Preparation method and application of dynamic carbon layer coated bimetallic copper-based catalyst

Through the dynamic carbon layer-coated bimetallic copper-based catalyst technology, the problems of instability and reduced selectivity of the synthesis gas-to-lower alcohol catalyst are solved, achieving high selectivity and high yield of low-carbon alcohol generation, and extending the catalyst life. , and reduce costs.

CN118744004APending Publication Date: 2024-10-08XIAMEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410727261.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing synthesis gas-to-lower alcohol catalysts suffer from catalyst instability and reduced selectivity. This is mainly due to the blockage of active sites due to carbon deposition and phase separation on the catalyst, making it difficult to achieve long life and high selectivity.

Method used

The preparation method of a bimetallic copper-based catalyst covered with a dynamic carbon layer is used to deposit a graphite structure carbon layer on the surface of the catalyst through the carbonization process, and the catalyst is regenerated in situ through the dynamic migration and replenishment of the carbon layer during the syngas hydrogenation reaction. Improve the stability of the catalyst and the selectivity of lower alcohols.

Benefits of technology

It significantly improves the selectivity and yield of low-carbon alcohols, extends the life of the catalyst, solves the problems of catalyst carbon deposition and phase separation, improves the production efficiency of the synthesis gas hydrogenation reaction, and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744004A_ABST
    Figure CN118744004A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a dynamic carbon layer coated bimetallic copper-based catalyst, which comprises the following steps: (1) adding a metal salt mixture, a metal molybdenum source, alkali metal salt and a protective agent into water, stirring, evaporating to dryness, grinding into powder, and roasting the obtained powder to obtain a catalyst precursor; (2) carrying out carburizing treatment on the catalyst precursor in carburizing gas containing a carbon source to obtain a catalyst containing a carburizing material; and (3) carrying out passivating treatment on the catalyst containing the carburizing material in an oxidizing atmosphere. The catalyst provided by the invention can also be used for a reaction for preparing low-carbon alcohol through synthesis gas hydrogenation, and a result shows that the catalyst prepared by the invention can inhibit phase separation in a synthesis gas hydrogenation reaction process through dynamic carbon layer encapsulation of bimetals Cu-Co and Cu-Fe, so that the selectivity of the low-carbon alcohol is greatly improved, and the catalyst shows high stability. The method provided by the invention creates a promising way for preparing the high-selectivity and high-stability catalyst for preparing the low-carbon alcohol from the synthesis gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, in particular to the preparation of a bimetallic copper-based catalyst coated with a dynamic carbon layer and its application in the reaction of hydrogenating synthesis gas to produce low-carbon alcohols. Background Art

[0002] Since the beginning of the 20th century, the preparation of low-carbon alcohols (HA) from syngas (CO+H2) has become an important part of converting non-petroleum carbon resources into high-value-added products. As a clean and sustainable process, it can reduce dependence on petroleum to meet the growing energy demand. Low-carbon alcohols can be used as fuels or fuel additives; they are also one of the important raw materials for detergents, cosmetics, plasticizers and many chemical reagents. Although the catalyst system for syngas to low-carbon alcohols has been significantly expanded and widely used in the past few decades, the preparation of catalysts with long life and high selectivity remains one of the most challenging issues. At present, there are mainly four catalytic systems for producing low-carbon alcohols from synthesis gas: modified methanol synthesis catalyst, modified Fischer-Tropsch synthesis catalyst, rhodium-based catalyst and molybdenum-based catalyst (HTLuk, et al., Chem. Soc. Rev. 46 (2017) 1358–1426; M. Ao, et al., ACS Catal. 8 (2018) 7025–7050); among them, the modified Fischer-Tropsch synthesis catalyst has attracted widespread attention due to its mild operating conditions and low cost.

