Carbon nanotube coated and doped precursor, preparation method thereof and positive electrode material

By using carbon nanotubes to coat the doping precursor in the lithium-ion battery cathode material, combined with co-precipitation and spray pyrolysis technology, the problems of unstable cathode material structure and uneven mixing of doping elements are solved, and the battery rate is improved. and cycle performance, and reduced manufacturing costs.

CN118745008APending Publication Date: 2024-10-08JINGMEN GEM NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202410811102.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing lithium-ion battery cathode materials suffer from structural instability, capacity fading, and safety issues in large-scale applications. The doping and coating processes are expensive, the preparation process is complex, and the doping elements are unevenly mixed, which affects electrochemical performance.

Method used

Carbon nanotubes are used to coat the doping precursor, and the nickel-cobalt-manganese ternary precursor is prepared through co-precipitation method. The carbon nanotube coating layer is formed by combining spray pyrolysis technology to improve the distribution uniformity and electrochemical performance of the doped metal. Reduce manufacturing costs.

Benefits of technology

It significantly improves the rate performance and cycle performance of lithium-ion batteries, shortens the process flow, reduces manufacturing costs, and enhances the application prospects of cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745008A_ABST
    Figure CN118745008A_ABST
Patent Text Reader

Abstract

The invention provides a carbon nanotube coated and doped precursor, a preparation method thereof and a positive electrode material. The carbon nanotube coated and doped precursor comprises a core and a carbon nanotube coating layer coated outside the core, the core comprises a nickel-cobalt-manganese ternary precursor core containing doped metal M; the doped metal M comprises any one or a combination of at least two of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum. According to the invention, the doped metal M is coated and combined with the carbon nanotubes to prepare a high-performance precursor, so that the discharge capacity, rate capability and cycle performance of the positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ternary precursors, and in particular to a carbon nanotube-coated doped precursor and a preparation method thereof and a positive electrode material. Background Art

[0002] Lithium-ion batteries have attracted widespread attention as an excellent portable energy storage device and automotive power battery. Lithium-ion batteries have the advantages of long life, high specific capacity, and stable cycle, and are widely used in portable devices, electric vehicles, hybrid vehicles and other fields. As the first commercial cathode material for lithium-ion batteries, LiCoO2 has occupied most of the lithium-ion battery market share in the past few years. However, the high price and toxicity of LiCoO2 limit its development prospects and are contrary to the requirements of green chemistry.

[0003] Moreover, nickel-rich layered materials LiNi x Co y Mn 1-x-y O2 (i.e. NCM) has received widespread attention and is being studied as a replacement for commercial LiCoO2 materials.

[0004] However, the development of nickel-rich layered materials in large-scale applications has been slow, mainly due to their structural instability, capacity fading, and safety issues related to oxygen release. + and Ni 2+ Similar ionic radii ( and ) leads to Li + / Ni 2+ Mixing is the main reason for the above problems in nickel-rich cathodes. The structure of nickel-rich layered materials is essentially closely related to the rock salt structure, that is, the α-NaFeO2 structure with an R-3m space group; the similar single cell size of these two structures leads to Li + / Ni 2+ Therefore, the Ni content in the final nickel-rich cathode is increased. 3+ The content ratio can alleviate the Li + and Ni 3+ Size mismatch caused by Li + / Ni 2+ Mixing effect ( and ). However, according to literature reports, Ni 3+ The ions are unstable under high-temperature solid-state reactions. Because of this, the stoichiometry of synthesizing nickel-rich layered materials in the atmosphere is very difficult.

