Method for innocent treatment of electrolytic solid waste
The electrolysis solid waste is treated through steps such as drying, crushing, roasting, water mixing, filtration and melting, which solves the problems of land occupation and environmental pollution in the solid waste treatment of electrolytic aluminum plants, realizes the harmless transformation of electrolysis solid waste, and reduces harm to the environment and human health.
Patent Information
- Application Number
- CN202410965849.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-08
AI Technical Summary
When existing electrolytic aluminum plants deal with electrolytic solid waste, they mainly use open-air stacking or soil landfill methods, which leads to land occupation and environmental pollution. In addition, soluble fluoride and cyanide contamination is serious, threatening the environment and human health.
Electrolysis solid waste is processed through steps such as drying, crushing, roasting, water mixing, filtration, and melting. Harmful substances are decomposed through physical and chemical methods and converted into harmless or low-toxic substances to reduce the impact on the environment and human health.
Effectively remove moisture and harmful substances from electrolysis solid waste, reduce harm to the environment and human health, reduce pollution, and achieve harmless treatment of electrolysis solid waste.
Smart Images

Figure CN118744147A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic solid waste recovery and treatment, and in particular to a method for harmlessly treating electrolytic solid waste. Background Art
[0002] Electrolytic solid waste mainly refers to various wastes generated in the electrolytic process, including waste anode carbon particles, waste cathode carbon blocks, and overhaul slag, etc. These wastes contain toxic and harmful substances, such as soluble fluoride and cyanide, which pose a threat to the environment and human health.
[0003] Most existing electrolytic aluminum plants use open-air stacking or direct soil landfill to deal with electrolytic aluminum solid waste, which not only occupies a large amount of land, but also the soluble fluoride contained in it not only pollutes the atmosphere but also flows into rivers with rainwater and seeps into the ground to pollute the soil and groundwater, causing great harm to the environment. Summary of the invention
[0004] The purpose of the present invention is to provide a method for harmlessly treating electrolytic solid waste to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for harmlessly treating electrolytic solid waste, comprising the following steps: S1. Obtain electrolytic solid waste and dry the electrolytic solid waste; S2, taking the electrolytic solid waste dried in step S1 and pulverizing it; S3, calcining the powder waste obtained in step S2; S4, adding the waste material roasted in step S3 into water, stirring and mixing thoroughly, and then filtering; S5, melting and burning the waste filtered in step S4, and removing slag after melting and burning.
[0006] Preferably, in step S1, the drying process is to place the electrolytic solid waste at an ambient temperature of 65°C to 85°C for 6h to 8h, and the electrolytic solid waste is spread out during drying, with a stacking thickness not exceeding 25cm.
[0007] Preferably, in step S2, a pulverizer is used to pulverize the electrolytic solid waste, and a sieve is used to screen the pulverized solid waste, wherein the sieve has a size of 100 to 160 meshes.
[0008] Preferably, in step S2, after screening, the powder waste is magnetically separated using a magnetic separator, and the remaining waste is retained for subsequent processing.
[0009] Preferably, in step S3, the calcination temperature is 1500° C. to 2000° C., the calcination time is not less than 90 min, and the calcination environment is filled with nitrogen for protection, maintaining the ambient pressure at 1.5 to 2.5 times the standard atmospheric pressure.
[0010] Preferably, in step S3, after the roasting process, air is filled into the roasting equipment, and the gas exhausted from the roasting equipment is adsorbed by an alkaline adsorption material, wherein the alkaline adsorption material is a mixture of any one or more of aluminum hydroxide, sodium hydroxide, and calcium hydroxide.
[0011] Preferably, in step S4, the calcined waste is cooled to room temperature in an open ventilated environment, and the temperature of the added water is 55°C to 65°C.
[0012] Preferably, in step S4, stirring is performed by a stirrer, the rotation speed of the stirrer is 60 r / min-80 r / min, and the stirring time is 40 min-60 min; after stirring, filtering is performed using a 60-mesh-80-mesh sieve.