[0003] The process of catalytic synthesis gas to produce low-carbon alcohols requires the dissociative adsorption of CO and the non-dissociative adsorption of CO, which means that catalysts with a single metal component are difficult to achieve. At present, metal Cu has been proven to have active sites for non-dissociative adsorption of CO, and bimetallic combinations of Cu-Co or Cu-Fe have also been proven to be effective catalytic combinations for hydrogenation of synthesis gas to produce low-carbon alcohols (PM Arvela, et al., Chem Cat Chem (2022) 1-22; G. Prieto, et al., Angew. Chem. Int. Ed. 53 (2014) 6397-6401; HTLuk, et al., ACS Catal. 8 (2018) 9604-9618). Therefore, in order to obtain higher selectivity for low-carbon alcohols, the commonly used methods are usually to strengthen the strong interaction between metal and support or to use a bimetallic catalytic system. However, the currently commonly used Cu-Co and Cu-Fe bimetallic catalysts have the following two challenges: On the one hand, the strong dissociative adsorption ability of Co or Fe makes the *CH produced by CO dissociative adsorption xIn addition to coupling to generate products, the intermediates will also deposit on the catalyst surface to block active sites; on the other hand, Co or Fe and Cu are often accompanied by phase changes during the reaction, resulting in instability of the catalyst structure and causing phase separation, which leads to a decrease in product selectivity. Therefore, in situ encapsulation of bimetallic active centers is considered to be an effective way to reduce phase separation during catalytic reactions (HOOtor, et al., ACS Catal. 10 (2020) 7630–7656; M.-H. Li, et al., Nano Res. 16 (2023) 3451–3474).

[0004] Carbides are widely used in various catalytic fields due to their excellent thermodynamic stability, high conductivity and unique electronic structure. Among them, molybdenum carbide (Mo2C) stands out as one of the ideal carriers for efficient hydrogenation of syngas because of its excellent thermodynamic stability, high conductivity and unique electronic structure. Specifically, it has been observed in previous experimental studies that during the carbonization process of Mo2C, a carbon layer with a graphite structure is deposited on the catalyst surface to form an in-situ encapsulation structure (AEAwadallah, et al., J.Environ.Chem.Eng.9(2021)1–11). In addition, some studies have found that carbon species on the catalyst surface can change the performance of the catalyst and affect the product selectivity during the synthesis gas hydrogenation reaction, but the dynamic reaction process is still unclear and the nature of the carbon promotion mechanism has not yet been revealed (Z. Cai, et al., Phys. Chem. Chem. Phys. 24 (2022) 11104–11111; X. Lin, et al., Ind. Eng. Chem. Res. 59 (2020) 14636–14642).

[0005] In summary, the reaction mechanism involved in preparing low-carbon alcohols from synthesis gas is relatively complex, and how to prepare a catalyst with high stability and high selectivity still faces many challenges. In view of this, this patent application is specially filed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer, and to apply the catalyst treated by the method to the hydrogenation of synthesis gas to produce low-carbon alcohols, so as to solve the problems of catalyst instability and reduced selectivity caused by carbon deposition and phase separation of existing catalysts.

[0007] To achieve the above-mentioned object of the invention, the present invention provides a method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer, comprising the following steps:

[0008] (1) adding a metal salt mixture, a metal molybdenum source, an alkali metal salt and a protective agent into water, stirring, evaporating and grinding into powder, and calcining the obtained powder to obtain a catalyst precursor;

[0009] (2) subjecting the catalyst precursor prepared in step (1) to carburizing treatment in a carburizing gas containing a carbon source to obtain a catalyst containing a carburizing material;

[0010] (3) The catalyst containing the carburizing material prepared in step (2) is passivated in an oxidizing atmosphere.

[0011] Preferably, the metal salt in step (1) is one or a mixture of two or more of copper nitrate, copper chloride, copper sulfate, cobalt nitrate, cobalt chloride, cobalt sulfate, ferric nitrate, ferric chloride or ferric sulfate; and the alkali metal salt is one of potassium carbonate, sodium carbonate, cesium carbonate or lithium carbonate.

[0012] Preferably, the metal molybdenum source in step (1) is one of ammonium molybdate, molybdenum trioxide or molybdenum chloride.

[0013] Preferably, the protective agent in step (1) is one or a combination of glucose, sucrose or sorbitol.

[0014] Preferably, the calcination temperature in step (1) is 400-600° C., and the calcination time is 3-5 hours.

[0015] Preferably, the carburizing treatment conditions described in step (2) are: CH4 / H2 mixed gas is selected as the carburizing gas, the carburizing treatment temperature is 600-800°C, the carburizing treatment time is 2-3h, and the flow rate of the carburizing gas is 50-250mL / min.

[0016] Preferably, the passivation treatment conditions described in step (3) are: the oxidizing atmosphere is an O2 / N2 mixed gas containing a low concentration of oxygen, the passivation treatment time is 3 to 6 hours, and the passivation treatment temperature is room temperature.

