Composite particle reinforced maritime work steel wire for ultra-large linear energy electro-gas welding and preparation method of composite particle reinforced maritime work steel wire for ultra-large linear energy electro-gas welding
By adding nano-scale La2O3 and ZrO2 to offshore steel welding materials, composite particles are formed, which solves the problems of pores, cracks and inclusions in ultra-large linear energy welding, improves the strength and toughness of welding, and achieves high strength and high toughness. and defect-free welded construction.
Patent Information
- Application Number
- CN202410980588.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Under ultra-large linear energy welding conditions, offshore steel welding materials are prone to produce pores, cracks and inclusions, leading to the coarsening of the welding heat-affected zone and the grains of the weld metal, affecting the strength and toughness of the welded joints, and threatening the safety of the ship structure. and longevity.
The composite particle-reinforced wire material for ultra-large linear energy gas-electric vertical welding of marine steel is used. By adding nano-scale La2O3 and ZrO2 to the flux core powder, the grain growth is suppressed, impurity elements are absorbed, and acicular iron is induced at high temperatures. The body nucleates to form small La-rich and Zr-rich inclusions, which promotes the generation of acicular ferrite at the weld, refines the grains, and reduces the tendency of cracks.
Significantly improve the strength and hardness of the weld metal, enhance the low-temperature toughness, reduce welding defects, obtain high-strength, high-toughness and defect-free marine steel welded structural parts, and extend the service life of the workpiece.
Smart Images

Figure CN118744295A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of welding materials, and in particular to a composite particle reinforced marine steel wire for ultra-large energy line gas-electric vertical welding and a preparation method thereof. Background technology:
[0002] At present, with the development of lightweight, large-scale, environmentally friendly and economical marine engineering structures, there are also higher requirements for the performance and thickness of marine structural steel. It is necessary to increase the thickness of steel and develop the hull steel towards high toughness, high strength and easy weldability. In order to effectively manufacture thick and high-quality marine structural parts, high-energy line welding technologies such as multi-wire submerged arc welding, gas-electric vertical welding and electroslag welding are widely used. For example, the welding heat input of gas-electric vertical welding can reach 600kJ / cm, and single-pass forming can be achieved during the welding process. However, at the same time, under such a large energy line heat input, defects such as pores, cracks and inclusions are easily generated, and the grains of the heat affected zone (HAZ) and weld metal are easily coarsened; in addition, the slow cooling rate after welding may also easily form coarse brittle structures such as side plate ferrite, Widmanstatten structure, and upper bainite during the phase transformation, which affects the strength and toughness of the welded joint, thereby threatening the safe use and life of the ship structure. Therefore, how to improve the strength, low-temperature toughness and weldability of weld microstructure under ultra-large linear energy is an urgent problem that needs to be solved.
[0003] Patent publication number CN104259688B discloses a high-energy gas-electrode vertical welding flux-cored wire and its preparation method. It abandons the traditional calcium fluoride deoxidizer and adopts sodium fluoride, which has better effects on deoxidation, arc stabilization and slag thinning, and adds appropriate amounts of Al and Mg to the flux core, which improves the deoxidation ability of the alloy and increases the slag removal effect during welding. The weld metal prepared by this high-energy gas-electrode vertical welding flux-cored wire is uniformly clad and the weld is well formed, which is suitable for thick plate welding. However, the mechanical properties and toughness of the metal at the high-energy weld are not significantly improved.
[0004] The invention with patent publication number CN109530961B discloses a flux-cored welding wire for gas shielded high-energy-line welding and its preparation method and application. This invention selects low-carbon steel strip as the coating, and the flux core accounts for 13.0-13.5% of the total mass of the welding wire; the flux core includes the following components and the mass percentage of the flux cored welding wire: TiO2: 5.0-5.6%, SiO2: 0.3-0.6%, Al2O3: 0.15-0.25%, NaF: 0.2-0.3%, Mg-Al alloy: 0.4-0.5%, Si: 0.4-0.5%, Mn: 2.0-2.5%, Ti: 0.04-0.11%, B: 0.009-0.01%, Fe and other inevitable impurities are the remainder. The shielding gas during welding is CO2, the welding current is 260-280A, the welding voltage is 27-28V, the line energy is 16-20kJ / cm, the interpass temperature is 135-165°C, and the yield strength ratio of the deposited metal is not higher than 0.83. The present invention optimizes the plasticity of the weld metal, reduces the generation of cracks at the weld, and controls the yield strength ratio of the alloy by optimizing the composition of the flux-cored wire. However, the welding heat input used in the patent is relatively low, and the effect under ultra-large line energy welding conditions is unknown.
