNA capture efficiency. Two peaks appeared in the PDA NSs group, which may be because part of the DNA / PDANSs conjugate was internalized. PDA@GM MSs were collected after co-culture with cells. Due to the fluorescence quenching properties of the contacting PDANSs, some weak fluorescence signals were observed at the edge of the PDA@GM MSs, co-localized with the fluorescence signal of Cy5-PDANSs ( Fig.12 Middle C), showing that CpG-DNA is captured and stored in the hydrogel microspheres.
[0123] Encouraged by the excellent cfDNA capture and storage capabilities, we then investigated whether PDA@GM MSs could block the pro-inflammatory signaling of cfDNA. HEK-blue human TLRs (hTLRs) cells were constructed using HEK 293 cells co-transfected with the hTLRs gene and the optimized embryonic alkaline phosphatase (SEAP) reporter gene, which was controlled by the IFN-β minimal promoter and fused with five NF-κB and AP-1 binding sites. cfDNA (as a TLR agonist) activated NF-κB and AP-1, leading to SEAP expression, thereby monitoring the downstream activation of NF-κB. GM MSs had negligible effects on the TLRs pathway, while PDA NSs and PDA@GMMSs had a significant inhibitory effect on CpG-induced hTLR9 activation ( Fig.12 D), FBS had no obvious negative effect on it. Similar phenomenon was observed in hTLR8 induced by ORN 06 and hTLR3 induced by Poly(I:C) ( Fig.12 In addition, LPS-induced hTLR4 cell activation was not inhibited ( Fig.13 ), suggesting that it specifically blocked nucleic acid-induced TLR and subsequent NF-κB activation ( Fig.12 Middle G).
[0124] After co-culture with CpG DNA, the transcriptional expressions of tumor necrosis factor-α (TNF-α) and interleukin-6 (IL-6) in macrophages were significantly increased, while the addition of PDANSs or PDA@GM MSs significantly decreased them, demonstrating that they have a good anti-inflammatory effect ( Fig.12 In addition, the ROS level in Rosup-stimulated macrophages was also decreased when co-cultured with PDANSs or PDA@GM MSs, indicating that it has the ability to assist in the scavenging of ROS and contributes to the anti-inflammatory effect ( Fig.12 (in Chinese).
[0125] 5. Chronic wound healing
[0126] Based on the excellent cfDNA capture and intervention of pro-inflammatory signal transduction of cfDNA, a diabetic full-thickness wound model was established as a chronic model to evaluate the feasibility of PDA@GM MSs in regulating inflammation in vivo ( Fig.14 (A).
[0127] First, the wound contraction of different groups was recorded to evaluate the healing process of full-thickness skin wounds. The wound size of each group became smaller, but the healing process of the wound treated with PDA@GM MSs was significantly faster than that of the other groups ( Fig.14 Middle B). Based on the wound surface images, the wound shrinkage rate of the PDA@GM MSs group was 33.2% after 3 days of treatment, which was significantly higher than that of the control group. On the 12th day, 98.3% of the wounds in the PDA@GM MSs group were healed ( Fig.14 Middle C).
[0128] In experiments using other cationic hydrogels (such as PAM) to adsorb cfDNA through electrostatic adsorption, the wound healing time took 14 days.
[0129] It is worth noting that although the wounds in the other groups also seemed to be almost healed on the 12th day, the internal structure and condition of the healed wounds were different. Fig.14As shown in D, H&E staining was used to evaluate the histopathological structure of the regenerated skin tissue. The wounds treated with PDA@GM MSs had the best healing. On the 3rd day, the wound thickness in the PDANSs group, GM MSs group, and PDA@GM MSs group was significantly greater than that in the control group, and no obvious inflammatory response was observed in all wounds. On the 7th day, the wound thickness increased in each group, and inflammatory cells infiltrated. However, in the PDA NSs group and PDA@GM MSs group, the vascular density increased significantly, and an appropriate level of inflammatory response is essential for tissue reconstruction. On the 12th day, the wound healed and the epidermis regenerated. The PDA@GM MSs group formed a relatively complete epidermis and mature dermis structure, and its histopathological structure was similar to that of normal skin tissue. The epidermal thickness of the PDA@GM MSs-treated wound ( Fig.14 Middle (E) is approximately 43.0 μm, which is much smaller than the control group (95.6 μm), PDA NSs group (95.0 μm) and GM MSs group (58.5 μm), and is closest to normal skin tissue (13.5 μm).