[0005] Existing technology improvements usually use doping, coating and other means to improve the electrochemical performance of positive electrode materials. Doping is done by adding elements so that the doping elements occupy the original Ni 2+ The site where Li + / Ni 2+ The ion spacing between the two increases, and some doping elements increase the interlayer spacing of the crystal structure, inhibiting the Li + / Ni 2+ Mixed arrangement is beneficial to Li + transmission, thereby improving the specific capacity of the material. The coating suppresses the dissolution of transition metal ions in the electrolyte inside the positive electrode material by directly adding a coating layer on the surface of the material, avoids the occurrence of side reactions, and improves the cycle performance of the material. For example, in CN117613222A, the first stage reaction generates a high-nickel polycrystalline core, and the second stage changes the reaction conditions to generate a high-nickel polycrystalline porous layer on the surface, which is then mixed and sintered with a lithium source, a first dopant, and a first coating agent, and then the mixture is sintered with a second coating agent to obtain a high-nickel polycrystalline material, the high-nickel single crystal core is pre-burned with a lithium source and a second dopant, and then the mixture is sintered with a third coating agent to obtain a high-nickel single crystal material. Mixing the two takes into account both the cycle performance and energy density of the material. In CN117276534A, a metal salt solution, a precipitant, a complexing agent and a zirconium salt solution are added in the first reaction stage. When the particles grow to the first particle size, the zirconium salt solution is replaced with a ruthenium salt solution, and the second reaction stage is carried out. When the particles in the second reaction system grow to the second particle size, the metal salt solution and the ruthenium salt solution are stopped, and the zirconium salt solution is re-introduced to carry out the third reaction stage. This doping and coating method makes the elements between the particles evenly mixed, and expands the inter-atom interlayer distance, the layered structure of the material is stable, and the cycle performance is improved. In CN117543020A, the precursor, the doping element and the lithium source are mixed and sintered, and the obtained matrix is ​​crushed and mixed with additives A and B respectively, and then sintered twice. The first coating layer obtained is distributed in a point-like manner close to the precursor, and the second coating layer is distributed in a plane-like manner close to the outer layer, covering the exposed surface of the substrate. The two work together to form a three-dimensional coating layer, thereby improving the specific capacity and cycle performance of the material.

[0006] However, the improvement of electrochemical performance is limited by the modification of a single doping or single coating process. Most of the existing doping elements are mixed with the lithium source and the matrix during the sintering process. Considering the influence of the primary morphology on the surface of the precursor, if the primary morphology is too rough, it will block the doping elements from entering the channel inside the matrix, resulting in uneven doping and mixing. In addition, if there are too many doping and coating elements, the manufacturing cost will be greatly increased, and if it is applied to mass production, there are also many limiting factors. These are all problems that need to be solved urgently. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a carbon nanotube-coated doped precursor and its preparation method and positive electrode material, so as to solve the problems of uneven mixing of doping elements and high preparation cost in the existing positive electrode material preparation method, greatly speed up the process flow while reducing manufacturing costs, and improve the discharge capacity, rate performance and cycle performance of the positive electrode material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a carbon nanotube coated doped precursor, comprising a core and a carbon nanotube coating layer coated on the outside of the core; the core comprises a nickel-cobalt-manganese ternary precursor core containing a doping metal M; the doping metal M comprises any one or a combination of at least two of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum, wherein typical but non-limiting combinations are a combination of aluminum and titanium, a combination of niobium and titanium, a combination of aluminum and niobium, a combination of zirconium and titanium, a combination of yttrium and zirconium, a combination of vanadium and titanium, a combination of aluminum and strontium, a combination of aluminum and cerium, a combination of aluminum and cerium, and a combination of lanthanum and cerium.

[0010] The core of the carbon nanotube-coated doped precursor provided by the present invention has a doped metal M, wherein the doping of the doped metal M increases the atomic layer spacing, shortens the distance of lithium ion transmission, improves the rate performance and cycle performance of the material, and stabilizes the crystal structure, thereby improving the safety during the electrochemical reaction process; and a carbon nanotube coating layer is coated on the outer side of the precursor, on the one hand, the carbon nanotube can further improve the conductivity of the precursor oxide, and at the same time further shorten the transmission path of lithium ions, reduce the polarization resistance during the reaction, and improve the rate performance and cycle performance of the material; on the other hand, the carbon in the carbon nanotube has a reducing property, and can reduce the doped metal M in the oxide state to the atomic state and attach it to the surface of the carbon nanotube, thereby improving the migration rate of lithium ions, that is, the carbon nanotube coating layer cooperates with the doped metal M in the core at the same time, and jointly improves the rate performance and cycle performance of the carbon nanotube-coated doped precursor, thereby improving the application prospects of the positive electrode material.

