Preparation method of metal or non-metal nano micro powder
Nanopowders are prepared using laser radiation in a normal pressure inert gas environment through high-temperature gasification decomposition and resynthesis processes, which solves the problems of inaccurate particle size control and low purity in the existing technology, and achieves high-efficiency, low-cost nanopowders. Production, suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202410964978.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-08
AI Technical Summary
Existing methods for preparing metal or non-metal nanopowders have problems such as imprecise particle size control, low purity, complex processes, low production capacity, high cost and environmental pollution, making it difficult to meet the needs of high-performance materials.
Using the preparation process of high-temperature gasification decomposition and resynthesis, in a closed normal pressure inert gas environment, the high-density energy radiation of the laser is used to quickly vaporize the metal or non-metal raw materials and undergo processes such as particle growth, quenching and shaping, and cooling. , to produce nano-scale micro-powder materials to achieve nano-powder with adjustable particle size, high purity and no pollution.
It achieves the production of high-purity, nanometer-sized, uniform particle size nanopowder materials, reduces production costs, increases output, is suitable for large-scale production, and the process is simple, safe and reliable, and is suitable for industrial applications.
Smart Images

Figure CN118744241A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials, and in particular relates to a method for preparing metal or non-metal nano powder. Background Art
[0002] With the rapid development of nanotechnology, nanomaterials exhibit properties that are completely different from macroscopic materials due to their unique size effects, surface effects, and quantum effects. They have shown great application potential in the fields of materials science, energy, electronics, and chemical engineering, providing unlimited possibilities for the design and development of new materials.
[0003] For example, in the field of metal or non-metal nanomaterials: Nano magnesium powder has a high hydrogen storage capacity and has potential application value in portable energy equipment, fuel cell vehicles and other fields. Compared with traditional liquid or gaseous hydrogen storage methods, nano magnesium powder as a solid hydrogen storage material has higher safety. Nano nickel powder has broad application prospects in electrochemical energy storage, catalysts, magnetic materials, electronics industry and other fields. Nano copper powder occupies an important position in the field of microelectronics and is mainly used in the manufacture of electronic components such as integrated circuits and multilayer ceramic capacitors (MLCC). Nano silicon powder is widely used in optoelectronic semiconductors, lithium battery negative electrode materials, coatings and other fields. Nano boron powder has the advantages of high energy density and high combustion calorific value, and has important application value in solid propellants, pyrotechnics, ignition powder, mixed explosives, high-energy combustion agents and other fields.
[0004] However, the existing metal or non-metal powder preparation methods often have defects such as inaccurate product particle size control, low purity, complex process, low production capacity, high cost, environmental pollution, etc., which are difficult to meet the growing demand for high-performance materials. Therefore, developing a simple, efficient method that can prepare high-purity metal or non-metal nano powder has become a current research hotspot. The present invention is based on the principle of economic, practical and industrial production, and develops a new nano material preparation method to achieve low-cost, high-yield, large-scale, pollution-free production, and produce nano-level ultra-fine, ultra-purified nano materials. Summary of the invention
[0005] In view of the problems of inaccurate product particle size control, low purity, complex process, low production capacity, high cost and environmental pollution in the current domestic and foreign metal or non-metal nano-powder preparation methods, the present invention proposes a new high-temperature gasification decomposition and resynthesis preparation process. The preparation process can realize and adapt to the production of high-purity, nano-level, adjustable particle size and uniform particle size nano-powder materials of various metals or non-metals. The average particle size of the produced micro-powder is nano-level D50 5-100nm, with the advantages of small investment, low production cost, high output and no pollution, and is suitable for large-scale production.
[0006] Technical solution:
[0007] The present invention provides a method for preparing metal or non-metal nano-powder, including a method for preparing elemental metal and non-metal nano-powder. The preparation method is to use high-density energy radiation of laser in a closed atmospheric pressure inert gas environment to rapidly gasify metal or non-metal raw materials, and then cool and condense into spherical or irregular particles, and then produce nano-powder materials through particle growth, quenching and shaping, cooling, and collection processes. The preparation method is completed by a set of equipment.
[0008] The complete set of equipment used in this preparation method includes: a high-power laser, a gasifier, a particle growth furnace, a quencher, a water-air cooler, a dust collector, an inert gas generator, a storage tank, a vacuum unit, and a monitoring system. The entire process is completed in a relatively closed airflow channel, starting from the preparation of the inert gas by the inert gas generator, and along the flow direction of the inert gas, the inner cavities of the gasifier, the particle growth furnace, the quencher, the water-air cooler, and the dust collector are connected in sequence through pipelines to form the entire airflow channel. At the same time, a circulation pipeline is installed at the end of the airflow channel and connected to the outlet of the inert gas generator to reflux the inert gas for recycling.
[0009] In the above equipment, the storage tank is used to store metal or non-metal raw materials, and is equipped with a feeding device for pushing the metal or non-metal raw materials to the gasification platform in the gasifier. The outlet of the inert gas generator is connected to two branch pipes, one of which is connected to the storage tank for replenishing inert gas to the storage tank; the other pipe is connected to a fan and an electric heater, and then connected to the gasifier, for providing the gasifier with an inert gas flow with controllable flow and temperature. The gasifier is equipped with an independent temperature control and cooling device. The particle growth furnace is equipped with a separate temperature control heat dissipation device and an adjustable damper for adjusting and controlling the air flow temperature and air flow rate. The vacuum unit is connected to the storage tank and the air flow channel respectively, and is used to pre-vacuum the storage tank and the air flow channel before the complete set of equipment is put into operation. The monitoring system is used to monitor, adjust and control the operating status, operating parameters and process parameters of the air flow in the furnace cavity of each device throughout the process.