[0005] Therefore, it is necessary to design a wire for ultra-high energy wire gas-electric vertical welding of marine engineering steel, which can effectively reduce defects such as pores, cracks and inclusions in the alloy during large energy wire welding under ultra-high energy wire welding conditions, improve the formability of the weld and the strength, low-temperature toughness and weldability of the weld structure under ultra-high energy wire, and obtain marine engineering steel welded structures with high strength, high toughness and no defects. Summary of the invention:
[0006] The purpose of the present invention is to provide a composite particle reinforced marine steel wire for ultra-large line energy gas-electric vertical welding and a preparation method thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A composite particle reinforced wire for super-large linear energy gas-electric vertical welding of marine engineering steel is composed of an outer steel strip and an inner flux core powder. The flux core powder filling rate is 20-30%. The flux core powder includes components and their mass percentages in the flux core welding wire are as follows: TiO2: 5.0-5.6%, SiO2: 0.32-0.64%, NaF: 0.18-0.3%, Al: 0.36-0.48%, Si: 0.28-0.5%, Mn: 1.3-1.7%, Ni: 2-4%, Mo: 1.8-3.6%, Ti: 0.1-0.3%, ZrO2: 0.05-0.2%, B: 0.009-0.01%, La2O3: 0.3-0.85%, and the balance is Fe and unavoidable impurities.
[0009] Preferably, the nano-scale ZrO2 content in the core powder is 0.1-0.2%, and the nano-scale La2O3 content is 0.36-0.82%.
[0010] Preferably, the wire diameter is 1.6 mm.
[0011] The addition of cheap nano-scale La2O3 can pin the original austenite grain boundary movement during high temperature welding, inhibit grain growth, and absorb impurity elements such as S and P in the weld metal to improve cleanliness. At the same time, the co-added ZrO2 is very stable at high temperatures and can act as a nucleation point during the cooling of the weld metal to induce the nucleation of acicular ferrite (AF). By adding nano-scale La2O3 and ZrO2 composite reinforcement particles, a large number of fine and dispersed La-rich and Zr-rich inclusions are formed, which on the one hand promotes the formation of acicular ferrite (AF) at the weld, and on the other hand refines the grains, reduces the tendency of welding cracks, inhibits the expansion of cracks during low-temperature impact, and greatly improves the strength and hardness of the cladding metal under ultra-high line energy welding (heat input ≥600kJ / cm). While the strength of the weld metal is improved, it also has excellent low-temperature toughness, which increases its service life, and finally obtains a marine steel welded structure with high strength, high toughness and no defects.
[0012] In the core powder, TiO2, SiO2 and NaF are slag-forming agents, which can protect the molten pool and stabilize the arc on the one hand, and adjust the viscosity and alkalinity of the molten pool on the other hand.
[0013] The particle size of other raw material powders in the core powder except nano-sized La2O3 and nano-sized ZrO2 is 60 meshes to 100 meshes.
[0014] The preparation steps of the composite particle reinforced marine steel wire for ultra-large energy line gas electric vertical welding include the following steps:
[0015] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through a 80-mesh sieve. According to the required proportions, nano-scale La2O3, ZrO2 powder, Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill to mix the powders. The ball milling parameters are a ball-to-material ratio of 5:1, a ball milling time of 1-2 hours in forward rotation and 1-2 hours in reverse rotation, and a rotation speed of 300 r / min to obtain a mixed powder after ball milling.
