Near-infrared light response Cu2O powder photo-thermal material and preparation method thereof
Cu2O powder photothermal materials prepared by the liquid phase reduction method show excellent photothermal properties under near-infrared light, solving the problem that traditional materials can only absorb ultraviolet-visible light, and achieving high efficiency in the fields of solar-driven water evaporation and photocatalysis. application.
Patent Information
- Application Number
- CN202410738595.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-07
AI Technical Summary
Traditional Cu2O photothermal materials can only absorb ultraviolet-visible light, resulting in limited photothermal performance and inability to effectively utilize near-infrared light to achieve efficient solar photothermal conversion.
Using the liquid phase reduction method, copper compounds, sodium hydroxide, p-benzoquinone and other materials are used to prepare Cu2O powder photothermal materials with near-infrared light responsiveness under low temperature conditions. Through steps such as ultrasonic dissolution, stirring, heating and drying, Forming materials with excellent photothermal properties.
It has been achieved that the photothermal performance of Cu2O powder photothermal materials can be significantly improved under near-infrared light without the need to load photosensitizers. The process is simple and suitable for industrial production. It also shows excellent performance in the fields of solar-driven water evaporation and photocatalysis.
Smart Images

Figure CN118744996A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photothermal material preparation, and specifically relates to a method for preparing a near-infrared light responsive Cu2O powder photothermal material, and also relates to the Cu2O powder photothermal material and its potential application in the field of solar-driven water evaporation. Background Art
[0002] The core component of solar water purification technology is the photothermal material with water vapor evaporation function. Common photothermal materials are mainly divided into: inorganic semiconductor materials, carbon materials and nanometal materials with plasmon effect. Although inorganic oxide semiconductor materials are low-cost and widely available, they usually have a wide bandgap and poor absorption capacity for sunlight, that is, they need to absorb incident light with higher energy, such as ultraviolet light and visible light, to excite electrons and release heat in the process of falling back to the ground state. However, according to the energy distribution of the solar spectrum (ultraviolet light wavelength 10 ~ 400nm, accounting for about 5%; visible light wavelength 400 ~ 700nm, accounting for about 43%; near-infrared light wavelength 700 ~ 2500nm, accounting for about 52%), near-infrared light response is the premise and basis for metal oxides to achieve efficient solar thermal conversion.
[0003] Cu2O is a low-cost narrow-bandgap p-type semiconductor photocatalytic material with a bandgap width of about 2.17eV. It has good photothermal stability, high conduction band potential, and can absorb sunlight to produce electrons with strong reducing ability, thereby converting O2 into strong oxidizing free radicals and non-free radicals, achieving efficient oxidation and degradation of organic pollutant molecules. In view of this, the use of this material can not only drive water evaporation by sunlight, but also play a role in disinfecting organic pollutants. Since traditional Cu2O can only absorb ultraviolet-visible light, it has limited photothermal performance. Although the red shift of the absorption spectrum of single-component Cu2O can be induced by modification methods such as doping with heteroenergetic elements and regulating the micromorphology, the absorption spectrum of the modified Cu2O is still limited to the visible light region. Therefore, it is urgent to develop a preparation process for near-infrared light-responsive Cu2O photothermal materials that are safe to operate and energy-saving and cost-reducing. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a near-infrared light responsive Cu2O powder photothermal material, wherein the material has excellent photothermal performance under near-infrared light irradiation.
[0005] Another object of the present invention is to provide a near-infrared light responsive Cu2O powder photothermal material.
[0006] The first technical solution adopted by the present invention is a method for preparing a near-infrared light responsive Cu2O powder photothermal material, which is specifically implemented according to the following steps:
[0007] Step 1, adding copper compound powder to deionized water, dissolving by ultrasonication to form a copper ion aqueous solution, and then adding ethanol to mix to obtain solution A;
[0008] Step 2, adding sodium hydroxide powder to deionized water, dissolving by ultrasonication to form a sodium hydroxide aqueous solution, and then adding ethanol to mix to obtain a solution B;
[0009] Step 3, stirring and heating the solution A obtained in step 1, then adding p-benzoquinone powder to react, then adding solution B, continuing the reaction, centrifuging, washing, and drying to obtain a near-infrared light-responsive Cu2O powder photothermal material.
[0010] The present invention is also characterized in that:
[0011] In step 1, the copper compound powder is specifically any one of copper nitrate powder, copper chloride powder, copper acetate powder, and copper sulfate powder.
[0012] In step 1, the concentration of the copper ion aqueous solution is 0.3-1 mol / L; the volume ratio of the copper ion aqueous solution to ethanol is 1:20-25.