[0010] The whole process includes the following steps:
[0011] Step (1): Select a single metal or non-metal material in the form of granules or powder with high purity as a raw material.
[0012] Step (2): Load the above raw materials required for 1 to 2 shifts into the storage tank from the feeding port of the storage tank, close the feeding port to make the storage tank airtight, and push a portion of the raw materials onto the gasification platform in the gasifier through the feeding device.
[0013] Step (3): Start the monitoring system and vacuum unit. Under the action of the vacuum pump, remove the original oxygen and air in the storage tank and the air flow channel, and reduce the vacuum pressure to below 100Pa. After the vacuum is completed, close the vacuum pipeline valve and shut down the vacuum unit. Then start the inert gas generator and fan to fill the storage tank and the air flow channel with inert gas, so that the pressure in the storage tank and the air flow channel reaches normal pressure, that is, 1 atmosphere.
[0014] Step (4): Start the high-power laser, gasification furnace and its temperature control and cooling device, particle growth furnace and its temperature control and heat dissipation device, quencher, water-air cooler, dust collector and other equipment in sequence to put the entire set of equipment into operation. Under the action of the fan, the inert gas circulates in the air flow channel and the circulation pipeline, and the inert gas is replenished by the inert gas generator. Optionally, for the preparation of metal or non-metal nanopowders with a melting point above 1000°C, the electric heater at the outlet of the inert gas generator can be started at the same time to heat the inert gas to 500°C to 800°C before entering the gasification furnace.
[0015] Step (5): In the gasifier, the laser light emitted by the high-power laser is directly applied to the raw material on the gasification platform. The high-density energy radiation of the laser is used to make the raw material absorb energy rapidly and heat up to a temperature exceeding its boiling point, decompose and gasify into vapor and disperse in the inert gas. The temperature gradient is rapidly reduced to a temperature below the boiling point of the raw material, so that the raw material vapor condenses into spherical or irregularly shaped liquid particles and is suspended in the inert gas. The inert gas is also rapidly heated to form a high-temperature airflow.
[0016] Step (6): under the action of airflow, the liquid particles of the raw material enter the particle growth furnace along with the high-temperature airflow; the particle growth furnace is equipped with a temperature-controlled heat dissipation device and an adjustable air door for adjusting and controlling the airflow temperature and airflow velocity, so that the airflow temperature at the outlet of the particle growth furnace is not lower than the melting point temperature of the raw material, and the liquid particles of the raw material further collide and condense in the high-temperature airflow disturbance to grow particles; the size of the grown particles is affected by the cavity length of the particle growth furnace, the airflow temperature, and the airflow velocity. By setting the cavity length of the particle growth furnace, and controlling the airflow temperature and airflow velocity by the temperature-controlled heat dissipation device and the adjustable air door, the collision growth time and particle size of the suspended particles are controlled, thereby achieving accurate particle size classification.
[0017] Step (7): The grown liquid particles flow rapidly into a quencher along with the air flow. The quencher uses carbon dioxide as a low-temperature refrigerant. In the low-temperature environment, the liquid particles are rapidly cooled to a temperature below the melting point of the raw material. The rapid temperature change causes the liquid particles to rapidly solidify and form solid micropowders.
[0018] Step (8): The solid micropowder then enters the water-air cooler along with the air flow. The water-air cooler uses a multi-stage cooling method of water cooling plus air cooling to reduce the temperature of the solid micropowder to below 160°C before entering the dust collector.
[0019] Step (9): Finally, the solid micropowder enters the dust collector along with the air flow and is collected by the dust collector to obtain high-purity nano-scale micropowder.
[0020] In the above steps, the raw material is any one of single metals and non-metals, including but not limited to: metals such as magnesium, copper, aluminum, nickel, tungsten, iron, calcium, chromium, zinc, titanium, zirconium, tin, gold, silver, palladium, cobalt, hafnium, cadmium, bismuth, molybdenum, tantalum, niobium, antimony, germanium, vanadium, and non-metals such as carbon, silicon, boron, selenium, and tellurium; the melting point temperature and boiling point temperature of the raw material are the melting point and boiling point temperature of the selected metal or non-metal material, wherein:
[0021] Magnesium melting point 651 ℃, boiling point 1107 ℃; copper melting point 1083.4 ℃, boiling point 2562 ℃; aluminum melting point 660 ℃, boiling point 2327 ℃; nickel melting point 1453 ℃, boiling point 2732 ℃; tungsten melting point 3407 ℃, boiling point 5655 ℃; iron melting point 1535 ℃, boiling point 2750 ℃; calcium melting point 842 ℃, boiling point 1484 ℃; chromium melting point 1857 ℃, boiling point 2672 ℃; zinc melting point 419.73℃, boiling point 907℃; titanium melting point 1660℃, boiling point 3287℃; zirconium melting point 1852℃, boiling point 4377℃; tin melting point 232.06℃, boiling point 2270℃; gold melting point 1063℃, boiling point 2807℃; silver melting point 961℃, boiling point 2163℃; palladium melting point 1552℃, boiling point 2964℃; cobalt melting point 1 495℃, boiling point 2870℃; Hafnium melting point 2227℃, boiling point 4603℃; Cadmium melting point 321.18℃, boiling point 765℃; Bismuth melting point 271.52℃, boiling point 1564℃; Molybdenum melting point 2617℃, boiling point 4612℃; Tantalum melting point 2996℃, boiling point 5425℃; Niobium melting point 2468℃, boiling point 4744℃; Antimony melting point 630.9℃ , boiling point 1587℃; germanium melting point 937.4℃, boiling point 2830℃; vanadium melting point 1902℃, boiling point 3409℃; carbon melting point 3500℃, boiling point 4827℃; silicon melting point 1410℃, boiling point 2355℃; boron melting point 2076℃, boiling point 3927℃; selenium melting point 221℃, boiling point 685℃; tellurium melting point 449.65℃, boiling point 988℃.