[0016] Step S2: TiO2, SiO2, and NaF slag-forming agents are mixed with the ball-milled mixed powder in a predetermined ratio, and the mixture is placed in a V-type mixer, and mixed for 30 minutes to obtain a uniformly mixed core powder;
[0017] Step S3: First, dry the low-carbon steel strip, then use a forming roller to roll the strip into a U shape, add the mixed flux-cored powder into the U-shaped strip according to the required filling rate through a powder feeding device, and then further roll it into a tube; then feed the tubular welding wire into a drawing die, control the drawing rate to 1.2-1.5m / min for drawing, repeat the above operation for re-drawing, until the required flux-cored welding wire with a diameter of 1.6mm is obtained.
[0018] The present invention also protects the application of the above-mentioned welding wire in the ultra-large linear energy welding of thick marine steel. The ultra-large linear energy welding is double-wire gas-electric vertical welding. The base material is EH36 grade marine steel with a thickness of 50-60 mm. The base material groove is designed as a single-sided V-shaped groove. The single-sided groove angle is 12°, the gap is 8-10 mm, the blunt edge groove is not greater than 1 mm, the dry extension of the two welding wires is 35 mm, the welding gun angle is 4°~8°, the distance from the rear wire to the pad is 20 mm, and the spacing between the two welding wires is 19 mm. The welding process parameters are as follows: the rear wire is connected by DC positive connection, fixed without swinging, the current is 450.1-481.9A, and the voltage is 40.2-42.3V; the front wire is connected by DC reverse connection, the swing width is 15-18mm, the current is 473.9-501.8A, and the voltage is 48.9-52.8; the speed is 6-7cm / min, the heat input is 606.7-781.3kJ / cm, and the entire welding process is carried out under 100% CO2 gas protection conditions.
[0019] The beneficial effects of the present invention are as follows:
[0020] 1) The present invention forms a large number of fine and dispersed La-rich and Zr-rich inclusions by jointly adding nano-scale La2O3 and ZrO2 composite reinforcing particles, which, on the one hand, promotes the formation of acicular ferrite (AF) at the weld, and on the other hand, refines the grains, reduces the tendency of welding cracks, and inhibits the expansion of cracks during low-temperature impact. The strength and hardness of the cladding metal under ultra-large linear energy welding (heat input ≥ 600kJ / cm) are greatly improved. While the strength of the weld metal is improved, it also has excellent low-temperature toughness, which increases its service life, and finally obtains a marine steel welded structure with high strength, high toughness and no defects.
[0021] 2) The welding wire of the present invention has the advantages of small welding spatter, high cladding speed, beautiful weld formation, and can be used for all-position welding. After double-wire gas-electric vertical welding, the weld formation effect is good, without defects such as cracks, pores and inclusions; the weld metal obtained by using the welding wire of the present invention under the conditions of ultra-large line energy welding (heat input ≥600kJ / cm) can still maintain high toughness, greatly increase the service life of the workpiece, and help save costs. Description of the drawings:
[0022] Figure 1This is the microstructure of the welding wire obtained in Example 1.
[0023] Figure 2 This is the microstructure of the welding wire obtained in Comparative Example 1. Specific implementation method:
[0024] The following is a further description of the present invention, rather than a limitation of the present invention.
[0025] Example 1: A composite particle reinforced marine steel wire for ultra-high energy line gas electric welding and its preparation method and application
[0026] A composite particle reinforced marine steel super-high energy line gas electric vertical welding wire for EH36 ship plate steel, which is composed of an outer commercial H08A low-carbon steel strip and an inner flux core powder. The flux core powder includes the following components and their mass percentages in the flux core welding wire: TiO2: 5.2%, SiO2: 0.48%, NaF: 0.24%, Al: 0.42%, Si: 0.38%, Mn: 1.5%, Ni: 3.1%, Mo: 2.2%, Ti: 0.15%, B: 0.009%, La2O3: 0.8%, ZrO2: 0.1%, and the balance is Fe and some inevitable impurities.
