Titanium dioxide-containing high-flame-retardant copper-clad plate and preparation method thereof
By adding materials such as nano-titanium dioxide and magnesium hydroxide to the modified impregnating material of the copper-clad laminate, combined with ultrasonic treatment and blending technology, the problems of halogen pollution and insufficient flame retardant performance in the existing technology are solved, and efficient halogen-free products are achieved. The preparation of flame-retardant and environmentally friendly high flame-retardant copper-clad laminates improves the fire resistance and flame retardant effect of the material.
Patent Information
- Application Number
- CN202410750740.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flame-retardant copper-clad laminates use halogen in the flame-retardant design, which causes environmental pollution, and the flame-retardant performance is insufficient, making it difficult to meet the environmentally friendly halogen-free flame-retardant design requirements.
A highly flame-retardant copper-clad laminate containing titanium dioxide is used. Nano-titanium dioxide, magnesium hydroxide, flexible phosphate and other materials are added to the modified impregnating material, followed by ultrasonic treatment and uniform blending, and combined with dicyandiamide solution and epoxy resin to form Efficient flame retardant, and high flame retardant copper clad laminates are prepared through hot pressing molding technology.
It achieves halogen-free flame retardancy, improves the flame retardant performance, reduces environmental pollution, enhances the fire resistance and flame retardant effect of the copper clad laminate, reduces the fire risk, and promotes the density and strength of the material.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminates, and more specifically to a highly flame-retardant copper clad laminate containing titanium dioxide and a preparation method thereof. Background Art
[0002] Copper clad laminate is mainly a plate-like material made by impregnating electronic glass fiber cloth or other reinforcing materials with resin material, covering one or both sides with copper foil and hot pressing. It is referred to as copper clad laminate.
[0003] The patent (CN113698738B) discloses a flame-retardant copper-clad laminate and a preparation method thereof. The materials required for the flame-retardant copper-clad laminate include, by weight: 100-150 parts of phosphorus-bromine epoxy resin, 20-35 parts of curing agent, 80-120 parts of acetone, 3-7 parts of accelerator, and 60-100 parts of composite flame retardant. The materials required for the composite flame retardant include, by weight: 40-70 parts of modified PET composite material, 30-50 parts of modified magnesium hydroxide, and 30-50 parts of modified aluminum hydroxide. The phosphorus-bromine epoxy resin uses phosphorus-based and bromine-based flame retardants in coordination to enhance the flame retardancy of the epoxy resin. The composite flame retardant has high-efficiency flame retardancy, thermal stability and heat resistance.
[0004] The flame-retardant copper clad laminate in the above patent uses phosphorus-bromine epoxy resin containing halogen as its main raw material, which does not meet the current design requirements for environmentally friendly halogen-free flame retardancy in terms of flame retardancy design and will cause environmental pollution during flame retardancy. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a highly flame-retardant copper-clad laminate containing titanium dioxide and a preparation method thereof.
[0006] A highly flame-retardant copper-clad laminate containing titanium dioxide comprises an electronic glass fiber cloth, a modified impregnating material and a copper foil, wherein the modified impregnating material contains titanium dioxide, the electronic glass fiber cloth is impregnated and cured in the modified impregnating material, and then the copper foil is hot-pressed into shape; the weight ratio of the electronic glass fiber cloth to the modified impregnating material is 1:6-8.
[0007] Furthermore, the modified impregnating material comprises, by weight percentage, 23-27% of a modified flame retardant, 23-27% of a dicyandiamide solution, 2.7-3.3% of a curing accelerator, and the remainder being epoxy resin.
[0008] Furthermore, the modified flame retardant comprises, by weight percentage, 9.6-10.4% of nanocellulose, 34-38% of flexible phosphate, 3.6-4.4% of nano titanium dioxide, 0.3-0.5% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0009] Furthermore, the weight ratio of the electronic glass fiber cloth to the modified impregnating material is 1:7; the modified impregnating material includes, by weight percentage, 24-26% of a modified flame retardant, 24-26% of a dicyandiamide solution, 2.9-3.1% of a curing accelerator, and the rest is an epoxy resin; the modified flame retardant includes, by weight percentage, 9.8-10.2% of nanocellulose, 35-37% of a flexible phosphate ester, 3.8-4.2% of nano titanium dioxide, 0.35-0.45% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0010] Furthermore, the weight ratio of the electronic glass fiber cloth to the modified impregnating material is 1:7; the modified impregnating material includes, by weight percentage: 25% of a modified flame retardant, 25% of a dicyandiamide solution, 3.0% of a curing accelerator, and the rest is an epoxy resin; the modified flame retardant includes, by weight percentage: 10.0% of nanocellulose, 36% of a flexible phosphate ester, 4.0% of nano titanium dioxide, 0.4% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0011] Furthermore, the solid content of the dicyandiamide solution is 10.3-10.7%.