[0013] Preferably, in step S5, the smelting temperature of the waste material is 750° C. to 980° C., and the smelting time is 2.5 h to 4.5 h; after smelting, the electrolyte ingot is obtained by cleaning, deslagging and casting.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: the treatment method provided by the present invention mainly comprises the steps of drying, crushing, roasting, water mixing filtration and sintering; Drying is to remove moisture from electrolytic solid waste so that subsequent treatment is more efficient; the dried electrolytic solid waste is crushed to reduce particle size and increase surface area, which helps to improve the efficiency of subsequent roasting and chemical reactions; the crushed waste is then heat treated at high temperature to decompose organic matter, destroy the chemical structure of harmful substances, and transform them into harmless or low-toxic substances; the roasted waste is added to water, fully stirred and mixed, and then filtered; the purpose is to remove soluble salts and other water-soluble impurities by water washing, and filter out insoluble solid particles at the same time; the filtered waste is subjected to high-temperature smelting to further remove residual organic and inorganic matter, and the residue after smelting is the treated electrolyte product; Harmful ingredients are converted into harmless or low-toxic forms through physical and chemical methods to reduce the impact on the environment and human health. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a flow chart of the steps of the present invention. DETAILED DESCRIPTION
[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Embodiment 1: A method for harmlessly treating electrolytic solid waste, comprising the following steps: S1. Obtain electrolytic solid waste and dry the electrolytic solid waste. The drying process is to place the electrolytic solid waste at an ambient temperature of 72° C. to 78° C. for 7 hours. The electrolytic solid waste is flattened during drying, and the stacking thickness is 30 cm.
[0018] S2. The electrolytic solid waste dried in step S1 is taken and crushed; the electrolytic solid waste is crushed by a crusher, and screened with a sieve after crushing, wherein the specification of the sieve is 130 mesh; after screening, the powder waste is magnetically separated by a magnetic separator, and the remaining waste is retained for subsequent treatment.
[0019] S3, the powder waste obtained in step S2 is calcined; the calcination temperature is 1800° C., the calcination time is 110 min, and the calcination environment is filled with nitrogen for protection, and the environmental pressure is maintained at 2 times the standard atmospheric pressure; after the calcination process, air is filled into the calcination equipment, and the gas discharged from the calcination equipment is adsorbed by an alkaline adsorption material, and the alkaline adsorption material is aluminum hydroxide.
[0020] S4, adding the waste material calcined in step S3 into water, stirring and mixing thoroughly, and then filtering; cooling the calcined waste material to room temperature in an open ventilated environment, and the temperature of the added water is 60° C.; stirring by a stirrer, the speed of the stirrer is 70 r / min, and the stirring time is 50 min; filtering through a 70-mesh sieve after stirring.
[0021] S5, smelting the waste filtered in step S4, the smelting temperature of the waste is 860°C, and the smelting time is 3.5 hours; after smelting, cleaning, slag removal and casting are performed to obtain electrolyte ingots.
[0022] Embodiment 2: A method for harmlessly treating electrolytic solid waste, comprising the following steps: S1. Obtain electrolytic solid waste and dry the electrolytic solid waste. The drying process is to place the electrolytic solid waste at an ambient temperature of 65°C to 70°C for 6 hours, and the electrolytic solid waste is flattened during drying, with a stacking thickness of 25 cm.
[0023] S2. The electrolytic solid waste dried in step S1 is taken and crushed; the electrolytic solid waste is crushed by a crusher, and screened with a sieve after crushing, wherein the specification of the sieve is 110 mesh; after screening, the powder waste is magnetically separated by a magnetic separator, and the remaining waste is retained for subsequent treatment.
[0024] S3, the powder waste obtained in step S2 is calcined; the calcination temperature is 1500° C., the calcination time is 90 min, and the calcination environment is filled with nitrogen for protection, and the environmental pressure is maintained at 1.5 times the standard atmospheric pressure; after the calcination process, air is filled into the calcination equipment, and the gas discharged from the calcination equipment is adsorbed by an alkaline adsorption material, wherein the alkaline adsorption material is a mixture of sodium hydroxide and calcium hydroxide.
[0025] S4, adding the waste material calcined in step S3 into water, stirring and mixing thoroughly, and then filtering; cooling the calcined waste material to room temperature in an open ventilated environment, and the temperature of the added water is 55° C.; stirring by a stirrer, the speed of the stirrer is 60 r / min, and the stirring time is 40 min; filtering through a 60-mesh sieve after stirring.
[0026] S5, melting the waste filtered in step S4, the melting temperature of the waste is 750°C, and the melting time is 2.5 hours; after melting, cleaning, slag removal and casting are performed to obtain electrolyte ingots.
[0027] Embodiment 3: A method for harmlessly treating electrolytic solid waste, comprising the following steps: S1. Obtain electrolytic solid waste and dry the electrolytic solid waste. The drying process is to place the electrolytic solid waste at an ambient temperature of 80° C. to 85° C. for 8 hours. The electrolytic solid waste is flattened during drying, and the stacking thickness is 35 cm.
[0028] S2. The electrolytic solid waste dried in step S1 is taken and crushed; the electrolytic solid waste is crushed by a crusher, and screened with a sieve after crushing, wherein the specification of the sieve is 160 mesh; after screening, the powder waste is magnetically separated by a magnetic separator, and the remaining waste is retained for subsequent treatment.