[0022] In the above complete set of equipment, according to the product precision requirements, the dust collector uses a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process combining these dust collectors, among which the electrostatic dust collector uses a single-stage or multi-stage electrostatic dust collector to achieve accurate classification and collection of micro-powder materials. The monitoring system is equipped with a monitoring platform, an early warning and alarm system, and various equipment monitoring subsystems, which are used to monitor, adjust and control the operating status, operating parameters and process parameters of the airflow in the furnace chamber of each equipment throughout the process.
[0023] In the above process flow, firstly, high-purity metal or non-metal raw materials are selected and stored in a sealed storage tank. When the outlet valve of the inert gas generator is closed, the inner cavity of the air flow channel of each device is connected with the circulation pipeline to form a completely closed channel. In this way, the vacuum unit can perform vacuum pretreatment on the air flow channel and the storage tank to reduce the vacuum pressure to below 100Pa. Then, the inert gas is filled into the air flow channel and the storage tank through the inert gas generator, and the air pressure reaches normal pressure, that is, 1 atmosphere, to form an oxygen-free, normal pressure, inert gas-filled process atmosphere. For the very small amount of oxygen that still remains after the air flow channel is evacuated, a small amount of high-temperature oxidation reaction of the raw materials occurs at the beginning of the operation of the gasifier, which can quickly consume the remaining oxygen completely, so that a completely oxygen-free production environment can be quickly established without affecting normal production.
[0024] After other equipment is started, the entire closed airflow channel is still maintained at normal pressure or close to normal pressure. When the airflow passes through the gasifier, the raw material undergoes a gasification reaction, and the inert gas expands due to heat, and the air pressure will increase. After that, the airflow passes through the particle growth furnace, the quencher, and the wind and water cooler to cool down, and the air pressure will decrease accordingly. At this time, the monitoring system monitors the changes in the air pressure and temperature of the inner cavity of each device in real time, and adjusts the air supply volume of the inert gas generator, the fan power, the radiation power of the high-power laser, the damper of the particle growth furnace, and the temperature of the quencher and the wind and water cooler to keep the air pressure in the inner cavity of the equipment at normal pressure or slightly positive pressure, and stably maintain it within the range of 100KPa to 110KPa. The inner cavity of the equipment is maintained at normal pressure or slightly positive pressure, which is conducive to reducing the pressure difference between the inner cavity of the equipment and the outside atmosphere, effectively preventing air from leaking into the seal of the equipment, and ensuring the safe operation of the equipment.
[0025] In order to prevent misoperation or other accidents, an automatic pressure relief valve is installed on the air flow pipeline of the equipment, which will automatically release the pressure when the air pressure in the air flow channel exceeds 120KPa.
[0026] In the above process flow, metal or non-metal raw materials are pre-stored in storage tanks, which are continuously fed to the gasifier by a feeding device, and the inert gas generator continuously replenishes inert gas to the air flow channel in the inner cavity of the equipment. The raw materials are continuously subjected to laser radiation gasification, condensation growth, rapid cooling and shaping, cooling, and collection. This is a continuous and uninterrupted production process.
[0027] The above technical scheme adopts laser radiation gasification method to produce high-quality nano-powder materials. In the gasification reactor, the metal or non-metal raw material is subjected to the focused radiation of high-power, high-energy density laser, quickly absorbs a large amount of energy to undergo explosive gasification, and quickly cools down and condenses in nitrogen to form liquid particles, and then enters the particle growth furnace with the airflow for further condensation and growth. The particle growth furnace is equipped with a temperature control heat dissipation device and an adjustable damper to adjust and control the airflow temperature and airflow velocity, which are monitored and controlled in real time by the monitoring system platform. During the particle growth process, by setting the particle growth furnace cavity length and controlling the particle growth process parameters such as growth temperature, temperature gradient, and airflow velocity by the monitoring system, it can ensure that the particles grow in an orderly manner under the temperature gradient, and affect the collision growth time and particle size of the suspended particles, so as to achieve accurate classification of the particle size. After being treated in the particle growth furnace, the grown particles enter the quencher for rapid cooling, the temperature drops below the melting point, and they are quickly solidified and shaped. Finally, after further cooling in the water-air cooler, they are collected by the dust collector to obtain high-purity, high-quality ultrafine nano-powder materials.
[0028] In a particle growth furnace, by increasing the airflow temperature in the particle growth furnace chamber, or reducing the temperature difference between the inlet and outlet airflows, the stability and uniformity of the particle condensation temperature can be maintained, the particles can be prevented from agglomerating, and the uniformity of the particle size can be improved. Appropriately reducing the design length of the particle growth furnace chamber, or increasing the airflow velocity, will shorten the collision growth residence time of the suspended particles in the chamber, and generate ultrafine particles. However, if the chamber is too short or the airflow velocity is too fast, the chamber airflow cooling will be difficult to control, and the cooling effect of the subsequent equipment will be affected, increasing the cooling load of the subsequent equipment; on the contrary, lengthening the design length of the chamber, or reducing the airflow velocity, will prolong the particle growth time, and generate particles with larger particle sizes, but reducing the airflow velocity (and the laser power needs to be reduced accordingly) will reduce the equipment productivity and affect the output.