[0130] As a good wound dressing, its basic function is to support and protect the wound. Therefore, proper bioadhesion and tissue integration are essential. GM MSs seemed to provide poor tissue integration, as cracks appeared between GM MSs and skin tissue on day 3 ( Fig.14 Interestingly, a seamless interface was observed between PDA@GM MSs and the surrounding tissue ( Fig.14 F, bottom), which may be due to the hydrogen bonding interaction between PDA@GM MSs and the endogenous lysine and glutamine residues of the surrounding tissue. In addition, H&E staining showed that a small number of immune cells were displayed in PDA@GM MSs and their surrounding tissues, while the aggregation of immune cells was observed at the interface of skin tissue and GM MSs, and the number of immune cells was about 4 times that of the PDA@GM MSs group ( Fig.14 These results indicate that the inflammatory response of wound tissue to PDA@GM MSs was significantly lower.
[0131] 6. Inflammation regulation and tissue regeneration
[0132] Chronic inflammation is the main problem that hinders wound healing. The expression of pro-inflammatory and anti-inflammatory cytokines, the phenotype of macrophages infiltrating the injured site, and the level of ROS are important indicators of inflammatory response. The immunofluorescence marker F4 / 80 of macrophages, the surface marker iNOS of pro-inflammatory M1 macrophages, and the surface marker CD206 of anti-inflammatory M2 macrophages were selected to study the infiltration and phenotype of macrophages. Fig.15 A, D and Fig.16As shown in Figure 3, the proportion of M1 macrophages in the wounds treated with PDA@GM MSs was extremely low and the proportion of M2 macrophages was high compared with the control group. Similarly, the M1 / M2 ratio of PDA@GM MSs was the lowest, followed by PDAMSs and GM MSs.
[0133] In addition, the expressions of TNF-α and IL-6 were significantly downregulated in the wounds treated with PDA@GM MSs compared with the other groups, indicating a decrease in inflammatory cell infiltration ( Fig.15 The expressions of anti-inflammatory IL-10 and transforming growth factor-β (TGF-β) in the PDA@GM MSs group were significantly higher than those in the control group or the PDANSs and GM MSs groups ( Fig.15 In addition, high levels of ROS were observed in the control group and GM MSs, which may be due to the production of ROS induced by inflammatory response. In contrast, the ROS level in the PDANSs group was relatively low, and the ROS signal in the PDA@GM MSs group was negligible ( Fig.17 ), which may benefit from the tissue integration of PDA@GM MSs and thus enable persistent scavenging of ROS compared with PDANSs.
[0134] Collagen deposition and angiogenesis are crucial for wound healing and tissue remodeling. Fig.18 , Fig.19 As shown in A and C, collagen fibers were scarce in each group on the third day, and collagen deposition in each group gradually increased over time. On the 12th day, the PDA@GM MSs group had the highest collagen deposition content, followed by the GM MSs group, the PDA NSs group, and the control group. The PDA@GM MSs-treated group had significant dermal vascular density, and the levels of anti-CD31 and α-SMA antibodies were higher, indicating that transmembrane proteins were expressed in the early stage of angiogenesis and cytoplasmic proteins were expressed in the late stage of angiogenesis ( Fig.19 This result is also consistent with the relatively high proportion of M2 macrophages observed in the PDA@GM MSs group. In addition, compared with the control group, no obvious pathological necrosis was observed in the heart, liver, spleen, lung, kidney and other major organs after slices of PDANSs, GM MSs and PDA@GM MSs ( Fig. 20 ), indicating that it is biosafe as a wound repair material.
[0135] In summary, PDA@GM MSs can significantly reduce inflammatory response, promote collagen deposition and angiogenesis, and thus accelerate diabetic wound healing and tissue regeneration.