[0017] The catalyst prepared by the preparation method of the above-mentioned dynamic carbon layer-coated bimetallic copper-based catalyst, the catalyst uses molybdenum carbide as a carrier, metallic copper as an active metal, metallic cobalt or metallic iron as a co-catalyst, and a graphite carbon layer is coated on the catalyst surface; wherein the content of metallic copper in the catalyst is 2-7%, the content of metallic cobalt or metallic iron is 2-7%; the remainder is the carrier.

[0018] The specific steps of using the aforementioned dynamic carbon layer-coated bimetallic copper-based catalyst in the hydrogenation of synthesis gas to produce low-carbon alcohols are as follows: in a continuous flow fixed bed reactor, the reaction mixture gas is contacted with the catalyst for reaction.

[0019] Preferably, the reaction mixture is a mixture of CO, H2 and N2, the gas flow rate of the reaction mixture is 10 to 50 mL / min, the reaction temperature is 110 to 260° C., and the reaction pressure is 2 to 5 MPa.

[0020] The design principle of the present invention is as follows:

[0021] The preparation method of the catalyst provided by the present invention firstly utilizes the carbonization process to deposit a carbon layer with a graphite structure in situ on the catalyst surface, and the formation of the carbon layer can not only significantly promote the generation of low-carbon alcohols in the reaction of catalyzing synthesis gas to prepare low-carbon alcohols, but also enhance the life of the catalyst by stabilizing the Cu-Co or Cu-Fe alloy. Specifically, the carbon material deposited in the catalyst prepared by the present invention is "dynamic" and participates in the reaction; therefore, there is a dynamic movement process of migration and replenishment of the carbon layer during the synthesis gas hydrogenation reaction, thereby realizing the in-situ regeneration of the catalyst. For example: in the Cu-Co bimetallic system, the dynamic circulation of the carbon layer can obtain a higher selectivity for low-carbon alcohols and a high space-time yield. Secondly, the Mo2C used in the preparation method of the dynamic carbon layer coated bimetallic copper-based catalyst provided by the present invention is carburized using CH4 / H2 as a carbon source: the carbon generated by the dissociation of CH4 at a higher temperature enters the catalyst body and replaces oxygen to form Mo2C. At the same time, the coexistence of Cu-Co and Cu-Fe is very important for the operation, which can make CH4 dissociate and replace Mo-O to form Mo-C, and at the same time, carbon segregates to the catalyst surface to form a layered graphite structure; in this way, the construction of the dynamic carbon layer and the coating of the active metal can be realized. The "dynamic" carbon layer is activated by H2 to form *CH during the synthesis gas hydrogenation reaction. x species, and then combine with non-dissociatively adsorbed *CO to hydrogenate to form alcohols. This reaction process is faster than *CH x The energy barrier for coupling to form hydrocarbon species is lower, so the reaction proceeds in the direction of producing alcohols, improving the selectivity of alcohols in the product.

[0022] The beneficial effects of the present invention are as follows:

[0023] (1) Compared with the existing methods for preparing catalysts for the reaction of preparing low-carbon alcohols from synthesis gas, the catalyst preparation method provided by the present invention can construct a layered graphite structure carbon layer in situ on the surface of the active metal, so that the formed carbon layer is more likely to react with hydrogen, and can thus be driven by the reaction gas into the product to form an "active" dynamic carbon layer. The prepared dynamic carbon layer successfully changes the reaction path to make the reaction more conducive to the direction of alcohol production. The carbon layer involved in the reaction solves the problem of catalyst carbon deposition and enables the wrapped metal to maintain an alloy structure, thereby obtaining highly selective low-carbon alcohols. In addition, the dynamic cyclic movement process of the carbon layer of the catalyst provided by the present invention in the synthesis gas hydrogenation reaction successfully promotes the synthesis gas to low-carbon alcohol reaction. This method provides more ideas for improving the yield and economic benefits of low-carbon alcohols.

[0024] (2) The preparation method provided by the present invention has the advantages of simple operation method and mild operation conditions. In addition, the catalyst provided by the present invention also has the advantages of cheap and readily available raw materials and low cost.