[0013] In step 2, the concentration of the sodium hydroxide aqueous solution is 3-12 mol / L; the volume ratio of the sodium hydroxide aqueous solution to ethanol is 1:1-5.
[0014] In step 3, the stirring and heating temperature is 40-70° C., the stirring speed is 200-800 r / min, and the stirring and heating time is 5-20 min; the first reaction time is 1-5 min, and the second reaction time is 5-60 min; the drying temperature is 60-120° C., and the drying time is 12 h to 24 h.
[0015] In step 3, the mass ratio of the p-benzoquinone powder to the copper compound powder in solution A is 1-10:1-10.
[0016] Another technical solution adopted by the present invention is the potential application of near-infrared light responsive Cu2O powder photothermal material in the field of solar-driven water evaporation and photocatalysis.
[0017] The beneficial effects of the present invention are:
[0018] (1) The present invention uses a simple liquid phase reduction method to prepare a Cu2O powder photothermal material with excellent photothermal performance under near-infrared light irradiation at low temperature. The preparation method has the advantages of a wide source of raw materials, mild reaction conditions, simple operation, short process flow, and suitability for industrial production;
[0019] (2) The Cu2O powder photothermal material prepared by the present invention can exhibit excellent photothermal performance under near-infrared light without loading any photosensitizer or other active components;
[0020] (3) The Cu2O powder photothermal material prepared by the present invention can break the dilemma that traditional cuprous oxide only responds to visible light, and provide new ideas for the design and development of new oxide photothermal materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the XRD spectrum of the Cu2O powder photothermal material prepared in Example 1 of the present invention;
[0022] Figure 2 This is a macroscopic photograph of the Cu2O powder photothermal material prepared in Example 1 of the present invention;
[0023] Figure 3 is a UV-visible-near infrared diffuse reflectance spectrum of the Cu2O powder photothermal material prepared in Example 1 of the present invention;
[0024] Figure 4 It is a photothermal curve diagram of an aqueous solution containing the Cu2O powder photothermal material prepared in Example 1 of the present invention and commercial Cu2O powder under near-infrared light irradiation. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention uses a copper compound as a copper source, sodium hydroxide as a precipitant, deionized water and ethanol as solvents, and p-benzoquinone as a reducing agent, and adopts a liquid phase reduction method to prepare the near-infrared light responsive Cu2O powder photothermal material with excellent photothermal performance;
[0027] Follow the steps below to implement it:
[0028] Step 1, adding copper compound powder to deionized water, dissolving by ultrasonication to form a copper ion aqueous solution, and then adding ethanol to mix to obtain solution A;
[0029] The copper compound powder is specifically any one of copper nitrate powder, copper chloride powder, copper acetate powder, and copper sulfate powder;
[0030] The concentration of the copper ion aqueous solution is 0.3-1 mol / L; the volume ratio of the copper ion aqueous solution to ethanol is 1:20-25;
[0031] Step 2, adding sodium hydroxide powder to deionized water, dissolving by ultrasonication to form a sodium hydroxide aqueous solution, and then adding ethanol to mix to obtain a solution B;
[0032] The concentration of the sodium hydroxide aqueous solution is 3-12 mol / L; the volume ratio of the sodium hydroxide aqueous solution to ethanol is 1:1-5.
[0033] Step 3, stirring and heating the solution A obtained in step 1, then adding p-benzoquinone powder to react, then adding solution B, continuing the reaction, centrifuging, washing, and drying to obtain a near-infrared light-responsive Cu2O powder photothermal material;
[0034] The stirring and heating temperature is 40-70°C, the stirring speed is 200-800r / min, and the stirring and heating time is 5-20min;
[0035] The mass ratio of the benzoquinone powder to the copper compound powder in solution A is 1-10:1-10, the first reaction time is 1-5 minutes, and the second reaction time is 5-60 minutes;
[0036] The washing process uses anhydrous ethanol for 3 to 4 times;
[0037] The drying temperature is 60-120°C and the drying time is 12h-24h.
[0038] Compared with other strong reducing agents, p-benzoquinone has weaker reducing properties, and is not easy to cause cuprous oxide to be over-reduced to copper. Under certain conditions, it is more stable than reducing agents such as ascorbic acid, and can maintain reducing properties within a certain range. In addition, p-benzoquinone has a special conjugated structure. This conjugated system makes the electron distribution more special, and it is easy to accept or give electrons, which makes it have higher reactivity. Secondly, its molecular structure is relatively unstable, and it is easy to undergo redox reactions to achieve a more stable state. It has high reactivity and can quickly participate in redox reactions.