[0012] The present invention also provides a method for preparing a highly flame-retardant copper-clad laminate containing titanium dioxide, and the specific preparation steps are as follows:
[0013] Step 1: weighing the dicyandiamide solution, curing accelerator, epoxy resin in the modified impregnating material raw material and the nanocellulose, flexible phosphate, nano titanium dioxide, 3-aminopropyltriethoxysilane, and magnesium hydroxide in the modified flame retardant raw material;
[0014] Step 2: Add the nano titanium dioxide in step 1 to anhydrous ethanol, perform ultrasonic treatment for 10 to 20 minutes, add 3-aminopropyltriethoxysilane and one-fifth of the weight of nanocellulose, continue the ultrasonic treatment for 30 to 50 minutes, centrifuge, wash, and dry to obtain material a;
[0015] Step 3: Evenly blend the remaining nanocellulose, flexible phosphate, magnesium hydroxide and material a in step 2 to obtain a modified flame retardant;
[0016] Step 4: subjecting the modified flame retardant prepared in step 3 to the dicyandiamide solution, curing accelerator and epoxy resin prepared in step 1 to shear treatment for 30 to 40 minutes, and simultaneously subjecting the modified flame retardant prepared in step 3 to ultrasonic treatment to obtain a modified impregnated material;
[0017] Step 5: insert the electronic glass fiber cloth into the modified impregnating material, impregnate for 30 to 40 minutes, and bake the impregnated electronic glass fiber cloth to obtain a prepreg;
[0018] Step 6: Hot-press the copper foil to both sides of the prepreg to obtain a highly flame-retardant copper-clad laminate containing titanium dioxide.
[0019] Furthermore, in step 2, the weight ratio of nano-titanium dioxide to ethanol solution is 1:30-50; anhydrous ethanol is used for washing and drying is performed at 80-90° C.; the ultrasonic frequency is 40-60 KHz and the ultrasonic power is 800-1000 W.
[0020] Further, in step three, a blending operation is performed using a mixer with a stirring speed of 1200 to 1600 r / min; in step four, shearing is performed by pipeline high-speed shearing treatment with a high-speed shear rate of 4400 to 4600 r / min, an ultrasonic frequency of 1.4 to 1.6 MHz, and an ultrasonic power of 500 to 600 W; in step six, hot pressing is performed at 240 to 260° C. with a pressure of 44.0 to 46.0 kg / m 2 .
[0021] Furthermore, in step 2, the weight ratio of nano-titanium dioxide to ethanol solution is 1:40; anhydrous ethanol is used for washing and drying at 85°C; the ultrasonic frequency is 50KHz and the ultrasonic power is 900W; in step 3, a blending operation is performed using a stirrer with a stirring speed of 1400r / min; in step 4, shearing is performed through pipeline high-speed shearing, with a high-speed shear rate of 4500r / min, an ultrasonic frequency of 1.5MHz, and an ultrasonic power of 550W; in step 6, hot pressing is performed at 250°C with a pressure of 45.0kg / m 2 .