[0025] (3) The catalyst provided by the present invention can improve the selectivity of low-carbon alcohols in the product in the synthesis gas hydrogenation reaction, which is beneficial to improving the production efficiency of the synthesis gas hydrogenation reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The catalyst CuCoMo@C prepared in Example 1 and the catalyst CuFeMo prepared in Example 3 1D @ TEM image of C;

[0027] Figure 2 The catalyst CuCoMo@C prepared in Example 1 and the catalyst CuFeMo prepared in Example 3 1D @C and stability data of the catalyst CuCoMo prepared in Comparative Example 2;

[0028] Figure 3 For CuCoMo@ 13 C catalyst and CuCoMo@ 12 TPSR characterization diagram of C catalyst;

[0029] Figure 4 CuFeMo 1D @ 13 C catalyst and CuFeMo 1D @ 12 C. Characterization of the catalytic product by GC-MS;

[0030] Figure 5 For CuCoMo@ 13 Raman characterization diagram of C catalyst after reaction. DETAILED DESCRIPTION

[0031] The present application is further described in detail below through the accompanying drawings and embodiments. Through these descriptions, the characteristics and advantages of the present application will become clearer and more specific.

[0032] All reagents in the examples of this application are ammonium molybdate ((NH4)6Mo7O 24 ·4H2O), copper nitrate (Cu(NO3)2·3H2O), cobalt nitrate (Co(NO3)2·6H2O), ferric nitrate (Fe(NO3)3·9H2O), potassium carbonate (K2CO3), and glucose can all be purchased through commercial channels; the strip molybdenum trioxide used can be prepared by hydrothermal reaction of ammonium molybdate, and the specific steps are as follows: weigh 4g of ammonium molybdate, add 40mL of 5mol / L nitric acid aqueous solution, transfer the resulting mixture to a hydrothermal kettle and stir at room temperature for 1h, then carry out hydrothermal reaction in an oven at 160℃ for 5h, wash the obtained precipitate and put it in an oven at 60℃ to dry overnight.

[0033] Example 1

[0034] The steps for preparing the catalyst are as follows:

[0035] (1) Weigh 4 g of ammonium molybdate ((NH4)6Mo7O 24 ·4H2O, with AR grade purity), 0.610g of cobalt nitrate (Co(NO3)2·6H2O, with AR grade purity), 0.506g of copper nitrate (Cu(NO3)2·3H2O, with AR grade purity) and 30mL of water were mixed, stirred at room temperature for 4h, and then the mixture was stirred and evaporated to dryness at 90°C to a paste, and then dried in an oven, the obtained solid was ground into powder and transferred to a muffle furnace, and calcined at 500°C for 4h to obtain a catalyst precursor;

[0036] (2) transferring the catalyst precursor prepared in step (1) into a tubular furnace, raising the temperature to 700° C. and calcining for 2 h in a CH4 / H2 atmosphere with a CH4 volume content of 15%, maintaining a CH4 / H2 flow rate of 150 mL / min, to prepare a catalyst containing a carburizing material;

[0037] (3) The catalyst containing carburizing material prepared in step (2) is passivated for 4 hours at room temperature in an O2 / N2 atmosphere with an O2 volume content of 1%.

[0038] The obtained catalyst is recorded as CuCo-Mo2C@C; wherein the mass fraction of CuCo is 10wt% and the molar ratio of CuCo is 1:1, which is abbreviated as CuCoMo@C. The obtained catalyst is characterized by transmission electron microscopy. The specific results are as follows Figure 1 a and Figure 1As shown in b: The results show that the prepared catalyst CuCoMo@C has a block structure and there is a carbon layer with a graphite structure covering the surface of the catalyst.

[0039] The evaluation steps of the catalyst are as follows:

[0040] 0.3g of the CuCoMo@C catalyst prepared in the previous step was mixed with 1.7g of quartz sand, filled in a quartz tube, placed in a continuous flow fixed bed reactor, and 15% CH4 / H2 was introduced at normal pressure, and the temperature was raised to 590°C and heated for 2h to pretreat the catalyst; after cooling, a synthesis gas with a volume ratio of 30:60:10 of CO / H2 / N2 was introduced, and the pressure was raised to 3MPa. The reaction temperature was 240°C and the mixed gas flow rate was 20mL / min. The reaction products were analyzed online using an Agilent 7890 gas chromatograph equipped with a flame ionization detector (FID) using a KB-PONA capillary column. CH4, CO, CO2, and N2 were analyzed online using a GC2060 gas chromatograph equipped with a thermal conductivity detector (TCD) using a TDX-01 filling column. The catalytic results are shown in Table 1, and the stability data are shown in Table 1. Figure 2 As shown in a: Figure 2 It can be seen from a that the catalyst CuCoMo@C used can operate stably for more than 200 hours at a reaction temperature of 240°C.