[0027] The specific steps of the preparation method of composite particle reinforced marine steel wire for ultra-large wire energy gas-electric vertical welding are as follows:
[0028] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through a 80-mesh sieve. According to the required proportions, nano-scale La2O3, ZrO2 powder, Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill to mix the powders. The ball milling parameters are a ball-to-material ratio of 5:1, a ball milling time of 1 h forward and 1 h reverse, and a rotation speed of 300 r / min to obtain a mixed powder after ball milling.
[0029] Step S2: TiO2, SiO2, and NaF slag-forming agents are mixed with the ball-milled mixed powder in a predetermined ratio, put into a V-type mixer, and mixed for 30 minutes to obtain a uniformly mixed core powder.
[0030] Step S3: First, dry the low-carbon steel strip (commercial H08A), then use a forming roller to roll the steel strip into a U shape, add the mixed flux-cored powder into the U-shaped steel strip according to the required filling rate through a powder feeding device, and then further roll it into a tube; then feed the tubular welding wire into a drawing die, control the drawing rate to 1.2 m / min for drawing, repeat the above operation for re-drawing, until the required flux-cored welding wire with a diameter of 1.6 mm is obtained.
[0031] The prepared flux-cored welding wire was used for double-wire gas-electric vertical welding according to the following process parameters. The base material was EH36 grade marine steel with a thickness of 60 mm. The base material groove was designed as a single-sided V-shaped groove with a single-sided groove angle of 12°, a gap of 8 mm, a blunt edge of 1 mm groove, a dry extension of the two welding wires of 35 mm, a welding gun angle of 4°°, a distance from the rear wire to the pad of 20 mm, and a spacing of the two welding wires of 19 mm. The welding process parameters were: the rear wire was a DC positive connection method, fixed without swinging, a current of 450.1 A, and a voltage of 40.2 V; the front wire was a DC reverse connection method, with a swing width of 15 mm, a current of 473.9 A, and a voltage of 48.9; the speed was 6 cm / min, and the heat input was 606.7 kJ / cm. The entire welding process was carried out under 100% CO2 gas protection conditions.
[0032] Embodiment 2:
[0033] The present embodiment provides a composite particle reinforced marine steel super high wire energy gas electric vertical welding wire for EH36 ship plate steel, which is composed of an outer commercial H08A low carbon steel strip and an inner flux core powder. The flux core powder includes components and their mass percentages of the flux cored welding wire are as follows: TiO2: 5.0%, SiO2: 0.4%, NaF: 0.18%, Al: 0.38%, Si: 0.29%, Mn: 1.4%, Ni: 3.5%, Mo: 2.4%, Ti: 0.2%, B: 0.009%, La2O3: 0.6%, ZrO2: 0.05%, and the balance is Fe and some unavoidable impurities.
[0034] The specific steps of the method for preparing composite particle reinforced marine steel wire for ultra-large wire energy gas-electric vertical welding are as follows:
[0035] Step S1: After the core powder raw material is dehydrated and dried, it is sieved through an 80-mesh sieve. According to the required proportions, nano-scale La2O3, ZrO2 powder, Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill to mix the powders. The ball milling parameters are a ball-to-material ratio of 5:1, a ball milling time of 2 h forward and 2 h reverse, and a rotation speed of 300 r / min to obtain a mixed powder after ball milling.
[0036] Step S2: TiO2, SiO2, and NaF slag-forming agents are mixed with the ball-milled mixed powder in a predetermined ratio, put into a V-type mixer, and mixed for 30 minutes to obtain a uniformly mixed core powder.
[0037] Step S3: First, dry the low-carbon steel strip (commercial H08A), then use a forming roller to roll the steel strip into a U shape, add the mixed flux-cored powder into the U-shaped steel strip according to the required filling rate through a powder feeding device, and then further roll it into a tube; then feed the tubular welding wire into a drawing die, control the drawing rate to 1.5 m / min for drawing, repeat the above operation for re-drawing, until the required flux-cored welding wire with a diameter of 1.6 mm is obtained.