[0011] Preferably, the core comprises nickel oxide, cobalt oxide and manganese oxide.

[0012] Preferably, the doped metal M in the core comprises doped metal M atoms attached to the carbon nanotube coating layer.

[0013] Preferably, the molar ratio of nickel, cobalt and manganese in the core is (60-90):(10-20):(0-20), wherein the proportion of nickel can be, for example, 60, 64, 67, 70, 74, 77, 80, 84, 87 or 90, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; the proportion of cobalt can be, for example, 10, 12, 13, 14, 15, 16, 17, 18, 19 or 20, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; the proportion of manganese can be, for example, 0, 3, 5, 7, 9, 12, 14, 16, 18 or 20, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; preferably 80:10:10.

[0014] Preferably, the doped metal M in the core accounts for 0.05-5% of the total molar percentage of nickel, cobalt and manganese, for example, it can be 0.05%, 0.6%, 1.15%, 1.7%, 2.25%, 2.8%, 3.35%, 3.9%, 4.45% or 5%, etc., but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0015] The present invention further preferably controls the molar percentage of the doped metal M within the above range, so as to better improve the grain morphology, expand the interlayer spacing and thus improve the rate performance of the material, while further interacting with the carbon nanotubes in the coating layer to improve the electrochemical performance of the material.

[0016] Preferably, the content of carbon nanotubes in the carbon nanotube-coated doping precursor is 0.1-10wt%, for example, it can be 0.1wt%, 1.2wt%, 2.3wt%, 3.4wt%, 4.5wt%, 5.6wt%, 6.7wt%, 7.8wt%, 8.9wt% or 10wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0017] Preferably, the density of the carbon nanotube coating is 100 to 1000 m 2 / g, for example, it can be 100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g, 600m 2 / g、700m 2 / g、800m 2 / g、900m 2 / g or 1000m 2 / g, etc., but are not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0018] Preferably, the doping metal M is cerium.

[0019] Preferably, the size of the core is 4-5 μm, for example, it can be 4 μm, 4.2 μm, 4.3 μm, 4.4 μm, 4.5 μm, 4.6 μm, 4.7 μm, 4.8 μm, 4.9 μm or 5 μm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0020] Preferably, the particle distribution span of the core is 1.0 to 1.5, for example, it can be 1.0, 1.06, 1.12, 1.17, 1.23, 1.28, 1.34, 1.39, 1.45 or 1.5, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0021] Preferably, the distribution uniformity of the doped metal M in the core is to form a uniformly dispersed distribution ring.

[0022] The main advantage of the carbon nanotube-coated doped precursor of the present invention is that the distribution uniformity of the doped metal M is high, and the distribution uniformity of the doped metal M can be within the above range, thereby having better electrochemical performance.

[0023] Preferably, the thickness of the carbon nanotube coating layer is 1 to 10 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0024] Preferably, the particle size range of the carbon nanotube-coated doped precursor is 4 to 5 μm, for example, it can be 4 μm, 4.2 μm, 4.3 μm, 4.4 μm, 4.5 μm, 4.6 μm, 4.7 μm, 4.8 μm, 4.9 μm or 5 μm, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0025] In a second aspect, the present invention provides a method for preparing a carbon nanotube-coated doped precursor according to the first aspect, the preparation method comprising the following steps:

[0026] An ammonia-containing base liquid is prepared, and then a doped metal salt solution, a ternary salt solution, a precipitant and a complexing agent are introduced into the base liquid to perform a first reaction to form a preliminary core; the preliminary core is sequentially aged and dried to obtain a core powder; the core powder is sequentially slurried, ground and spray-pyrolyzed to obtain an oxide core; the oxide core is mixed with a suspension containing carbon nanotubes and dried to obtain the carbon nanotube-coated doped precursor.