[0041] Example 2

[0042] The steps for preparing the catalyst are as follows:

[0043] (1) Weigh 4 g of ammonium molybdate ((NH4)6Mo7O 24 ·4H2O, AR grade purity), 0.610g cobalt nitrate (Co(NO3)2·6H2O, AR grade purity), 0.506g copper nitrate (Cu(NO3)2·3H2O, AR grade purity), 0.014g potassium carbonate (K2CO3, AR grade purity), 0.5g glucose and 30mL water are mixed and stirred at room temperature for 4h, and then the obtained mixed solution is stirred and evaporated to a paste at 90°C and then dried in an oven to obtain a pre-calcination mixture; the obtained pre-calcination mixture is ground into powder and transferred to a tubular furnace, and the temperature is raised to 500°C and calcined for 4h under N2 atmosphere with a N2 flow rate of 50mL / min to obtain a pre-carburizing precursor;

[0044] (2) transferring the carburizing precursor obtained in step (1) to a tube furnace, raising the temperature to 700° C. and calcining for 2 h in a 15% CH4 / H2 atmosphere, with a CH4 / H2 flow rate of 150 mL / min, to obtain a catalyst containing a carburizing material after the carburizing treatment is completed;

[0045] (3) The catalyst containing carburizing material obtained in step (2) is passivated with 1% O2 / N2 at room temperature for 4 hours.

[0046] The obtained catalyst is recorded as K-CuCo-Mo2C@C; wherein the mass fraction of CuCo is 10wt%, the molar ratio of CuCo is 1:1, the mass fraction of metal K is 0.3wt%, and this catalyst is abbreviated as K-CuCoMo@C.

[0047] The evaluation steps of the catalyst are as follows:

[0048] The above 0.3 g CuCoMo@C catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor for reaction. The specific operating conditions refer to Example 1. The catalytic results are shown in Table 1.

[0049] Example 3

[0050] The steps for preparing the catalyst are as follows:

[0051] (1) Weigh 3.261 g of ribbon molybdenum trioxide (MoO 3-1D ), 0.412g ferric nitrate (Fe(NO3)3·9H2O, AR grade purity), 0.246g copper nitrate (Cu(NO3)2·3H2O, AR grade purity), 0.5g glucose C6H 12 O6 was mixed with 30 mL of water, and after stirring at room temperature for 4 h, the obtained mixture was stirred and evaporated to dryness at 90°C to a paste, and then dried in an oven to obtain a pre-calcination mixture; the obtained pre-calcination mixture was ground into powder and transferred to a tube furnace, and calcined for 4 h under N2 atmosphere at a N2 flow rate of 50 mL / min and a temperature of 500°C to obtain a pre-carburizing precursor;

[0052] (2) subjecting the carburizing precursor obtained in step (1) to carburizing treatment, wherein the specific conditions are: the carburizing gas is 15% CH4 / H2, the carburizing treatment temperature is 700°C, the carburizing treatment time is 2h, and the carburizing gas flow rate is 150mL / min; after the carburizing treatment, a catalyst containing a carburizing material is prepared;

[0053] (3) The catalyst containing the carburizing material obtained in step (2) is passivated in a 1% O2 / N2 atmosphere at room temperature for 4 hours.

[0054] The obtained catalyst was recorded as CuFe-Mo2C 1D @C; the mass fraction of CuFe in the catalyst is 5wt%, and the molar ratio of CuFe is 1:1; this catalyst is abbreviated as CuFeMo 1D @C. The obtained catalyst was characterized by transmission electron microscopy. The specific results are as follows Figure 1 c and Figure 1 As shown in d, the results show that the prepared catalyst CuFeMo 1D @C is a one-dimensional nanoribbon structure with a graphite carbon layer on the surface.

[0055] The evaluation steps of the catalyst are as follows:

[0056] The above 0.3g CuFeMo 1D The catalyst @C was mixed with 1.7 g of quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The reaction temperature was 170°C, and the other conditions were the same as in Example 1. The catalytic results are shown in Table 1, and the stability data are shown in Table 1. Figure 2 As shown in b: Figure 2 b shows that the catalyst CuFeMo 1D @C can operate stably for more than 100 hours at a reaction temperature of 170°C.