[0029] In order to solve the above problems, make the whole production line more convenient for fine adjustment, produce ultrafine powder or larger particle size powder, ensure the stability of particle growth temperature control, and achieve the expected equipment productivity, two sets of particle growth furnaces with the same furnace cavity size can be set in parallel and connected between the gasification furnace and the quencher. The design of the furnace cavity size of a single set of particle growth furnaces can meet the production of ultrafine powders, and are equipped with independent temperature control and heat dissipation devices and adjustable air doors. In this way, when only one set of particle growth furnaces is opened to participate in production operation, ultrafine powder can be produced when the airflow reaches the set flow rate Q and flow velocity V; when two sets of particle growth furnaces are opened at the same time to participate in production operation, due to the diversion effect, the airflow flow rate of a single set of particle growth furnaces is reduced to Q / 2, and the airflow velocity is reduced to V / 2, so that the collision growth residence time of suspended particles in the furnace cavity is doubled, thereby generating larger particle size powders, and the total flow rate of the two sets of particle growth furnaces is Q, which can also achieve the expected equipment productivity. In both cases, the air flow velocity in the furnace cavity can be further fine-tuned by adjusting the fan and the size of the adjustable damper in the furnace cavity to ensure stable operation of the equipment and accurate control of the operating process parameters and product particle size.
[0030] Among the equipment used in the above technical solution, except for the gasification furnace and the particle growth furnace which are special equipment, the rest of the equipment are conventional process equipment. Among them, the gasification furnace and the particle growth furnace equipment are required to have strong high temperature resistance. The solution is that, first, the gasification furnace and the particle growth furnace use refractory materials that can withstand ultra-high temperatures (>2300°C) in non-vacuum or non-inert atmospheres, such as zirconium boride and hafnium boride composite ultra-high temperature ceramic refractory materials with a refractory temperature of more than 3000°C; second, the gasification furnace and the particle growth furnace are equipped with their own independent temperature control cooling devices and temperature control heat dissipation devices, and the temperature of the furnace cavity wall is automatically monitored and controlled through the monitoring system and the temperature control cooling and heat dissipation devices, so that the temperature of the furnace cavity wall is kept below the refractory temperature; third, the inner diameter of the furnace cavity is appropriately increased to increase the temperature difference between the gasification area in the gasification furnace and the inner wall of its furnace cavity, and the temperature difference between the central high-temperature jet area in the particle growth furnace and the inner wall of its furnace cavity, so as to prevent the cavity material from being damaged by high temperature.
[0031] The above technical solution can produce high-purity, nano-scale, high-quality nano-powder materials with adjustable particle size and uniform particle size, and the average particle size of the powder is D50 5-100nm.
[0032] As attached Figure 2 The TESCAN electron microscope image of nano-spherical silicon powder sample 1 prepared by the pilot production line of the complete set of equipment of the present invention shows that the sample has a high spheroidization rate, the powder particles are spherical and round, the particle size distribution is uniform, and the particle size is about 30-50nm.
[0033] As attached Figure 3This is a ZEISS electron microscope image of a nano-spherical silicon powder sample 2 prepared by the pilot production line of the complete set of equipment of the present invention. The particle sizes of four particles measured randomly are: 27.26nm, 32.97nm, 39.76nm, and 30.37nm.
[0034] The complete set of equipment and process flow in the above technical solution are also applicable to the preparation of metal or non-metal compound nanopowders, including: the preparation of metal carbides, oxides, sulfides, borides, nitrides or non-metal carbides, oxides, sulfides, borides, nitrides nanopowders. The specific preparation process flow is: in the above step (1), a high-purity metal or non-metal compound material in granular or powder form is selected as a raw material for standby use; in the above step (5): in the gasification furnace, the metal or non-metal compound is rapidly gasified and decomposed under high-power laser radiation. The gas is dispersed in an inert gas and cooled by a temperature gradient to form a gaseous compound and collide and condense into liquid particles, or recrystallize into compound crystal nucleus particles. In the above step (6), the compound particles enter the particle growth furnace with the airflow and further collide and grow. The remaining process flow is the same as steps (2) to (4) and steps (7) to (9). The compound particles grown in the particle growth furnace are then subjected to quenching, shaping, cooling, and collection processes, and the particle size can be accurately graded and controlled to obtain the compound nanopowder with an average particle size of D50 5 to 100 nm.
[0035] Taking the preparation of nano silicon carbide whiskers as an example, high-purity silicon carbide raw materials are selected for use, and high-power lasers are used to irradiate the silicon carbide raw materials in a gasification furnace to quickly reach a boiling point of more than 2700°C, decompose into gas molecules of C and Si, and mainly vaporize into Si, Si2C, and SiC2 gases. Silicon carbide crystal nuclei are naturally formed by cooling and collision in an inert gas, and then enter a particle growth furnace with the airflow for further crystallization to grow whiskers. After that, they are subjected to quenching, shaping, cooling, and collection processes, and the particle size of the silicon carbide whiskers can be accurately controlled by graded control to obtain nano-scale silicon carbide whiskers with an average diameter of 2nm to 1.5μm and an aspect ratio of 40 to 200.
[0036] In particular, it is pointed out that the above technical scheme adopts an anaerobic storage and feeding process in a closed storage tank, including pre-storing raw materials in the storage tank, pre-vacuuming the storage tank and then filling it with inert gas, and continuously feeding the material by a feeding device, so that the raw material storage and feeding process are in an anaerobic environment, achieving safe and reliable continuous feeding capabilities, solving the problem of continuous feeding under anaerobic production conditions, and making continuous batch production and industrial production possible.