[0027] The carbon nanotube-coated doped precursor described in the first aspect of the present invention is preferably prepared by the preparation method of the second aspect. By the co-precipitation method, the precursor in the kettle is ensured to grow and form at one time. The preparation method is simple, the particle size is highly controllable, and the application prospect is broad.

[0028] Moreover, in the present invention, the preliminary core must first be slurried, ground and spray pyrolyzed to form an oxide core before it can be mixed with a suspension containing carbon nanotubes to prepare a coating layer; the sand grinding treatment makes the co-precipitation doping reaction more uniform, and at the same time, the spray pyrolysis method is combined to effectively reduce the particle size, and a more evenly dispersed particle ball is formed by granulation, which avoids agglomeration, and is also beneficial to the synthesis of single crystals in the subsequent sintering process, which can make the distribution of doping elements more uniform and improve the performance of the positive electrode material.

[0029] Preferably, the first reaction is carried out in a reaction atmosphere.

[0030] Preferably, the reaction atmosphere comprises nitrogen.

[0031] Preferably, the nitrogen introduction rate is 0.2 to 2 m 3 / h, for example, it can be 0.2m 3 / h、0.4m 3 / h、0.6m 3 / h、0.8m 3 / h、1m 3 / h、1.2m 3 / h、1.4m 3 / h、1.6m 3 / h、1.8m 3 / h or 2m 3 / h, etc., but are not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0032] Preferably, the precipitant comprises an alkaline solution, and preferably the precipitant is a sodium hydroxide solution.

[0033] Preferably, the concentration of the alkaline solution is 30-35wt%, for example, it can be 30wt%, 30.6wt%, 31.2wt%, 31.7wt%, 32.3wt%, 32.8wt%, 33.4wt%, 33.9wt%, 34.5wt% or 35wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0034] Preferably, the complexing agent comprises aqueous ammonia.

[0035] Preferably, the concentration of the ammonia water is 10 to 20wt%, for example, it can be 10wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0036] Preferably, the ammonia concentration of the base liquid is 4 to 10 g / L, for example, it can be 4 g / L, 4.7 g / L, 5.4 g / L, 6 g / L, 6.7 g / L, 7.4 g / L, 8 g / L, 8.7 g / L, 9.4 g / L or 10 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0037] Preferably, the pH of the base solution is 10-12, for example, 10, 10.3, 10.5, 10.7, 10.9, 11.2, 11.4, 11.6, 11.8 or 12, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0038] Preferably, the temperature of the base liquid is 40-60°C, for example, it can be 40°C, 43°C, 45°C, 47°C, 49°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0039] Preferably, the ternary salt solution comprises nickel salt, cobalt salt, manganese salt and doped metal salt.

[0040] Preferably, the nickel salt comprises any one of nickel sulfate, nickel nitrate, nickel acetate or nickel chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of nickel sulfate and nickel nitrate, a combination of nickel acetate and nickel nitrate, a combination of nickel sulfate and nickel acetate, a combination of nickel chloride and nickel acetate, preferably nickel acetate.

[0041] Preferably, the cobalt salt comprises any one of cobalt sulfate, cobalt nitrate, cobalt acetate or cobalt chloride, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of cobalt sulfate and cobalt nitrate, a combination of cobalt acetate and cobalt nitrate, a combination of cobalt sulfate and cobalt acetate, a combination of cobalt chloride and cobalt acetate, preferably cobalt acetate.

[0042] Preferably, the manganese salt comprises any one of manganese sulfate, manganese nitrate, manganese acetate or manganese chloride, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of manganese sulfate and manganese nitrate, a combination of manganese acetate and manganese nitrate, a combination of manganese sulfate and manganese acetate, a combination of manganese chloride and manganese acetate, preferably manganese acetate.

[0043] Preferably, the total element concentration of Ni, Co and Mn in the ternary salt solution is 20 to 120 g / L, for example, it can be 20 g / L, 32 g / L, 43 g / L, 54 g / L, 65 g / L, 76 g / L, 87 g / L, 98 g / L, 109 g / L or 120 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0044] Preferably, the molar ratio of the three elements Ni, Co and Mn in the ternary salt solution is (60-90):(10-20):(0-20), wherein the proportion of nickel can be, for example, 60, 64, 67, 70, 74, 77, 80, 84, 87 or 90, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; the proportion of cobalt can be, for example, 10, 12, 13, 14, 15, 16, 17, 18, 19 or 20, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; the proportion of manganese can be, for example, 0, 3, 5, 7, 9, 12, 14, 16, 18 or 20, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; preferably 80:10:10, preferably 80:10:10.