[0057] Example 4

[0058] The preparation steps of the catalyst are as in Example 2, except that the protective agent glucose in step (1) is replaced by a mixed protective agent consisting of 0.2 g sucrose and 0.3 g sorbitol, and the remaining steps are the same as in Example 2. The obtained catalyst is recorded as K-CuCo-Mo2C@C-2, abbreviated as K-CuCoMo@C-2.

[0059] The evaluation steps of the catalyst are as follows:

[0060] The above 0.3 g K-CuCoMo@C-2 catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The reaction temperature was 170° C., and the other conditions were the same as in Example 1. The catalytic results are shown in Table 1.

[0061] Example 5

[0062] The preparation steps of the catalyst are similar to those of Example 2, except that the protective agent glucose in step (1) is replaced with 0.5 g of sorbitol, and the remaining steps are the same as those of Example 2. The obtained catalyst is recorded as K-CuCo-Mo2C@C-3, abbreviated as K-CuCoMo@C-3.

[0063] The evaluation steps of the catalyst are as follows:

[0064] The above 0.3 g K-CuCoMo@C-3 catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The reaction temperature was 170° C., and the other conditions were the same as in Example 1. The catalytic results are shown in Table 1.

[0065] Example 6

[0066] The preparation steps of the catalyst are similar to those of Example 1, except that the volume content of CH4 in the mixed gas CH4 / H2 in step (2) is adjusted to 20%, and the remaining steps are the same as those of Example 1. The obtained catalyst is recorded as CuCo-Mo2C@C-2, abbreviated as CuCoMo@C-2.

[0067] The evaluation steps of the catalyst are as follows:

[0068] The above 0.3 g CuCoMo@C-2 catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The reaction temperature was 170° C., and the other conditions were the same as in Example 1. The catalytic results are shown in Table 1.

[0069] Example 7

[0070] CuCoMo@ 13 The specific preparation method of catalyst C refers to the preparation steps of the catalyst in Example 1, except that 13 CH4 / H2 replaces CH4 / H2; the resulting CuCoMo@ 13 C catalyst and CuCoMo@ prepared in Example 1 12 The C catalyst was subjected to temperature programmed surface reaction (TPSR) characterization test, and the specific conditions were as follows: the reaction gas was 12 CO / H2 / N2, reaction temperature is 240℃; the reaction results are as follows Figure 3 As shown: For mass spectrometry signals 32 and 33, CuCoMo@ 13 The signal intensity of C catalyst is greater than that of CuCoMo@ 12 C catalyst, and mass spectrometry signals 32 and 33 are both isotope fragment peaks representing alcohols, which indicates that during the catalytic reaction, the carbon in the carbon layer of the catalyst will participate in the reaction and enter the reaction product.

[0071] CuFeMo 1D @ 13 The preparation method of catalyst C is based on the preparation steps of catalyst in Example 3, except that glucose 13 C6H 12 O6 replaces glucose C6H 12 O6; the obtained CuFeMo 1D @ 13 C catalyst and CuFeMo obtained in Example 3 1D @ 12 C catalyst 12 The reaction was carried out in CO / H2 / N2 gas at a reaction temperature of 170°C. The products after the reaction were characterized by GC-MS. The results are as follows Figure 4 As shown, from Figure 4It can be seen that the isotopic fragment peak (m / z=32) representing alcohol in the catalytic product is CuFeMo 1D @ 13 The strength of C catalyst is much higher than that of CuFeMo 1D @ 12 C catalyst, which further proves that the carbon in the catalyst carbon layer will participate in the reaction and enter the product.

[0072] In addition, we will also CuCoMo@ 13 C catalyst 12 The reaction was carried out in a CO / H2 / N2 atmosphere. The specific reaction conditions were as described in the catalyst evaluation step in Example 1. The catalyst obtained after the reaction was characterized by Raman. The results were as follows: Figure 5 As shown, from Figure 5 It can be seen that after the catalytic reaction, 13 The characteristic Raman band of C appears 12 This indicates that during the catalytic reaction, the carbon in the CO in the reaction gas is added to the catalyst carbon layer, and it does not form physically deposited amorphous carbon, but directly enters the graphite structure of the catalyst, which further explains the CuCoMo@ 13 The C catalyst forms a dynamic cyclic movement process involving carbon migration and replenishment during the synthesis gas to low-carbon alcohol reaction.