[0022] Technical effects and advantages of the present invention:
[0023] 1. The high flame retardant copper clad laminate containing titanium dioxide processed by the raw material formula of the present invention does not use halogen in the raw materials, so the halogen-free flame retardant and environmental protection requirements are achieved, and the flame retardant performance can be effectively improved to reduce pollution to the environment; the nano titanium dioxide can be surface modified to effectively enhance the dispersion uniformity of the nano titanium dioxide in the modified impregnating material; the nano titanium dioxide can play a synergistic flame retardant role, improve the flame retardant effect of the flame retardant, slow down the combustion and spread of the copper clad laminate, and reduce the fire hazard; the addition of nano titanium dioxide can promote the combustion of the internal materials of the copper clad laminate to char, and the flame retardant synergy improves the strength of the internal materials of the copper clad laminate, making the internal materials of the copper clad laminate dense, and can effectively block the internal combustible gas and the external oxygen, delay the transfer of heat, and promote the improvement of the fire resistance of the material; the modified Adding an appropriate amount of nano-titanium dioxide to the modified impregnation material helps to form a continuous and dense flaky carbon layer during combustion, and improves the defects and holes of the carbon layer; using polyphosphate and nano-titanium dioxide as raw materials to synthesize a nano-composite flexible PPE flame retardant, adding nano-titanium dioxide can effectively improve the carbon-forming ability and flame retardant and smoke suppression properties of the coating; magnesium hydroxide can interact with the hydrophilic hydroxyl groups on the surface of nanocellulose, so that it can be better dispersed in the modified impregnation material. Although nanocellulose has no flame retardant function, its presence can improve the dispersibility of magnesium hydroxide, so that it can be evenly dispersed in the modified impregnation material; magnesium hydroxide is the main component of the modified flame retardant. The magnesium oxide produced by the decomposition of magnesium hydroxide covers the surface of the polymer, which can prevent heat conduction and radiation, and isolate oxygen, thereby improving the flame retardant properties of the polymer;
[0024] 2. In the process of processing a high flame retardant copper-clad laminate containing titanium dioxide, the present invention adds nano titanium dioxide into anhydrous ethanol for ultrasonic treatment, which can effectively disperse the nano titanium dioxide in anhydrous ethanol and effectively ensure the subsequent modification effect of the nano titanium dioxide. 3-aminopropyl triethoxysilane and nanocellulose are added, and 3-aminopropyl triethoxysilane and nanocellulose can modify the surface of the nano titanium dioxide. At the same time, ultrasonic treatment is performed, which can effectively enhance the surface modification effect of the nano titanium dioxide. , flexible phosphate, magnesium hydroxide and surface-modified nano titanium dioxide are blended to effectively blend the modified flame retardant evenly and ensure the mixing effect of subsequent materials; the modified flame retardant is sheared with dicyandiamide solution, curing accelerator and epoxy resin, and ultrasonically treated at the same time to effectively ensure the uniform mixing and distribution of the raw materials in the modified impregnating material; the electronic glass fiber cloth is inserted into the modified impregnating material for impregnation treatment, and a semi-cured sheet is made after baking; the copper foil is hot-pressed and compounded to both sides of the semi-cured sheet to obtain a highly flame-retardant copper clad laminate containing titanium dioxide. DETAILED DESCRIPTION
[0025] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Embodiment 1:
[0027] The invention provides a highly flame-retardant copper-clad laminate containing titanium dioxide, comprising an electronic glass fiber cloth, a modified impregnating material and a copper foil, wherein the modified impregnating material contains titanium dioxide, and after the electronic glass fiber cloth is impregnated and cured in the modified impregnating material, the copper foil is hot-pressed and formed; the weight ratio of the electronic glass fiber cloth to the modified impregnating material is 1:7; the modified impregnating material comprises, by weight percentage, 23% of a modified flame retardant, 23% of a dicyandiamide solution, 2.7% of a curing accelerator, and the remainder is an epoxy resin; the modified flame retardant comprises, by weight percentage, 9.6% of nanocellulose, 34% of a flexible phosphate, 3.6% of nano titanium dioxide, 0.3% of 3-aminopropyltriethoxysilane, and the remainder is magnesium hydroxide;
[0028] The solid content of the dicyandiamide solution is 10.5%;
[0029] The present invention also provides a method for preparing a highly flame-retardant copper-clad laminate containing titanium dioxide, and the specific preparation steps are as follows:
[0030] Step 1: weighing the dicyandiamide solution, curing accelerator, epoxy resin in the modified impregnating material raw material and the nanocellulose, flexible phosphate, nano titanium dioxide, 3-aminopropyltriethoxysilane, and magnesium hydroxide in the modified flame retardant raw material;
[0031] Step 2: Add the nano titanium dioxide in step 1 to anhydrous ethanol, perform ultrasonic treatment for 15 minutes, add 3-aminopropyltriethoxysilane and one-fifth of the weight of nanocellulose, continue ultrasonic treatment for 40 minutes, centrifuge, wash, and dry to obtain material a;
[0032] Step 3: Evenly blend the remaining nanocellulose, flexible phosphate, magnesium hydroxide and material a in step 2 to obtain a modified flame retardant;
[0033] Step 4: subjecting the modified flame retardant prepared in step 3, the dicyandiamide solution prepared in step 1, the curing accelerator, and the epoxy resin to shear treatment for 35 minutes, and simultaneously subjecting the modified flame retardant prepared in step 3 to ultrasonic treatment to obtain a modified impregnated material;
[0034] Step 5: insert the electronic glass fiber cloth into the modified impregnating material, impregnate for 35 minutes, and bake the impregnated electronic glass fiber cloth to obtain a prepreg;
[0035] Step 6: Hot-press the copper foil to both sides of the prepreg to obtain a highly flame-retardant copper-clad laminate containing titanium dioxide.