[0045] The doping metal M in the doping metal salt solution includes any one or a combination of at least two of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum, wherein a typical but non-limiting combination is a combination of aluminum and titanium, a combination of niobium and titanium, a combination of aluminum and niobium, a combination of zirconium and titanium, a combination of yttrium and zirconium, a combination of vanadium and titanium, a combination of aluminum and strontium, a combination of aluminum and cerium, a combination of aluminum and cerium, a combination of lanthanum and cerium, and preferably the doping metal M is cerium;

[0046] Preferably, the doping metal salt comprises any one of sulfate, nitrate, acetate or chloride salts or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of sulfate and nitrate, a combination of sulfate and acetate, a combination of acetate and nitrate, a combination of chloride and nitrate, and a combination of sulfate and chloride.

[0047] Preferably, when the doping metal M is cerium, the cerium source is any one of cerium sulfate, cerium nitrate, cerium acetate or cerium trichloride, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of cerium sulfate and cerium nitrate, a combination of cerium acetate and cerium nitrate, a combination of cerium sulfate and cerium acetate, a combination of cerium trichloride and cerium nitrate, and a combination of cerium sulfate and cerium trichloride.

[0048] Preferably, the doping metal M accounts for 0.05-5% of the total molar percentage of the ternary elements Ni, Co and Mn, for example, it can be 0.05%, 0.6%, 1.15%, 1.7%, 2.25%, 2.8%, 3.35%, 3.9%, 4.45% or 5%, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0049] Preferably, the concentration of the doped metal salt solution is 10 to 50 g / L, for example, it can be 10 g / L, 15 g / L, 19 g / L, 24 g / L, 28 g / L, 33 g / L, 37 g / L, 42 g / L, 46 g / L or 50 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0050] Preferably, the general formula of the preliminary core is Ni a Co b Mn c Ce d (OH)2, wherein 0.8<a<0.9, 0.1<b<0.2, 0<c<0.1, 0<d<0.1, a+b+c+d=1.

[0051] Wherein a can be, for example, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88 or 0.89, etc., but is not limited to the listed values, and other values ​​not listed in the range are also applicable; b can be, for example, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18 or 0.19, etc., but is not limited to the listed values, and other values ​​not listed in the range are also applicable ; c can be, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08 or 0.09, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable; d can be, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08 or 0.09, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0052] Preferably, the first reaction includes a first stage reaction, a second stage reaction, a third stage reaction and a fourth stage reaction which are performed sequentially.

[0053] Preferably, in the first stage reaction, the flow rate of the complexing agent is controlled to be 600-800 ml / L, for example, 600 ml / L, 623 ml / L, 645 ml / L, 667 ml / L, 689 ml / L, 712 ml / L, 734 ml / L, 756 ml / L, 778 ml / L or 800 ml / L; the flow rate of the precipitating agent is 1.2-1.6 L / h, for example, 1.2 L / h, 1.25 L / h, 1.29 L / h, 1.34 L / h, 1.38 L / h, 1.43 L / h, 1.47 L / h, 1.52 L / h, 1.64 L / h, 1.70 L / h, 1.81 L / h, 1.87 L / h, 1.90 L / h, 1.91 L / h, 1.93 L / h, 1.97 L / h, 1.98 L / h, 1.99 L / h, 1.10 L / h, 1.11 L / h, 1.12 L / h, 1.13 L / h, 1.14 L / h, 1.15 L / h, 1.16 L / h, 1.17 L / h, 1.18 L / h, 1.19 L / h, 1.20 L / h, 1.21 L / h, 1.23 L / h, 1.24 L / h, 1.25 L / h .56L / h or 1.6L / h, etc.; the flow rate of the ternary salt solution is 3-6L / h, for example, it can be 3L / h, 3.4L / h, 3.7L / h, 4L / h, 4.4L / h, 4.7L / h, 5L / h, 5.4L / h, 5.7L / h or 6L / h, etc.; the flow rate of the doped metal salt solution is 100-500ml / h, for example, it can be 100ml / h, 145ml / h, 189ml / h, 234ml / h, 278ml / h, 323ml / h, 367ml / h, 412ml / h, 456ml / h or 500ml / h, etc.