[0037] Secondly, this technical solution adopts an inert gas preheating process, and the inert gas is heated to 500℃ to 800℃ through an electric heater before entering the gasifier. First, it increases the air flow temperature in the gasifier, helps to improve the gasification efficiency of laser irradiated raw materials, is beneficial to improve equipment productivity, and saves energy consumption of high-power lasers; second, it increases the temperature of the raw materials after condensation into liquid particles after gasification, to ensure the stability of subsequent high-temperature particle growth in the particle growth furnace.
[0038] In addition, as mentioned above, the technical solution specifically proposes a dual particle growth furnace parallel process, which can produce ultra-fine powder or larger particle size powder on a production line without reducing the equipment productivity, meet the precision requirements of different products, achieve fine adjustment and product precision classification, and do not need to transform the production line due to product precision, which is conducive to reducing equipment investment costs and product costs. The gasification furnace and the particle growth furnace use their own independent temperature control cooling and heat dissipation processes to effectively protect the furnace cavity material from high temperature damage, extend the service life of the equipment, and keep the high-temperature airflow temperature in the particle growth furnace stable, adjustable and controllable, ensuring stable particle growth and fine particle size adjustment.
[0039] In summary, the above technical scheme proposes a feasible process scheme for preparing metal or non-metallic nano-powder materials by laser gasification. The specific process measures include: vacuum pretreatment process, normal pressure, closed inert gas environment production process, storage tank oxygen-free storage and feeding process, inert gas preheating process, continuous and uninterrupted production process, high-power laser radiation gasification process, gasification furnace temperature control and cooling process, particle suspension growth control process, dual particle growth furnace parallel process, particle growth furnace temperature control and heat dissipation process, sudden cooling and shaping process, multi-stage rapid cooling process, multi-stage dust collection process, inert gas circulation process, and full-process monitoring process.
[0040] The whole process is simple, with few steps and easy control and operation. The gasification, synthesis growth, cooling and collection of materials are completed quickly and continuously in a short time, with short production cycle, high efficiency, low energy consumption, no pollution, small equipment investment, and is very suitable for large-scale production.
[0041] At the same time, by adjusting the process parameters, this process can be applied to the production of a variety of metal or non-metallic nano-powder materials. It has strong adaptability to raw materials, and both powder and sand can be put into production. There is no need to replace the production line when the raw materials change. Therefore, it can significantly save equipment investment costs and reduce production costs.
[0042] The beneficial effects of the present invention are summarized as follows:
[0043] (1) Simple, efficient and widely applicable process: The present invention proposes a feasible solution for preparing metal or non-metal nano-powder materials by laser vaporization, which utilizes high-power laser, efficient and clean energy. The process is simple, fast and efficient, and does not require complicated equipment and operation. The production line is suitable for a variety of metal or non-metal raw materials and has a wide range of applications.
[0044] (2) Safe and reliable process: The production process is carried out under normal pressure and closed inert gas environment, which does not require complicated vacuum or ultra-low pressure and highly closed process equipment. This significantly reduces the complexity of process equipment and the design and manufacturing costs, improves production safety, makes process control operation simple and easy, and ensures safe and reliable equipment operation.
[0045] (3) Controllable particle size: A high-temperature particle growth control process is proposed. By setting the furnace chamber length and adjusting process parameters such as air flow velocity, air flow temperature, and temperature drop gradient, the particle size and distribution range of the micropowder can be precisely controlled, including ultrafine powder or larger particle size powder. This can meet the diverse needs of different fields for nanomaterials.
[0046] (4) High quality of product particle size and uniformity: The suspended particle growth process is adopted, and the condensed particles are suspended in the high-temperature airflow and further collide and grow naturally. The carbon dioxide low-temperature refrigerant rapid cooling and shaping process is adopted to make the suspended particles quickly condense and shape into spheres or irregular crystals, which significantly improves the product spheroidization rate and crystal quality. Then, through the multi-stage dust collection process, the product can be accurately graded, and the product fineness and uniformity quality can be further improved, thereby effectively improving the product performance.
[0047] (5) High product purity: The production process uses high-purity raw materials, vacuum pretreatment and a closed inert gas environment at normal pressure. The laser radiation energy used is a non-contact heat source, and no impurities are generated during the production process, ensuring the high purity of the product.
[0048] (6) Continuous batch production: Through the storage tank pre-storage device, continuous feeding device and subsequent continuous process flow, continuous feeding and continuous production are achieved, meeting the needs of batch and large-scale production and realizing industrial production.
[0049] (7) Energy saving and consumption reduction: Through the inert gas circulation process, the inert gas in the production process is recycled and reused to reduce emissions, effectively reducing energy consumption and production costs.
[0050] (8) Pollution-free production: No waste gas, waste water or solid waste is discharged during the production process, which does not cause environmental pollution.
[0051] In summary, the present invention can prepare ultrafine, high-purity, uniform-size, high-quality nano-scale metal or non-metal micropowders, the production process is simple and easy, the production process is pollution-free, safe and reliable, the production cycle is short, the efficiency is high, the energy consumption is low, the investment is small, the output is high, and it can be used for mass industrial production, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0053] Figure 1 It is a schematic diagram of the structural principle of the complete set of equipment system of the present invention.
[0054] Figure 2 This is a TESCAN electron microscope image of a nano-spherical silicon powder sample 1 prepared by the pilot production line of the complete set of equipment of the present invention.
[0055] Figure 3 This is a ZEISS electron microscope image of nano-spherical silicon powder sample 2 prepared by the pilot production line of the complete set of equipment of the present invention.