[0038] The prepared flux-cored welding wire was used to perform twin-wire gas-electric vertical welding according to the process parameters described in Example 1.
[0039] Embodiment 3:
[0040] Provided in this embodiment is a composite particle reinforced marine steel super high wire energy gas electric vertical welding wire for EH36 ship plate steel, which is composed of an outer commercial H08A low carbon steel strip and an inner flux core powder. The flux core powder includes components and their mass percentages of the flux cored welding wire are as follows: TiO2: 5.6%, SiO2: 0.64%, NaF: 0.25%, Al: 0.39%, Si: 0.41%, Mn: 1.6%, Ni: 3.3%, Mo: 2.4%, Ti: 0.2%, B: 0.01%, La2O3: 0.3%, ZrO2: 0.06%, and the remainder is Fe and some unavoidable impurities.
[0041] The preparation method of composite particle reinforced marine steel wire for ultra-high energy line gas electric vertical welding is the same as that in Example 1.
[0042] The prepared flux-cored welding wire was used to perform twin-wire gas-electric vertical welding according to the process parameters described in Example 1.
[0043] Embodiment 4:
[0044] Provided in this embodiment is a composite particle reinforced marine steel super high energy wire gas electric vertical welding wire for EH36 ship plate steel, which is composed of an outer commercial H08A low carbon steel strip and an inner flux core powder. The flux core powder includes components and their mass percentages of the flux cored welding wire are as follows: TiO2: 5.1%, SiO2: 0.52%, NaF: 0.3%, Al: 0.39%, Si: 0.38%, Mn: 1.4%, Ni: 4%, Mo: 2.2%, Ti: 0.25%, B: 0.009%, La2O3: 0.36%, ZrO2: 0.19%, and the remainder is Fe and some unavoidable impurities.
[0045] The preparation method of composite particle reinforced marine steel wire for ultra-high energy line gas electric vertical welding is the same as that in Example 1.
[0046] The prepared flux-cored welding wire was used to perform twin-wire gas-electric vertical welding according to the process parameters described in Example 1.
[0047] Embodiment 5:
[0048] Provided in this embodiment is a wire for super-high energy gas-electric welding of EH36 ship plate steel, a composite particle reinforced marine steel, which is composed of an outer commercial H08A low-carbon steel strip and an inner flux-cored powder. The flux-cored powder includes the following components and their mass percentages of the flux-cored welding wire: TiO2: 5.3%, SiO2: 0.57%, NaF: 0.22%, Al: 0.42%, Si: 0.36%, Mn: 1.6%, Ni: 3.8%, Mo: 3.6%, Ti: 0.3%, B: 0.009%, La2O3: 0.82%, ZrO2: 0.20%, and the remainder is Fe and some unavoidable impurities.
[0049] The preparation method of composite particle reinforced marine steel wire for ultra-high energy line gas electric vertical welding is the same as that in Example 1.
[0050] The prepared flux-cored welding wire was used to perform twin-wire gas-electric vertical welding according to the process parameters described in Example 1.
[0051] Comparative Example 1:
[0052] Refer to Example 1, the difference is that the core powder does not contain La2O3 and ZrO2, and the other preparation processes are the same.
[0053] Comparative Example 2:
[0054] Refer to Example 1, the difference is that the core powder does not contain La2O3, and the other preparation processes are the same.
[0055] Comparative Example 3:
[0056] Refer to Example 1, the difference is that the core powder does not contain ZrO2, and the other preparation processes are the same.
[0057] The weld performance after the butt welding obtained in Examples 1-5 and Comparative Examples 1-3 was tested, and the test method was based on GB / T 2652 "Weld and Cladding Metal Tensile Test Method" and GB / T 2650 "Weld Joint Impact Test Method". The impact test was carried out on an Instron Dynatup 9200 series drop hammer impact tester at a test temperature of -40°C. The results are shown in Table 1.
[0058] From the comparison of the data of Example 1 and Comparative Examples 1-3 in Table 1, it can be seen that the synergistic effect of La2O3 and ZrO2 in the present invention greatly improves the tensile properties and impact energy of the weld after twin-wire gas-electrode vertical welding.