[0054] In the present invention, the introduction rate of each solution in the first stage reaction is preferably controlled within the above range, which can better ensure that the precipitation reaction is completely carried out, and can further control the growth particle size of the precursor within a reasonable range to ensure uniform distribution of the doped metal.

[0055] Preferably, in the second stage reaction, the flow rate of the complexing agent is controlled to be 600-800 ml / L, for example, 600 ml / L, 623 ml / L, 645 ml / L, 667 ml / L, 689 ml / L, 712 ml / L, 734 ml / L, 756 ml / L, 778 ml / L or 800 ml / L; the flow rate of the precipitating agent is 1.6-2.0 L / h, for example, 1.6 L / h, 1.65 L / h, 1.69 L / h, 1.74 L / h, 1.78 L / h, 1.83 L / h, 1.87 L / h, 1.92 L / h, 1.9 6L / h or 2.0L / h, etc.; the flow rate of the ternary salt solution is 4-8L / h, for example, it can be 4L / h, 4.5L / h, 4.9L / h, 5.4L / h, 5.8L / h, 6.3L / h, 6.7L / h, 7.2L / h, 7.6L / h or 8L / h, etc., the flow rate of the doped metal salt solution is 100-500ml / h, for example, it can be 100ml / h, 145ml / h, 189ml / h, 234ml / h, 278ml / h, 323ml / h, 367ml / h, 412ml / h, 456ml / h or 500ml / h, etc.

[0056] Preferably, the pH of the second stage reaction is greater than that of the first stage reaction.

[0057] In the present invention, the pH of the second stage reaction is preferably greater than that of the first stage reaction, which has the effect of promoting the nucleation of small particles. When the pH of the second stage reaction is too high, there is a problem of uneven distribution of small particle sizes.

[0058] Preferably, the ammonia concentration in the first stage reaction is 7 to 9 g / L, for example, 7 g / L, 7.3 g / L, 7.5 g / L, 7.7 g / L, 7.9 g / L, 8.2 g / L, 8.4 g / L, 8.6 g / L, 8.8 g / L or 9 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0059] Preferably, the pH in the first stage reaction is controlled to be 11-11.3, for example, 11, 11.1, 11.2 or 11.3, but is not limited to the listed values, and other values ​​not listed in the range are also applicable.

[0060] Preferably, the ammonia concentration in the second stage reaction is 7 to 9 g / L, for example, 7 g / L, 7.3 g / L, 7.5 g / L, 7.7 g / L, 7.9 g / L, 8.2 g / L, 8.4 g / L, 8.6 g / L, 8.8 g / L or 9 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0061] Preferably, the pH in the second stage reaction is controlled to be 11.3-11.6, for example, 11.3, 11.4, 11.5 or 11.6, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0062] The present invention preferably controls the pH within the above range during the precipitation process, which is more conducive to forming a core-shell precursor with a target particle size. The present invention preferably controls the ammonia concentration within the above range, which is more conducive to obtaining a core-shell precursor with a moderate density, thereby avoiding the problem that lithium ions are difficult to diffuse during the sintering process and ultimately lead to a decrease in the charge and discharge performance of the positive electrode material. In addition, primary crystal grains with a smaller particle size can be obtained, further improving the stability of the positive electrode material.

[0063] Preferably, the particle size of the particles after the first stage reaction is 3-4 μm, for example, 3 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm, 3.8 μm, 3.9 μm or 4 μm.

[0064] Preferably, the particle span after the second stage reaction is 1.5 to 2, for example, 1.5, 1.56, 1.62, 1.67, 1.73, 1.78, 1.84, 1.89, 1.95 or 2, etc.