[0056] exist Figure 1 In: 1. High-power laser; 2. Gasification furnace; 3. Gasification platform; 4. Particle growth furnace; 5. Quench cooler; 6. Water-air cooler; 7. Dust collector; 8. Storage tank; 9. Feeding device; 10. Inert gas generator; 11. Fan; 12. Electric heater; 13. Vacuum unit; 14. Circulation pipeline; 15. Monitoring system. DETAILED DESCRIPTION
[0057] Example 1: Preparation method of nano-spherical copper powder.
[0058] like Figure 1As shown, the complete set of equipment used in the preparation method includes: a high-power laser 1, a gasifier 2, a particle growth furnace 4, a quencher 5, a water-air cooler 6, a dust collector 7, an inert gas generator 10, a storage tank 8, a vacuum unit 13, and a monitoring system 15. The entire process is completed in a relatively closed airflow channel, starting from the preparation of the inert gas by the inert gas generator 10, and along the flow direction of the inert gas, the gasifier 2, the particle growth furnace 4, the quencher 5, the water-air cooler 6 and the inner cavity of the dust collector 7 are connected in sequence through pipelines to form the entire airflow channel. At the same time, a circulation pipeline 14 is installed at the end of the airflow channel and connected to the outlet of the inert gas generator 10 to reflux the inert gas for recycling. The storage tank 8 is used to store raw materials and is equipped with a feeding device 9 for pushing the raw materials to the gasification platform 3 in the gasifier 2. The outlet of the inert gas generator 10 is connected to two branch pipes, one of which is connected to the storage tank 8; the other is connected to the fan 11 and the electric heater 12, and then connected to the gasifier 2, which is used to provide the gasifier with an inert gas flow with controllable flow and temperature. The gasifier 2 is equipped with an independent temperature control and cooling device. The particle growth furnace 4 is equipped with a separate temperature control and heat dissipation device and an adjustable damper to adjust and control the air flow temperature and air flow rate; if the product accuracy requires, it is convenient for more refined adjustment, and two sets of particle growth furnaces 4 with the same furnace cavity size can be connected in parallel and connected between the gasifier 2 and the quencher 5. The vacuum unit 13 is connected to the storage tank 8 and the air flow channel respectively, and is used to pre-vacuum the storage tank 8 and the air flow channel before the complete set of equipment is put into operation. According to the product accuracy requirements, the dust collector 7 uses a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process combining these dust collectors. The equipment airflow pipeline is equipped with an automatic pressure relief valve, which will automatically release the pressure when the air pressure in the airflow channel exceeds 120KPa. The monitoring system 15 is equipped with a monitoring platform, an early warning and alarm system, and each equipment monitoring subsystem, which is used to monitor, adjust and control the operating status, operating parameters of each equipment and the process parameters of the airflow in the furnace chamber.
[0059] Material selection: Use high-purity copper raw materials in granular or powdered form for future use.
[0060] Process preparation: Load the copper raw materials required for 1 to 2 shifts into the storage tank 8 from the feeding port of the storage tank 8, close the feeding port to make the storage tank 8 in a closed state, and push a portion of the copper raw materials to the gasification platform 3 in the gasifier through the feeding device 9. Start the monitoring system 15 and the vacuum unit 13, and under the action of the vacuum pump, remove the original oxygen and air in the storage tank 8 and the air flow channel, and reduce the vacuum pressure to below 100Pa. After the vacuum is completed, close the vacuum pipeline valve and shut down the vacuum machine 13. Then start the inert gas generator 10 and the fan 11, fill the storage tank 8 and the air flow channel with inert gas, so that the pressure of the storage tank 8 and the air flow channel reaches normal pressure, that is, 1 atmosphere.
[0061] Process flow: The electric heater 12 at the outlet of the inert gas generator 10, the high-power laser 1, the gasification furnace 2 and its temperature control and cooling device, the particle growth furnace 4 and its temperature control and heat dissipation device, the quencher 5, the water-air cooler 6, the dust collector 7 and other equipment are started in sequence to put the entire set of equipment into operation. Under the action of the fan 11, the inert gas circulates in the air flow channel and the circulation pipeline 14, and the inert gas is supplemented by the inert gas generator 10. At the same time, the power of the electric heater 12 is adjusted and controlled to heat the inert gas to above 500°C. In the gasification furnace 2, the laser emitted by the high-power laser 1 directly acts on the raw materials on the gasification platform 3, so that the raw materials are rapidly heated to exceed their boiling point, decomposed and gasified into copper vapor dispersed in the inert gas, and the temperature gradient is rapidly reduced to below its boiling point, condensed into spherical liquid copper particles, and suspended in the inert gas. Under the action of airflow, liquid copper particles enter the particle growth furnace 4 with high-temperature airflow. The temperature and velocity of the airflow are adjusted by adjusting the temperature control and heat dissipation device and the adjustable air door of the particle growth furnace 4, so that the airflow temperature at the outlet of the particle growth furnace 4 is not lower than the melting point of copper. The liquid copper particles further collide and condense in the high-temperature airflow disturbance to grow particles. Then, they enter the quencher 5 with the airflow. The quencher 5 uses carbon dioxide low-temperature refrigerant. The liquid copper particles are rapidly cooled, the temperature drops below the melting point of copper, and they are rapidly solidified and shaped to form solid spherical copper powder. Then, they enter the water-air cooler 6 with the airflow, the temperature drops below 160°C, and finally enter the dust collector 7 with the airflow to collect high-purity nano-scale spherical copper powder with an average particle size of D50 5-100nm.
[0062] In the above process flow, the boiling point of copper is 2562°C and the melting point is 1083.4°C.
[0063] Example 2: Preparation method of nano-spherical nickel powder.
[0064] The complete set of equipment used in this preparation method is the same as that in Example 1.