[0073] Table 1: Catalyst activity test results

[0074]

[0075] Comparative Example 1

[0076] The steps for preparing the catalyst are as follows:

[0077] (1) Weigh 4 g of ammonium molybdate ((NH4)6Mo7O 24 ·4H2O, purity is AR grade) after grinding, transferred to a muffle furnace, and calcined at 500℃ for 4h to obtain a carburizing precursor;

[0078] (2) transferring the carburizing precursor obtained in step (1) to a tube furnace, raising the temperature to 700° C. and calcining for 2 h in a 15% CH4 / H2 atmosphere, with a CH4 / H2 gas flow rate of 150 mL / min; after the carburizing treatment, a catalyst containing a carburizing material is prepared;

[0079] (3) The catalyst containing the carburizing material obtained in step (2) is passivated in a 1% O2 / N2 atmosphere at room temperature for 4 hours.

[0080] The obtained catalyst was recorded as Mo2C.

[0081] The evaluation steps of the catalyst are as follows:

[0082] The above 0.3 g Mo2C catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The remaining operations were the same as in Example 1. The catalytic results are shown in Table 1.

[0083] Comparative Example 2

[0084] The steps for preparing the catalyst are as follows:

[0085] (1) Weigh 2.310 g of Mo2C prepared in Comparative Example 1, 0.610 g of cobalt nitrate (Co(NO3)2·6H2O, AR purity), and 0.506 g of copper nitrate (Cu(NO3)2·3H2O, AR purity) and impregnate with water in equal volumes, ultrasonically impregnate for 1 h, transfer to a vacuum drying oven, stand at 30°C for 10 h, and then heat to 80°C for drying; after grinding, transfer the resulting mixture to a tube furnace, and heat to 500°C and calcine for 4 h in a 5% H2 / N2 atmosphere at a flow rate of 50 mL / min to obtain a pre-carburizing precursor;

[0086] (2) the precursor obtained in step (1) is further calcined in a tube furnace under a 15% CH4 / H2 atmosphere at a flow rate of 150 mL / min, with the temperature raised to 590°C for 2 h, to obtain a catalyst containing a carburizing material;

[0087] (3) The catalyst containing the carburizing material obtained in step (2) is passivated in a 1% O2 / N2 atmosphere at room temperature for 4 hours.

[0088] The obtained catalyst was recorded as CuCoMo, wherein the mass fraction of CuCo was 10 wt % and the molar ratio of CuCo was 1:1.

[0089] The evaluation steps of the catalyst are as follows:

[0090] The above 0.3 g CuCoMo catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The rest of the operation was the same as in Example 1. The catalytic results are shown in Table 1, and the stability data are shown in Table 1. Figure 2 As shown in a: Figure 2 It can be seen from a that the catalyst CuCoMo used cannot operate stably for a long time at a reaction temperature of 240°C.

[0091] Comparative Example 3

[0092] The steps for preparing the catalyst are as follows:

[0093] (1) Weigh 4 g of ammonium molybdate ((NH4)6Mo7O 24·4H2O, AR grade purity), 0.610g cobalt nitrate (Co(NO3)2·6H2O, AR grade purity), 0.506g copper nitrate (Cu(NO3)2·3H2O, AR grade purity), 0.014g potassium carbonate (K2CO3, AR grade purity) and 30mL water were mixed and stirred at room temperature for 4h, and then the mixture was stirred and evaporated to a paste at 90°C, and dried in an oven to obtain a pre-calcination mixture. The mixture was ground into powder and transferred to a muffle furnace, and then calcined at 500°C for 4h to obtain a pre-carburizing precursor;

[0094] (2) transferring the precursor obtained in step (1) to a tube furnace, raising the temperature to 700° C. and calcining for 2 h in a 15% CH4 / H2 atmosphere at a flow rate of 150 mL / min; after completion, a catalyst containing a carburizing material is prepared;

[0095] (3) The catalyst containing the carburizing material obtained in step (2) is passivated in a 1% O2 / N2 atmosphere at room temperature for 4 hours.

[0096] The obtained catalyst is recorded as K-CuCoMo, wherein the mass fraction of CuCo is 10wt%, the molar ratio of CuCo is 1:1, and the mass fraction of K is 0.3wt%.

[0097] The evaluation steps of the catalyst are as follows:

[0098] The above 0.3 g K-CuCoMo catalyst was mixed with 1.7 g quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The remaining operations were the same as in Example 1. The catalytic results are shown in Table 1.