[0065] Preferably, the third stage reaction includes: aging the material after the second stage reaction to obtain an aged material; extracting the first particles in the aged material, and growing the first particles alone to a first particle size range in a seed-like manner to obtain grown particles; putting the grown particles into the aged material to continue the subsequent fourth stage reaction; the particle size range of the first particles is <1.0μm.

[0066] The present invention extracts small particles (i.e., first particles) from the material after the second stage reaction and performs stable growth of separate crystal seeds. The particles are small and fewer crystal surface cracks are generated during the electrochemical cycle, which is more conducive to improving the cycle performance, shortening the reaction time, and simplifying the process.

[0067] Preferably, the process of stable seed growth includes: mixing water and the first particles, and then introducing a doped metal salt solution, a ternary salt solution, a precipitant and a complexing agent to perform stable seed growth.

[0068] Preferably, the ratio of the water to the first particles is 3-5 L / kg, for example, 3 L / kg, 3.3 L / kg, 3.5 L / kg, 3.7 L / kg, 3.9 L / kg, 4.2 L / kg, 4.4 L / kg, 4.6 L / kg, 4.8 L / kg or 5 L / kg, etc.

[0069] Preferably, the flow rate of the complexing agent during the stable growth of the seed crystal is controlled to be 300-500 ml / L, for example, 300 ml / L, 323 ml / L, 345 ml / L, 367 ml / L, 389 ml / L, 412 ml / L, 434 ml / L, 456 ml / L, 478 ml / L or 500 ml / L; the flow rate of the precipitating agent is 0.8-1.2 L / h, for example, 0.8 L / h, 0.85 L / h, 0.89 L / h, 0.94 L / h, 0.98 L / h, 1.03 L / h, 1.07 L / h, 1.12 L / h, 1.19 L / h, 1.20 L / h, 1.31 L / h, 1.44 L / h, 1.58 L / h, 1.60 L / h, 1.70 L / h, 1.81 L / h, 1.91 L / h, 1.97 L / h, 1.18 L / h, 1.29 L / h, 1.30 L / h, 1.41 L / h, 1.52 L / h, 1.64 L / h, 1.70 L / h, 1.81 L / h, 1.98 L / h, 1. 16L / h or 1.2L / h, etc.; the flow rate of the ternary salt solution is 2-5L / h, for example, it can be 2L / h, 2.4L / h, 2.7L / h, 3L / h, 3.4L / h, 3.7L / h, 4L / h, 4.4L / h, 4.7L / h or 5L / h, etc.; and the flow rate of the doped metal salt solution is 100-500ml / h, for example, it can be 100ml / h, 145ml / h, 189ml / h, 234ml / h, 278ml / h, 323ml / h, 367ml / h, 412ml / h, 456ml / h or 500ml / h, etc.

[0070] Preferably, the temperature for stable growth of the seed crystal is 50-60°C, for example, it can be 50°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0071] Preferably, the stirring speed for stable growth of the seed crystal is 300-400 rpm, for example, it can be 300 rpm, 312 rpm, 323 rpm, 334 rpm, 345 rpm, 356 rpm, 367 rpm, 378 rpm, 389 rpm or 400 rpm, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0072] Preferably, the first particle size ranges from 1.0 to 1.5 μm, for example, it may be 1.0 μm, 1.06 μm, 1.12 μm, 1.17 μm, 1.23 μm, 1.28 μm, 1.34 μm, 1.39 μm, 1.45 μm or 1.5 μm.