[0065] Material selection: Use high-purity nickel raw materials in granular or powdered form for future use.
[0066] Process preparation: The nickel raw materials required for 1 to 2 shifts are pre-loaded into the storage tank 8, and the remaining operations are the same as the process preparation in Example 1.
[0067] Process flow: The process flow is similar to that of Example 1, except that the boiling point of nickel is 2732°C and the melting point is 1453°C. The nickel raw material is gasified and condensed into liquid nickel particles in the gasifier 2, grows with the air flow in the particle growth furnace 4, solidifies into spherical nickel powder in the quencher 5, and then is cooled by the water-air cooler 6 and collected by the dust collector 7 to obtain high-purity nano-scale spherical nickel powder with an average particle size of D50 5 to 100 nm.
[0068] Example 3: Preparation method of nano boron powder.
[0069] The complete set of equipment used in this preparation method is the same as that in Example 1.
[0070] Material selection: Use high-purity boron raw materials in granular or powdered form for standby use.
[0071] Process preparation: The boron raw materials required for 1 to 2 shifts are pre-loaded into the storage tank 8, and the remaining operations are the same as the process preparation in Example 1.
[0072] Process flow: The process flow is similar to that of Example 1, except that the boiling point of boron is 3927°C and the melting point is 2076°C. The boron raw material is gasified and condensed into liquid boron particles in the gasifier 2, grows with the air flow in the particle growth furnace 4, solidifies into boron powder in the quencher 5, and then is cooled by the water-air cooler 6 and collected by the dust collector 7 to obtain high-purity nano boron powder with an average particle size of D50 5 to 100 nm.
Claims
1. A method for preparing metal or non-metal nanopowder, characterized in that: The invention comprises a method for preparing single metal and non-metal nano powders; the method comprises the following steps: in a closed atmospheric pressure inert gas environment, using high-density energy radiation of laser to rapidly gasify metal or non-metal raw materials, and then cooling and condensing them into spherical or irregular particles, and then subjecting the particles to particle growth, rapid cooling and shaping, cooling, and collection processes to produce nano-level powder materials; the method comprises a set of equipment to complete the process flow; The complete set of equipment includes: a high-power laser, a gasifier, a particle growth furnace, a quencher, a water-air cooler, a dust collector, an inert gas generator, a storage tank, a vacuum unit, and a monitoring system; the entire process is completed in a relatively closed airflow channel, starting from the inert gas generator preparing the inert gas, along the inert gas flow direction, the gasifier, the particle growth furnace, the quencher, the water-air cooler and the inner cavity of the dust collector are connected in sequence through pipelines to form the entire airflow channel; at the same time, a circulation pipeline is installed at the end of the airflow channel and connected to the outlet of the inert gas generator to reflux the inert gas for recycling; In the complete set of equipment, the storage tank is used to store metal or non-metal raw materials, and is equipped with a feeding device for pushing the metal or non-metal raw materials to the gasification platform in the gasifier; the outlet of the inert gas generator is connected to two branch pipes, one of which is connected to the storage tank for replenishing inert gas to the storage tank, and the other is connected to a fan and an electric heater, and then connected to the gasifier, for providing the gasifier with an inert gas flow with controllable flow and temperature; the gasifier is equipped with an independent temperature control and cooling device; the particle growth furnace is equipped with a separate temperature control and heat dissipation device and an adjustable damper for adjusting and controlling the air flow temperature and air flow rate; the vacuum unit is respectively connected to the storage tank and the air flow channel, and is used to pre-vacuum the storage tank and the air flow channel before the complete set of equipment is put into operation; the monitoring system is used to monitor, adjust and control the operating status, operating parameters of each equipment and the process parameters of the air flow in the furnace cavity throughout the process; The process measures adopted in the process flow include: vacuum pretreatment process, normal pressure and closed inert gas environment production process, oxygen-free storage and feeding process in storage tanks, inert gas preheating process, continuous and uninterrupted production process, high-power laser radiation gasification process, gasification furnace temperature control and cooling process, particle suspension growth control process, particle growth furnace temperature control and heat dissipation process, quenching and shaping process, multi-stage rapid cooling process, multi-stage dust collection process, inert gas circulation process, and full-process monitoring process; The process specifically comprises the following steps: Step (1): Select a high-purity metal or non-metal material in granular or powder form as a raw material; Step (2): loading the raw materials required for one to two shifts into the storage tank from the feeding port of the storage tank, closing the feeding port to make the storage tank airtight, and pushing a portion of the raw materials onto the gasification platform in the gasifier through the feeding device; Step (3): Start the monitoring system and the vacuum unit, and under the action of the vacuum pump, remove the original oxygen and air in the storage tank and the air flow channel, and reduce the vacuum pressure to below 100Pa; after the vacuuming is completed, close the vacuum pipeline valve and shut down the vacuum unit; then start the inert gas generator and the fan to fill the storage tank and the air flow channel with inert gas, so that the pressure of the storage tank and the air flow channel reaches normal pressure, that is, 1 atmosphere; Step (4): sequentially start the high-power laser, the gasification furnace and its temperature control and cooling device, the particle growth furnace and its temperature control and heat dissipation device, the quencher, the water-air cooler, and the dust collector to put the entire set of equipment into operation; under the action of the fan, the inert gas circulates in the air flow channel and the circulation pipeline, and the inert gas is supplemented by the inert gas generator; optionally, for the preparation of metal or non-metal nanopowders with a melting point above 1000°C, the electric heater at the outlet of the inert gas generator can be started at the same time to heat the inert gas to 500°C to 800°C before entering the gasification furnace; Step (5): In the gasifier, the laser light emitted by the high-power laser is directly applied to the raw material on the gasification platform. The high-density energy radiation of the laser is used to make the raw material absorb