[0036] In step 2, the weight ratio of nano-titanium dioxide and ethanol solution is 1:30; anhydrous ethanol is used for washing and drying at 80°C; the ultrasonic frequency is 40KHz and the ultrasonic power is 800W; in step 3, a blending operation is performed using a stirrer with a stirring speed of 1200r / min; in step 4, shearing is performed through pipeline high-speed shearing, with a high-speed shear rate of 4400r / min, an ultrasonic frequency of 1.4MHz, and an ultrasonic power of 500W; in step 6, hot pressing is performed at 240°C with a pressure of 44.0kg / m 2 .
[0037] Embodiment 2:
[0038] Different from Example 1, the modified impregnating material includes, by weight percentage, 27% of modified flame retardant, 27% of dicyandiamide solution, 3.3% of curing accelerator, and the rest is epoxy resin; the modified flame retardant includes, by weight percentage, 10.4% of nanocellulose, 38% of flexible phosphate, 4.4% of nano titanium dioxide, 0.5% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0039] Embodiment 3:
[0040] Different from Examples 1-2, the modified impregnating material comprises, by weight percentage, 25% of a modified flame retardant, 25% of a dicyandiamide solution, 3.0% of a curing accelerator, and the remainder is an epoxy resin; the modified flame retardant comprises, by weight percentage, 10.0% of nanocellulose, 36% of a flexible phosphate ester, 4.0% of nano titanium dioxide, 0.4% of 3-aminopropyltriethoxysilane, and the remainder is magnesium hydroxide.
[0041] Embodiment 4:
[0042] The difference from Example 3 is that in step 2, the weight ratio of nano-titanium dioxide and ethanol solution is 1:40; anhydrous ethanol is used for washing and drying at 85°C; the ultrasonic frequency is 50KHz and the ultrasonic power is 900W; in step 3, a blending operation is performed using a stirrer with a stirring speed of 1400r / min; in step 4, shearing is performed through a pipeline high-speed shearing process with a high-speed shear rate of 4500r / min, an ultrasonic frequency of 1.5MHz and an ultrasonic power of 550W; in step 6, hot pressing is performed at 250°C with a pressure of 45.0kg / m 2 .
[0043] Comparative Example 1:
[0044] Different from Example 4, the modified impregnating material includes, by weight percentage, 25% of a modified flame retardant, 25% of a dicyandiamide solution, 3.0% of a curing accelerator, and the rest is an epoxy resin; the modified flame retardant includes, by weight percentage, 10.0% of nanocellulose, 36% of a flexible phosphate ester, 0.4% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0045] Comparative Example 2:
[0046] Different from Example 4, the modified impregnating material includes, by weight percentage, 25% of a modified flame retardant, 25% of a dicyandiamide solution, 3.0% of a curing accelerator, and the rest is an epoxy resin; the modified flame retardant includes, by weight percentage, 36% of a flexible phosphate ester, 4.0% of nano-titanium dioxide, 0.4% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
[0047] Comparative Example 3:
[0048] Different from Example 4, the preparation method of the highly flame-retardant copper-clad laminate containing titanium dioxide has the following specific preparation steps:
[0049] Step 1: weighing the dicyandiamide solution, curing accelerator, epoxy resin in the modified impregnating material raw material and the nanocellulose, flexible phosphate, nano titanium dioxide, 3-aminopropyltriethoxysilane, and magnesium hydroxide in the modified flame retardant raw material;
[0050] Step 2: Evenly blend the nano titanium dioxide, nano cellulose, 3-aminopropyltriethoxysilane, flexible phosphate and magnesium hydroxide in step 1 to obtain a modified flame retardant;
[0051] Step 3: subjecting the modified flame retardant prepared in step 2, the dicyandiamide solution prepared in step 1, the curing accelerator, and the epoxy resin to shear treatment for 30 to 40 minutes, and simultaneously subjecting the modified flame retardant prepared in step 2 to ultrasonic treatment to obtain a modified impregnated material;
[0052] Step 4: insert the electronic glass fiber cloth into the modified impregnating material, impregnate for 30 to 40 minutes, and bake the impregnated electronic glass fiber cloth to obtain a semi-cured sheet;
[0053] Step 5: hot-pressing and laminating the copper foil to both sides of the prepreg to obtain a highly flame-retardant copper-clad laminate containing titanium dioxide;
[0054] In step 2, a blending operation is performed using a mixer with a stirring speed of 1400 r / min; in step 3, shearing is performed through a pipeline high-speed shearing process with a high-speed shear rate of 4500 r / min, an ultrasonic frequency of 1.5 MHz, and an ultrasonic power of 550 W; in step 5, hot pressing is performed at 250°C with a pressure of 45.0 kg / m 2 .