[0039] The Cu2O powder photothermal material prepared by the method of the present invention has more oxygen vacancies, resulting in a large amount of lattice distortion, which leads to a shortened bandgap width, thereby having better absorption capacity under near-infrared light; and the narrower bandgap width makes it easier for electrons to transition from the valence band to the conduction band, and the generation of excited electrons and holes is easier, which further increases the efficiency of energy transfer and conversion into heat, so that it has an excellent photothermal effect.
[0040] The specific method for determining the photothermal effect of the prepared Cu2O powder photothermal material under near-infrared light is as follows: 20 mg of the sample is ultrasonically dispersed in 50 mL of an aqueous solution, a photothermal experiment is performed under a 300 W xenon lamp light source equipped with a cutoff filter (λ>700 nm), the surface temperature of the aqueous solution is tested with an infrared thermal imager, and the temperature change trend is recorded.
[0041] Example 1
[0042] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention is specifically as follows:
[0043] Step 1: Mix 1 mL of a 0.6 mol / L copper nitrate aqueous solution and 25 mL of ethanol to obtain solution A.
[0044] Step 2: Mix 1 mL of 3 mol / L sodium hydroxide aqueous solution and 5 mL of ethanol to obtain solution B.
[0045] Step 3, solution A is stirred at a speed of 600 r / min for 10 min at an oil bath temperature of 60°C, then 0.3 g of p-benzoquinone powder is added to react for 5 min, and then solution B is added, and the reaction is continued for 20 min, followed by centrifugation while hot, and the product is washed 4 times with anhydrous ethanol, and then placed in an oven at 60°C for 24 h to obtain the Cu2O powder photothermal material.
[0046] XRD pattern of the prepared Cu2O powder photothermal material ( Figure 1 ) shows that the product prepared in Example 1 is pure phase Cu2O. Its macroscopic photo is as follows Figure 2 As shown, it is a black powder, indicating that it has a wider light absorption range, and the UV-visible-near infrared diffuse reflectance spectrum ( Figure 3 )It can be seen that the prepared sample can respond in the near-infrared light region.
[0047] The photothermal curve test results show that: under the above experimental conditions, after 75 minutes of near-infrared light irradiation, the temperature of the aqueous solution containing the Cu2O powder photothermal material prepared in Example 1 (62.1°C) is 1.46 times that of the aqueous solution containing the commercial Cu2O powder (42.3°C). Figure 4 ), and then both remain stable in this temperature range. The reason is that the Cu2O powder photothermal material prepared in Example 1 has more oxygen vacancies than the commercial Cu2O powder, which causes a large amount of lattice distortion, resulting in a shortened bandgap, making it easier for its electrons to absorb lower photon energy and be excited, thereby having better absorption capacity under near-infrared light; and the narrower bandgap makes it easier for electrons to transition from the valence band to the conduction band, and the generation of excited electrons and holes is easier, further increasing the efficiency of energy transfer and conversion into heat, thereby better driving the water evaporation process and realizing the utilization of clean energy.
[0048] Example 2
[0049] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention is specifically as follows:
[0050] Step 1, mixing 1 mL of 0.3 mol / L copper nitrate aqueous solution and 20 mL of ethanol to obtain solution A.
[0051] Step 2: Mix 1 mL of 6 mol / L sodium hydroxide aqueous solution and 4 mL of ethanol to obtain solution B.
[0052] Step 3, solution A was stirred at a speed of 200 r / min for 20 min at an oil bath temperature of 65°C, then 0.7 g of p-benzoquinone powder was added to react for 3 min, and then solution B was added. After continuing the reaction for 40 min, the solution was centrifuged while hot, and the product was washed 4 times with anhydrous ethanol, and then dried in an oven at 90°C for 12 h to obtain a Cu2O powder photothermal material with excellent photothermal properties.
[0053] Example 3
[0054] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention is specifically as follows:
[0055] Step 1, mixing 1 mL of 0.3 mol / L copper nitrate aqueous solution and 20 mL of ethanol to obtain solution A.
[0056] Step 2: Mix 1 mL of 3 mol / L sodium hydroxide aqueous solution and 1 mL of ethanol to obtain solution B.
[0057] Step 3, stirring solution A at a speed of 800 r / min for 5 min at an oil bath temperature of 50°C, then adding 0.5 g of p-benzoquinone powder to react for 2 min, then adding solution B, continuing the reaction for 5 min, centrifuging while hot, washing the product with anhydrous ethanol 3 times, and then drying it in an oven at 120°C for 12 h to obtain a Cu2O powder photothermal material with excellent photothermal properties.