energy rapidly and heat up to a temperature exceeding its boiling point, decompose and gasify into vapor and disperse in the inert gas. The temperature gradient is rapidly reduced to a temperature below the boiling point of the raw material, so that the raw material vapor is condensed into spherical or irregular liquid particles and suspended in the inert gas. The inert gas is also rapidly heated to form a high-temperature airflow. Step (6): under the action of airflow, the liquid particles of the raw material enter the particle growth furnace along with the high-temperature airflow; the particle growth furnace is equipped with a temperature-controlled heat dissipation device and an adjustable air door for adjusting and controlling the airflow temperature and airflow velocity, so that the airflow temperature at the outlet of the particle growth furnace is not lower than the melting point temperature of the raw material, and the liquid particles of the raw material further collide and condense in the high-temperature airflow disturbance to grow particles; the size of the growing particles is affected by the cavity length of the particle growth furnace, the airflow temperature, and the airflow velocity of the particle growth furnace. By setting the cavity length of the particle growth furnace, and controlling the airflow temperature and airflow velocity by the temperature-controlled heat dissipation device and the adjustable air door, the collision growth time and particle size of the suspended particles are controlled, thereby achieving accurate particle size classification; Step (7): the grown liquid particles flow rapidly into a quencher along with the airflow, and the quencher uses carbon dioxide as a low-temperature refrigerant; in the low-temperature environment, the liquid particles are rapidly cooled, and the temperature drops below the melting point of the raw material. The rapid temperature change causes the liquid particles to rapidly solidify and form solid micropowders; Step (8): the solid micropowder then enters the water-air cooler along with the air flow. The water-air cooler adopts a multi-stage cooling method of water cooling plus air cooling to reduce the temperature of the solid micropowder to below 160° C. before entering the dust collector. Step (9): Finally, the solid micropowder enters the dust collector along with the airflow and is collected by the dust collector to obtain high-purity nano-scale micropowder; In the above process flow, metal or non-metal raw materials are pre-stored in storage tanks, which are continuously fed to the gasifier by a feeding device, and the inert gas generator continuously replenishes inert gas to the air flow channel in the inner cavity of the equipment. The raw materials are continuously subjected to laser radiation gasification, condensation growth, rapid cooling and shaping, cooling, and collection. This is a continuous and uninterrupted production process.
2. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The raw material is any one of a single metal or a non-metal, including any one of magnesium, copper, aluminum, nickel, tungsten, iron, calcium, chromium, zinc, titanium, zirconium, tin, gold, silver, palladium, cobalt, hafnium, cadmium, bismuth, molybdenum, tantalum, niobium, antimony, germanium, vanadium, carbon, silicon, boron, selenium, and tellurium.
3. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The particle growth furnace is provided with two sets of particle growth furnaces with the same furnace chamber size connected in parallel and connected between the gasification furnace and the quencher, wherein the furnace chamber size of a single set of particle growth furnaces is designed to meet the production of ultrafine powders, and both are provided with independent temperature control and heat dissipation devices and adjustable air doors; when only one set of particle growth furnaces is opened to participate in production operation, ultrafine powders can be produced; when both sets of particle growth furnaces are opened to participate in production operation at the same time, due to the diversion effect, the air flow velocity in the furnace chamber is reduced, and the collision growth residence time of the suspended particles in the furnace chamber is prolonged, thereby generating powders with larger particle sizes to meet the product precision requirements.
4. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The average particle size of the metal or non-metal nano powder produced by the preparation method is: D50 5-100nm.
5. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The dust collector is a cyclone dust collector, a bag dust collector or an electrostatic dust collector, or a multi-stage dust collection process combining these dust collectors, wherein the electrostatic dust collector uses a single-stage or multi-stage electrostatic dust collector to achieve accurate classification and collection of micro-powder materials.
6. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The monitoring system is provided with a monitoring platform, an early warning and alarm system and various equipment monitoring subsystems.
7. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The air flow pipeline of the complete set of equipment is equipped with an automatic pressure relief valve, which will automatically relieve pressure when the air pressure in the air flow channel exceeds 120KPa.
8. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The furnace chamber materials of the gasification furnace and the particle growth furnace are made of zirconium boride and hafnium boride composite ultra-high temperature ceramic material with a refractory temperature of more than 3000°C.
9. The method for preparing metal or non-metal nanopowder according to claim 1, characterized in that: The complete set of equipment and process flow are also applicable to the preparation of metal or non-metal compound nano-powders, including: the preparation of metal carbides, oxides, sulfides, borides, nitrides or non-metal carbides, oxides, sulfides, borides, nitrides nano-powders, and the preparation process flow is: in the step (1), a high-purity metal or non-metal compound material in granular or powder form is selected as a raw material for standby use; in the step (5), in a gasification furnace, the metal or non-metal compound is rapidly gasified and decomposed into steam under high-power laser radiation, The particles are dispersed in an inert gas and cooled by a temperature gradient, then synthesized into a gaseous compound and collided to condense into liquid particles, or recrystallized into compound crystal nucleus particles; in the step (6), the compound particles enter the particle growth furnace with the gas flow and further collide and grow; the remaining process flow is the same as the steps (2) to (4) and (7) to (9), and the compound particles grown in the particle growth furnace are then subjected to a quenching and shaping, cooling, and collection process, and the particle size can be accurately graded and controlled to obtain a compound nanopowder with an average particle size of D50 5 to 100 nm.
Citation Information
Cited By
Method and device for preparing nano tin oxide powder by liquid tin feeding plasma equipment
CN122355337A