[0029] S3, the powder waste obtained in step S2 is calcined; the calcination temperature is 2000° C., the calcination time is 100 min, and the calcination environment is filled with nitrogen for protection, and the environmental pressure is maintained at 2.5 times the standard atmospheric pressure; after the calcination process, air is filled into the calcination equipment, and the gas discharged from the calcination equipment is adsorbed by an alkaline adsorption material, and the alkaline adsorption material is sodium hydroxide.
[0030] S4, adding the waste material calcined in step S3 into water, stirring and mixing thoroughly, and then filtering; cooling the calcined waste material to room temperature in an open ventilated environment, and the temperature of the added water is 65° C.; stirring by a stirrer, the speed of the stirrer is 80 r / min, and the stirring time is 60 min; filtering through an 80-mesh sieve after stirring.
[0031] S5. Sintering the waste filtered in step S4 at a temperature of 980° C. for 4.5 hours. After sintering, cleaning, slag removal and casting are performed to obtain electrolyte ingots.
[0032] The difference between Example 1, Example 2 and Example 3 is that the condition parameters in the steps are different; the solution provided by the present invention mainly converts harmful components into harmless or low-toxic forms through physical and chemical methods to reduce the impact on the environment and human health.
[0033] The drying in step S1 is to remove moisture from the electrolytic solid waste so that subsequent processing is more efficient; it is usually done using hot air drying, steam drying or other drying equipment; In step S2, the dried electrolytic solid waste is crushed to reduce the particle size and increase the surface area, which helps to improve the efficiency of subsequent roasting and chemical reactions; In step S3, the crushed waste is subjected to heat treatment at high temperature, which can decompose organic matter, destroy the chemical structure of harmful substances, and transform them into harmless or low-toxic substances; In step S4, the calcined waste is added to water, fully stirred and mixed, and then filtered; the purpose is to remove soluble salts and other water-soluble impurities by water washing, and filter out insoluble solid particles; In step S5, the filtered waste is subjected to high-temperature calcination to further remove residual organic and inorganic substances, and the residue after calcination is the treated electrolyte product.
[0034] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for harmlessly treating electrolytic solid waste, Features: The steps include: S1. Obtain electrolytic solid waste and dry the electrolytic solid waste; S2, taking the electrolytic solid waste dried in step S1 and pulverizing it; S3, calcining the powder waste obtained in step S2; S4, adding the waste material roasted in step S3 into water, stirring and mixing thoroughly, and then filtering; S5, melting and burning the waste filtered in step S4, and removing slag after melting and burning.
2. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In the step S1, the drying process is to place the electrolytic solid waste at an ambient temperature of 65°C to 85°C for 6h to 8h, and the electrolytic solid waste is flattened during drying, with a stacking thickness not exceeding 25cm.
3. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In the step S2, a pulverizer is used to pulverize the electrolytic solid waste, and a sieve is used to screen the pulverized solid waste, wherein the sieve has a specification of 100-160 meshes.
4. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In the step S2, after screening, the powder waste is magnetically separated using a magnetic separator, and the remaining waste is retained for subsequent processing.
5. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In the step S3, the calcination temperature is 1500°C to 2000°C, the calcination time is not less than 90 minutes, and the calcination environment is filled with nitrogen for protection, and the ambient pressure is maintained at 1.5 to 2.5 times the standard atmospheric pressure.
6. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In step S3, after the roasting process, air is filled into the roasting equipment, and the gas exhausted from the roasting equipment is adsorbed by an alkaline adsorption material, wherein the alkaline adsorption material is a mixture of any one or more of aluminum hydroxide, sodium hydroxide, and calcium hydroxide.
7. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In step S4, the calcined waste is cooled to room temperature in an open ventilated environment, and the temperature of the added water is 55°C to 65°C.
8. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In the step S4, stirring is performed by a stirrer, the rotation speed of the stirrer is 60 r / min-80 r / min, and the stirring time is 40 min-60 min; after stirring, filtering is performed using a 60-mesh-80-mesh sieve.
9. A method for harmlessly treating electrolytic solid waste according to claim 1, Features: In step S5, the smelting temperature of the waste material is 750° C. to 980° C., and the smelting time is 2.5 h to 4.5 h; after smelting, the waste material is cleaned, deslagging and cast to obtain an electrolyte ingot.
Citation Information
Patent Citations
Method for recovering rare earth from rare earth fluoride fused salt electrolysis waste with effects of environmental protection and low cost
CN104843761A
Aluminum electrolysis waste cathode calcination treatment method
CN107628614A
Electrolyte block based on carbon residue extraction and extraction process thereof
CN110067009A
Microwave-ultrasonic-alkaline leaching synergistic fluorine removal method for aluminum electrolysis waste and old cathode carbon block
CN111777054A
Acidification roasting method for efficiently treating aluminum electrolysis solid waste
CN114031099A