[0058] Example 4
[0059] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention is specifically as follows:
[0060] Step 1, mixing 1 mL of a 0.9 mol / L copper nitrate aqueous solution and 24 mL of ethanol to obtain solution A.
[0061] Step 2: Mix 1 mL of 12 mol / L sodium hydroxide aqueous solution and 4 mL of ethanol to obtain solution B.
[0062] Step 3, stirring solution A at a speed of 500 r / min for 10 min at an oil bath temperature of 60°C, then adding 0.2 g of p-benzoquinone powder to react for 1 min, then adding solution B, continuing the reaction for 60 min, centrifuging while hot, washing the product with anhydrous ethanol 3 times, and then drying it in an oven at 60°C for 24 h, to obtain a Cu2O powder photothermal material with excellent photothermal properties.
[0063] Example 5
[0064] The preparation method of the near-infrared light responsive Cu2O powder photothermal material of the present invention is specifically as follows:
[0065] Step 1: Mix 1 mL of 1 mol / L copper nitrate aqueous solution and 25 mL of ethanol to obtain solution A.
[0066] Step 2: Mix 1 mL of 9 mol / L sodium hydroxide aqueous solution and 3 mL of ethanol to obtain solution B.
[0067] Step 3, solution A was stirred at a speed of 200 r / min for 20 min at an oil bath temperature of 40°C, then 1 g of p-benzoquinone powder was added to react for 5 min, and then solution B was added to react for 30 min, followed by centrifugation while hot, and the product was washed 4 times with anhydrous ethanol, and then dried in an oven at 60°C for 24 h to obtain a Cu2O powder photothermal material with excellent photothermal properties.
[0068] The present invention can prepare Cu2O powder photothermal material with excellent photothermal performance under near-infrared light irradiation through a simple liquid phase reduction method, which will provide new ideas for other researchers to design and prepare new high-efficiency oxide near-infrared light-responsive photothermal materials.
Claims
1. A method for preparing near-infrared light-responsive Cu2O powder photothermal material, characterized in that: Follow the steps below to implement it: Step 1, adding copper compound powder to deionized water, dissolving by ultrasonication to form a copper ion aqueous solution, and then adding ethanol to mix to obtain solution A; Step 2, adding sodium hydroxide powder to deionized water, dissolving by ultrasonication to form a sodium hydroxide aqueous solution, and then adding ethanol to mix to obtain a solution B; Step 3, stirring and heating the solution A obtained in step 1, then adding p-benzoquinone powder to react, then adding solution B, continuing the reaction, centrifuging, washing, and drying to obtain a near-infrared light-responsive Cu2O powder photothermal material.
2. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In the step 1, the copper compound powder is specifically any one of copper nitrate powder, copper chloride powder, copper acetate powder, and copper sulfate powder.
3. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In the step 1, the concentration of the copper ion aqueous solution is 0.3-1 mol / L; the volume ratio of the copper ion aqueous solution to ethanol is 1:20-25.
4. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In step 2, the concentration of the sodium hydroxide aqueous solution is 3-12 mol / L; the volume ratio of the sodium hydroxide aqueous solution to ethanol is 1:1-5.
5. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In step 3, the stirring and heating temperature is 40-70° C., the stirring speed is 200-800 r / min, and the stirring and heating time is 5-20 min; the first reaction time is 1-5 min, and the second reaction time is 5-60 min; the drying temperature is 60-120° C., and the drying time is 12 h to 24 h.
6. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In the step 3, the mass ratio of the p-benzoquinone powder to the copper compound powder in the solution A is 1-10:1-10.
7. The method for preparing the near-infrared light responsive Cu2O powder photothermal material according to claim 1, characterized in that: In step 3, the washing process uses anhydrous ethanol for 3 to 4 times.
8. Near-infrared light responsive Cu2O powder photothermal material, characterized in that: The method is prepared by any one of claims 1 to 7.
Citation Information
Patent Citations
Sheet-like structure CuO nano-photothermal conversion material and preparation method thereof
CN110342564A
Method for preparing nano copper oxide by microwave hydrothermal method and application of nano copper oxide
CN111892078A
Cu2O and precious metal composite particle with Yolk-Shell structure as well as preparation method and application of Cu2O and precious metal composite particle
CN117019171A
Method of manufacturing cuprous oxide particles, and cuprous oxide particles
JP2006069879A
Method of manufacturing cuprous oxide particles, and cuprous oxide particles
JP2006069880A