[0059] Table 1 Tensile properties and impact energy of welds after double-wire gas-electrode vertical welding of flux-cored welding wire in the embodiments and comparative examples
[0060]
[0061] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite particle reinforced marine steel wire for ultra-large energy line gas electric vertical welding, characterized in that: The invention is composed of an outer steel strip and an inner flux core powder, the filling rate of the flux core powder is 20-30%, the flux core powder comprises the following components and their mass percentages in the flux core welding wire are as follows: TiO2: 5.0-5.6%, SiO2: 0.32-0.64%, NaF: 0.18-0.3%, Al: 0.36-0.48%, Si: 0.28-0.5%, Mn: 1.3-1.7%, Ni: 2-4%, Mo: 1.8-3.6%, Ti: 0.1-0.3%, ZrO2: 0.05-0.2%, B: 0.009-0.01%, La2O3: 0.3-0.85%, and the balance is Fe and unavoidable impurities.
2. The composite particle reinforced marine steel super high energy line gas electric vertical welding wire according to claim 1, characterized in that: The content of nanometer-scale ZrO2 in the core powder is 0.1-0.2%, and the content of nanometer-scale La2O3 is 0.36-0.82%.
3. The composite particle reinforced marine steel super high energy line gas electric vertical welding wire according to claim 1, characterized in that: The wire diameter is 1.6 mm.
4. The composite particle reinforced marine steel super high energy line gas electric vertical welding wire according to claim 1, characterized in that: The particle size of other raw material powders in the core powder except nano-sized La2O3 and nano-sized ZrO2 is 60 meshes to 100 meshes.
5. The preparation process of the composite particle reinforced marine steel super high energy line gas electric vertical welding wire according to claim 1, characterized in that: The steps include: Step S1: After the core powder raw material is dehydrated and dried, it is sieved through a 80-mesh sieve. According to the required proportions, nano-scale La2O3, ZrO2 powder, Al, Si, Mn, Ni, Mo, Ti, B and iron powder are added to a ball mill to mix the powders. The ball milling parameters are a ball-to-material ratio of 5:1, a ball milling time of 1-2 hours in forward rotation and 1-2 hours in reverse rotation, and a rotation speed of 300 r / min to obtain a mixed powder after ball milling. Step S2: TiO2, SiO2, and NaF slag-forming agents are mixed with the ball-milled mixed powder in a predetermined ratio, and the mixture is placed in a V-type mixer, and mixed for 30 minutes to obtain a uniformly mixed core powder; Step S3: First, dry the low-carbon steel strip, then use a forming roller to roll the strip into a U shape, add the mixed flux-cored powder into the U-shaped strip according to the required filling rate through a powder feeding device, and then further roll it into a tube; then feed the tubular welding wire into a drawing die, control the drawing rate to 1.2-1.5m / min for drawing, repeat the above operation for re-drawing, until the required flux-cored welding wire with a diameter of 1.6mm is obtained.
6. Application of the welding wire material according to claim 1 in ultra-high energy input welding of thick marine engineering steel, characterized in that: The ultra-large line energy welding is double-wire gas-electric vertical welding, the base material is EH36 grade marine steel, the thickness is 50-60mm, the base material groove form is designed as a single-sided V-shaped groove, the single-sided groove angle is 12°, the gap is 8-10mm, the blunt groove is not more than 1mm, the dry extension of the two welding wires is 35mm, the welding gun angle is 4°~8°, the distance from the rear wire to the pad is 20mm, and the spacing between the two welding wires is 19mm; the welding process parameters are: The rear wire is connected by DC positive connection, fixed without swinging, with a current of 450.1-481.9A and a voltage of 40.2-42.3V; the front wire is connected by DC reverse connection, with a swing width of 15-18mm, a current of 473.9-501.8A and a voltage of 48.9-52.8; the speed is 6-7cm / min, and the heat input is 606.7-781.3kJ / cm. The entire welding process is carried out under 100% CO2 gas protection conditions.