[0055] In the above comparative examples and embodiments: dicyandiamide was purchased from Shanghai Yuanye Biotechnology Co., Ltd., item number: S26828; epoxy resin was purchased from Wuhan Prov Biotechnology Co., Ltd. hydrogenated bisphenol A epoxy resin, item number: 0002; nanocellulose was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., item number: lnb-1130; flexible phosphate was purchased from Xi'an Qiyue Biotechnology Co., Ltd., item number: 2353252; nano titanium dioxide was purchased from Hubei Wei's Chemical Reagent Co., Ltd., item number: HBWS-N123; 3-aminopropyltriethoxysilane was purchased from Hubei Shiteng Chemical Technology Co., Ltd., item number: 0231; magnesium hydroxide was purchased from Shandong Guangxun Chemical Co., Ltd.;
[0056] The high flame retardant copper clad laminate containing titanium dioxide in the comparative example and the embodiment of the present invention was tested, and the size of the copper clad laminate specimen was 100mm×100mm×5mm; the flame retardant performance of the composite material was tested using a cone calorimeter (Zhongnuo ZY6243 model): referring to GB / T16172-2007, the thermal radiation power of the equipment was 35kW / m 2 , the temperature is 625℃, pulse spark ignition is used, the ignition time (TTI) and total heat release (THR) combustion parameters are tested, the thermal conductivity of the copper clad laminates in the embodiments and comparative examples is tested; and the limiting oxygen index of the high flame retardant copper clad laminate containing titanium dioxide is tested: according to ASTMD2863, the limiting oxygen index is tested; the results are shown in Table 1:
[0057] Table 1:
[0058] Ignition time TTI(s) Total heat release THR(MJ) Limiting oxygen index (%) Comparative Example 1 38.6 0.149 29.6 Comparative Example 2 35.7 0.164 28.4 Comparative Example 3 37.3 0.157 28.9 Example 1 55.2 0.132 35.5 Example 2 55.1 0.135 35.1 Example 3 55.9 0.126 36.8 Example 4 56.2 0.121 37.6
[0059] It can be seen from the above table that the highly flame-retardant copper-clad laminate containing titanium dioxide of the present invention does not use halogen in the raw materials, thus achieving the halogen-free flame-retardant and environmental protection requirements, and at the same time can effectively improve the flame-retardant performance and reduce the pollution to the environment.