[0099] Comparative Example 4

[0100] The steps for preparing the catalyst are as follows:

[0101] (1) Weigh 3.261 g of ribbon molybdenum trioxide (MoO 3-1D ), 0.412g of ferric nitrate (Fe(NO3)3·9H2O, AR grade purity), 0.246g of copper nitrate (Cu(NO3)2·3H2O, AR grade purity), mixed with 30mL of water, stirred at room temperature for 4h, then stirred and evaporated the mixed solution to dryness at 90°C to a paste, and dried in an oven to obtain a pre-carburizing mixture;

[0102] (2) Grinding the pre-carburizing mixture obtained in step (1) into powder and transferring it to a tube furnace, raising the temperature to 700° C. and calcining for 2 h in a 15% CH4 / H2 atmosphere at a flow rate of 150 mL / min; after completion, a catalyst containing a carburizing material is prepared;

[0103] (3) The catalyst containing the carburizing material obtained in step (2) is passivated in a 1% O2 / N2 atmosphere at room temperature for 4 hours.

[0104] The obtained catalyst was recorded as CuFeMo 1D ; Among them, the mass fraction of CuFe is 5wt%, and the molar ratio of CuFe is 1:1.

[0105] The evaluation steps of the catalyst are as follows:

[0106] The above 0.3g CuFeMo 1D The catalyst was mixed with 1.7 g of quartz sand, filled in a quartz tube, and placed in a continuous flow fixed bed reactor. The reaction temperature was 170° C., and the remaining operations were the same as in Example 1. The catalytic results are shown in Table 1.

Claims

1. A method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer, characterized in that: The following steps are involved: (1) adding a metal salt mixture, a metal molybdenum source, an alkali metal salt and a protective agent into water, stirring, evaporating and grinding into powder, and calcining the obtained powder to obtain a catalyst precursor; (2) subjecting the catalyst precursor prepared in step (1) to carburizing treatment in a carburizing gas containing a carbon source to obtain a catalyst containing a carburizing material; (3) The catalyst containing the carburizing material prepared in step (2) is passivated in an oxidizing atmosphere.

2. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The metal salt described in step (1) is one or a mixture of two or more of copper nitrate, copper chloride, copper sulfate, cobalt nitrate, cobalt chloride, cobalt sulfate, ferric nitrate, ferric chloride or ferric sulfate; the alkali metal salt is one of potassium carbonate, sodium carbonate, cesium carbonate or lithium carbonate.

3. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The metal molybdenum source described in step (1) is one of ammonium molybdate, molybdenum trioxide or molybdenum chloride.

4. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The protective agent in step (1) is one or a combination of glucose, sucrose or sorbitol.

5. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The calcination temperature in step (1) is 400-600° C., and the calcination time is 3-5 hours.

6. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The carburizing treatment conditions described in step (2) are: using CH4 / H2 mixed gas as the carburizing gas, the carburizing treatment temperature is 600-800°C, the carburizing treatment time is 2-3h, and the carburizing gas flow rate is 50-250mL / min.

7. The method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 1, characterized in that: The passivation treatment conditions described in step (3) are: the oxidizing atmosphere is an O2 / N2 mixed gas containing a low concentration of oxygen, the passivation treatment time is 3 to 6 hours, and the passivation treatment temperature is room temperature.

8. The catalyst prepared by the method for preparing a bimetallic copper-based catalyst coated with a dynamic carbon layer according to claims 1-7, characterized in that: The catalyst uses molybdenum carbide as a carrier, metallic copper as an active metal, metallic cobalt or metallic iron as a promoter, and a graphite carbon layer is coated on the catalyst surface; wherein the content of metallic copper in the catalyst is 2-7%, the content of metallic cobalt or metallic iron is 2-7%; the remainder is the carrier.

9. The use of the preparation method according to claims 1-7 or the bimetallic copper-based catalyst coated with a dynamic carbon layer according to claim 8 in the hydrogenation of synthesis gas to produce low-carbon alcohols, characterized in that: The specific steps are as follows: in a continuous flow fixed bed reactor, the reaction mixture gas is contacted with a catalyst to react.

10. The use of the dynamic carbon layer-coated bimetallic copper-based catalyst according to claim 9 in the hydrogenation of synthesis gas to produce low-carbon alcohols, characterized in that: The reaction mixed gas is a mixed gas composed of CO, H2 and N2, the gas flow rate of the reaction mixed gas is 10-50 mL / min, the reaction temperature is 110-260° C., and the reaction pressure is 2-5 MPa.