[0136] Conclusion
[0137] The present invention develops a composite hydrogel microsphere as an intervention medium for cfDNA-related proinflammatory signaling pathways to prevent the malignant interaction between cfDNA and immune cells. Composite hydrogel microspheres are prepared by coupling PDANSs with GelMA hydrogel microspheres. This cfDNA capture strategy based on π-π stacking / hydrogen bonding between PDANS and cfDNA π-rich bases achieves high binding efficiency of cfDNA without being affected by electronegative molecules such as serum proteins. The storage of cfDNA is achieved through the cage-like confined space created by the polymer network of the hydrogel microspheres, which can clarify the fate of the captured cfDNA, that is, it falls off with the hydrogel microspheres during wound healing instead of being uncontrollably released in the body and inducing inflammatory response again. After the concentration of cfDNA is reduced, it can specifically inhibit TLR9 and its downstream NF-κB pathway, significantly reduce the expression of inflammatory factors, and thus reduce chronic inflammation of diabetic wounds. PDANSs can also remove excessive ROS, which helps to optimize the inflammatory microenvironment. The present invention provides a new perspective for exploring the regulatory strategies of key inflammatory mediators and the intervention of pro-inflammatory signals, thereby demonstrating the great potential of biomaterials that regulate chronic inflammation in the treatment of other inflammatory diseases.
[0138] Comparative Example 1
[0139] According to the method of Example 1, a layer of dopamine self-polymerization coating was covered on the surface of GelMA hydrogel microspheres to prepare composite hydrogel microspheres, which were then used to capture cfDNA. The results are shown in Fig.21 .
[0140] Fig.21 The results show that after dopamine is self-polymerized on the surface of GelMA hydrogel microspheres to form a coating, the microspheres can still show a certain DNA binding ability, but compared with the hydrogel microspheres loaded with PDA nanosheets, their DNA binding efficiency is significantly reduced, only 24.2% (10wt% FBS) and 33% (no FBS) under the same conditions. The reason may be that compared with PDA nanosheets, the dopamine oligomers in the PDA self-polymerized coating have a higher degree of disorder in the plane arrangement and do not have a two-dimensional structure, which leads to insufficient exposure of the overall π-conjugated plane. The π-π stacking effect between the π-conjugated plane of PDA and the DNA base plane realizes the DNA adsorption effect, while the electrostatic repulsion between the negatively charged phosphate groups on the side of double-stranded DNA and the negatively charged PDA (when pH is greater than 4) leads to the desorption effect of DNA from the PDA nanostructure. Therefore, if the overall π-conjugated plane of the PDA structure is insufficiently exposed, the adsorption effect on DNA is less than the desorption effect, which ultimately leads to a decrease in DNA binding efficiency.
Claims
1. A method for preparing hydrogel microspheres for capturing and storing free DNA, characterized in that: The following steps are involved: (1) preparing polydopamine nanosheets; (2) Preparation of GelMA hydrogel microspheres using a microfluidic device; (3) The freeze-dried GelMA hydrogel microspheres are swelled in a polydopamine nanosheet suspension to prepare GelMA hydrogel microspheres encapsulating polydopamine nanosheets.
2. The preparation method according to claim 1, characterized in that: The preparation method of the polydopamine nanosheets in step (1) is as follows: uniformly mixing the herring sperm DNA solution and the dopamine hydrochloride solution, then adding the tris(hydroxymethyl)aminomethane) solution, reacting at room temperature for 24 hours under stirring conditions, centrifuging and discarding the supernatant to obtain a nanosheet product, namely the polydopamine nanosheets.
3. The preparation method according to claim 2, characterized in that: The concentration ratio of the herring sperm DNA solution, the dopamine hydrochloride solution and the tris(hydroxymethyl)aminomethane solution is 2:4:
3.
4. The preparation method according to claim 1, characterized in that: In step (2), GelMA solution is used as the dispersed phase, and liquid paraffin containing 10 wt % of Span 80 is used as the continuous phase, and then GelMA hydrogel microspheres are prepared by photocrosslinking.
5. The preparation method according to claim 1, characterized in that: In step (3), the weight ratio of GelMA hydrogel microspheres to polydopamine nanosheets is 1:0.04 to 1:0.
05.
6. The preparation method according to claim 1, characterized in that: The swelling time in step (3) is 10 min.
7. Hydrogel microspheres for capturing and storing free DNA prepared by the method according to any one of claims 1 to 6.
8. Use of the hydrogel microspheres according to claim 7 in preparing a pharmaceutical preparation for reducing the concentration of free DNA.
9. Use of the hydrogel microspheres according to claim 7 in the preparation of anti-inflammatory drugs.
10. Use of the hydrogel microspheres according to claim 7 in the preparation of a drug for promoting healing of diabetic wounds.
Citation Information
Cited By
Preparation method and application of resveratrol nanocrystal-loaded GelMA Cryogel microspheres
CN119033705A
Modified montmorillonite nanosheet capable of being used as cfDNA scavenger as well as preparation method and application of modified montmorillonite nanosheet