[0060] The modified flame retardant in the present invention contains titanium dioxide, which can effectively enhance the flame retardant performance of the copper clad laminate; the 3-aminopropyltriethoxysilane in the modified flame retardant can perform surface modification treatment on nano titanium dioxide, which can effectively enhance the dispersion uniformity of nano titanium dioxide in the modified impregnating material, and further enhance the dispersion uniformity of nano titanium dioxide inside the copper clad laminate; the nano titanium dioxide can play a synergistic flame retardant role, improve the flame retardant effect of the flame retardant, slow down the combustion and spread of the copper clad laminate, and reduce the fire hazard; the addition of nano titanium dioxide can promote the combustion and carbonization of the internal material of the copper clad laminate, and the flame retardant synergy improves the strength of the internal material of the copper clad laminate, makes the internal material of the copper clad laminate dense, and enhances the stability of the internal material of the copper clad laminate. Such a burning carbon layer can effectively block the internal combustible gas and external oxygen, delay the transfer of heat, and promote the fire resistance of the material; adding an appropriate amount of nano-titanium dioxide to the modified impregnating material helps to form a continuous and dense flaky carbon layer during combustion, improving the defects and holes of the carbon layer; adding nano-titanium dioxide can effectively fill or insert the gaps in the semi-cured sheet, making the carbon layer produced after combustion dense and thick; and nano-titanium dioxide can catalyze the esterification reaction between the acid source and the carbon source during the combustion of the copper-clad laminate, reduce the volatilization of flame retardants during combustion, and thus increase the residual carbon; using polyphosphate and nano-titanium dioxide as raw materials to synthesize a nano-composite flexible PPE flame retardant, adding nano-titanium dioxide can effectively improve the carbon-forming energy of the coating Magnesium hydroxide can interact with the hydrophilic hydroxyl groups on the surface of nanocellulose, so that it can be better dispersed in the modified impregnation material. Although nanocellulose does not have a flame retardant function, its presence can improve the dispersibility of magnesium hydroxide, so that it can be evenly dispersed in the modified impregnation material. Magnesium hydroxide is the main component of the modified flame retardant. The magnesium oxide produced by the decomposition of magnesium hydroxide covers the surface of the polymer, which can prevent heat conduction and radiation, and isolate oxygen, thereby improving the flame retardant properties of the polymer. Magnesium oxide can also promote the carbonization of polymer materials and quickly form a carbonized layer during the combustion process, thereby preventing heat and oxygen from entering the polymer and preventing flammable gases produced by the thermal decomposition of the polymer. The nano-titanium dioxide enters the gas phase; in step 2, the nano-titanium dioxide is added to anhydrous ethanol for ultrasonic treatment, which can effectively disperse the nano-titanium dioxide in the anhydrous ethanol, and can effectively ensure the subsequent modification effect of the nano-titanium dioxide, and 3-aminopropyl triethoxysilane and nano-cellulose are added. 3-aminopropyl triethoxysilane and nano-cellulose can modify the surface of the nano-titanium dioxide, and ultrasonic treatment is performed at the same time, which can effectively enhance the surface modification effect of the nano-titanium dioxide; in step 3, the nano-cellulose, flexible phosphate, magnesium hydroxide and the surface-modified nano-titanium dioxide are blended, and the modified flame retardant can be effectively blended evenly to ensure the mixing effect of the subsequent materials;In step 4, the modified flame retardant is sheared with the dicyandiamide solution, the curing accelerator and the epoxy resin, and ultrasonic treatment is performed at the same time, which can effectively ensure that the raw materials in the modified impregnated material are evenly mixed and distributed; in step 5, the electronic glass fiber cloth is inserted into the modified impregnated material for impregnation treatment, and a prepreg is prepared after baking; in step 6, the copper foil is hot-pressed and compounded on both sides of the prepreg to obtain a highly flame-retardant copper-clad laminate containing titanium dioxide. ;
[0061] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A highly flame-retardant copper-clad laminate containing titanium dioxide, characterized in that: The invention comprises electronic glass fiber cloth, modified impregnating material and copper foil, wherein the modified impregnating material contains titanium dioxide, the electronic glass fiber cloth is impregnated and cured in the modified impregnating material, and then the copper foil is hot-pressed and formed; the weight ratio of the electronic glass fiber cloth to the modified impregnating material is 1:6-8.
2. A highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 1, characterized in that: The modified impregnating material comprises, by weight percentage, 23-27% of a modified flame retardant, 23-27% of a dicyandiamide solution, 2.7-3.3% of a curing accelerator, and the remainder being epoxy resin.
3. A highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 2, characterized in that: The modified flame retardant comprises, by weight percentage, 9.6-10.4% of nano cellulose, 34-38% of flexible phosphate, 3.6-4.4% of nano titanium dioxide, 0.3-0.5% of 3-aminopropyltriethoxysilane, and the rest is magnesium hydroxide.
4. A highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 3, characterized in that: The weight ratio of the electronic glass fiber cloth to the modified impregnated material is 1:7; The modified impregnating material comprises, by weight percentage, 24-26% of a modified flame retardant, 24-26% of a dicyandiamide solution, 2.9-3.1% of a curing accelerator, and the remainder is an epoxy resin; the modified flame retardant comprises, by weight percentage, 9.8-10.2% of nanocellulose, 35-37% of a flexible phosphate ester, 3.8-4.2% of nano titanium dioxide, 0.35-0.45% of 3-aminopropyltriethoxysilane, and the remainder is magnesium hydroxide.
5. The highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 3, characterized in that: The weight ratio of the electronic glass fiber cloth to the modified impregnated material is 1:7; The modified impregnating material comprises, by weight percentage, 25% of a modified flame retardant, 25% of a dicyandiamide solution, 3.0% of a curing accelerator, and the remainder being an epoxy resin; the modified flame retardant comprises, by weight percentage, 10.0% of nanocellulose, 36% of a flexible phosphate ester, 4.0% of nano titanium dioxide, 0.4% of 3-aminopropyltriethoxysilane, and the remainder being magnesium hydroxide.
6. The highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 3, characterized in that: The solid content of the dicyandiamide solution is 10.3-10.7%.
7. A method for preparing a highly flame-retardant copper-clad laminate containing titanium dioxide, characterized in that: The specific preparation steps are as follows: Step 1: weighing the dicyandiamide solution, curing accelerator, epoxy resin in the modified impregnating material raw material and the nanocellulose, flexible phosphate, nano titanium dioxide, 3-aminopropyltriethoxysilane, and magnesium hydroxide in the modified flame retardant raw material; Step 2: Add the nano titanium dioxide in step 1 to anhydrous ethanol, perform ultrasonic treatment for 10 to 20 minutes, add 3-aminopropyltriethoxysilane and one-fifth of the weight of nanocellulose, continue the ultrasonic treatment for 30 to 50 minutes, centrifuge, wash, and dry to obtain material a; Step 3: Evenly blend the remaining nanocellulose, flexible phosphate, magnesium hydroxide and material a in step 2 to obtain a modified flame retardant; Step 4: subjecting the modified flame retardant prepared in step 3 to the dicyandiamide solution, curing accelerator and epoxy resin prepared in step 1 to shear treatment for 30 to 40 minutes, and simultaneously subjecting the modified flame retardant prepared in step 3 to ultrasonic treatment to obtain a modified impregnated material; Step 5: insert the electronic glass fiber cloth into the modified impregnating material, impregnate for 30 to 40 minutes, and bake the impregnated electronic glass fiber cloth to obtain a prepreg; Step 6: Hot-press the copper foil to both sides of the prepreg to obtain a highly flame-retardant copper-clad laminate containing titanium dioxide.
8. The highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 7, characterized in that: In step 2, the weight ratio of nano titanium dioxide to ethanol solution is 1:30-50; anhydrous ethanol is used for washing and drying is performed at 80-90° C.; the ultrasonic frequency is 40-60 KHz and the ultrasonic power is 800-1000 W.
9. A highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 8, characterized in that: In step 3, a blending operation is performed using a mixer at a stirring speed of 1200 to 1600 r / min; in step 4, shearing is performed by pipeline high-speed shearing treatment at a high-speed shear rate of 4400 to 4600 r / min, an ultrasonic frequency of 1.4 to 1.6 MHz, and an ultrasonic power of 500 to 600 W; in step 6, hot pressing is performed at 240 to 260° C. at a pressure of 44.0 to 46.0 kg / m 2 .
10. A highly flame-retardant copper-clad laminate containing titanium dioxide according to claim 9, characterized in that: In step 2, the weight ratio of nano-titanium dioxide and ethanol solution is 1:40; anhydrous ethanol is used for washing and drying at 85°C; the ultrasonic frequency is 50KHz and the ultrasonic power is 900W; in step 3, a blending operation is performed using a stirrer with a stirring speed of 1400r / min; in step 4, shearing is performed through pipeline high-speed shearing, with a high-speed shear rate of 4500r / min, an ultrasonic frequency of 1.5MHz, and an ultrasonic power of 550W; in step 6, hot pressing is performed at 250°C with a pressure of 45.0kg / m 2 .
Citation Information
Patent Citations
Darkcoloured halogen-free expandable polyolefine fire retardant and preparation method thereof
CN101550242A
LED (light-emitting diode) heat dissipation paint with alloy powder and preparation method thereof
CN103881439A
Bactericidal flame-retardant smoke-proof moisture-proof non-toxic environmentally-friendly sound-insulating material and preparation method thereof
CN108285572A
Resin-based copper-clad plate filled with aluminum hydroxide micro powder and preparation method of resin-based copper-clad plate
CN115433435A
Hydrocarbon resin-based copper-clad plate and preparation method thereof
CN116080212A