[0073] Preferably, in the fourth stage reaction, the flow rate of the complexing agent is controlled to be 800-1000 ml / L, for example, 800 ml / L, 823 ml / L, 845 ml / L, 867 ml / L, 889 ml / L, 912 ml / L, 934 ml / L, 956 ml / L, 978 ml / L or 1000 ml / L; the flow rate of the precipitating agent is 2.5-3.0 L / h, for example, 2.5 L / h, 2.56 L / h, 2.62 L / h, 2.67 L / h, 2.73 L / h, 2.78 L / h, 2.84 L / h, 2.89 L / h, 2.9 5L / h or 3.0L / h, etc.; the flow rate of the ternary salt solution is 8-10L / h, for example, it can be 8L / h, 8.3L / h, 8.5L / h, 8.7L / h, 8.9L / h, 9.2L / h, 9.4L / h, 9.6L / h, 9.8L / h or 10L / h, etc.; the flow rate of the doped metal salt solution is 100-500ml / h, for example, it can be 100ml / h, 145ml / h, 189ml / h, 234ml / h, 278ml / h, 323ml / h, 367ml / h, 412ml / h, 456ml / h or 500ml / h, etc.

[0074] Preferably, the ammonia concentration in the fourth stage reaction is 5 to 7 g / L, for example, it can be 5 g / L, 5.3 g / L, 5.5 g / L, 5.7 g / L, 5.9 g / L, 6.2 g / L, 6.4 g / L, 6.6 g / L, 6.8 g / L or 7 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0075] Preferably, the pH in the fourth stage reaction is controlled to be 10.2-10.5, for example, 10.2, 10.3, 10.4 or 10.5, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0076] Preferably, washing is further included between the aging and drying.

[0077] Preferably, the washing method is: washing with hot water at least three times.

[0078] Preferably, the drying temperature is 100-150°C, for example, it can be 100°C, 106°C, 112°C, 117°C, 123°C, 128°C, 134°C, 139°C, 145°C or 150°C.

[0079] Preferably, after the slurrying, a slurry is obtained, and the solid content of the slurry is 20-40wt%, for example, it can be 20wt%, 23wt%, 25wt%, 27wt%, 29wt%, 32wt%, 34wt%, 36wt%, 38wt% or 40wt%, etc.

[0080] Preferably, the grinding comprises sanding.

[0081] Preferably, the grinding balls for sand grinding include zirconium balls of 0.1-1 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm or 1 mm.

[0082] Preferably, the sanding time is 2 to 10 hours, for example, it can be 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.

[0083] Preferably, the inlet temperature of the spray pyrolysis is 200-300°C, for example, it can be 200°C, 212°C, 223°C, 234°C, 245°C, 256°C, 267°C, 278°C, 289°C or 300°C.

[0084] Preferably, the outlet temperature of the spray pyrolysis is 80-150°C, for example, it can be 80°C, 88°C, 96°C, 104°C, 112°C, 119°C, 127°C, 135°C, 143°C or 150°C.

[0085] Preferably, the carbon nanotubes are single-walled carbon nanotubes and / or multi-walled carbon nanotubes, preferably multi-walled carbon nanotubes.

[0086] Preferably, the concentration of carbon nanotubes in the carbon nanotube suspension is 0.1-100 g / L, for example, 0.1 g / L, 1 g / L, 12 g / L, 23 g / L, 34 g / L, 45 g / L, 56 g / L, 67 g / L, 78 g / L, 89 g / L or 100 g / L, etc., preferably 5 g / L.

[0087] Preferably, the ratio of the oxide core to the suspension containing carbon nanotubes is 20-100 g / L, for example, it can be 20 g / L, 29 g / L, 38 g / L, 47 g / L, 56 g / L, 65 g / L, 74 g / L, 83 g / L, 92 g / L or 100 g / L, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0088] Preferably, the oxide cores are mixed with the suspension containing carbon nanotubes by stirring followed by ultrasonication.

[0089] Preferably, the power of the ultrasound is 1000-3000 W, for example, it can be 1000 W, 1223 W, 1445 W, 1667 W, 1889 W, 2112 W, 2334 W, 2556 W, 2778 W or 3000 W, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0090] Preferably, the ultrasonic time is 10 to 100 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min or 100 min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0091] The present invention has no special limitation on the solid-liquid separation in the above process. Any device and method for solid-liquid separation known to those skilled in the art can be used, and can also be adjusted according to the actual process, such as filtration, centrifugation or sedimentation separation, or a combination of different methods.

[0092] The present invention has no particular limitation on the drying in the above process. Any drying device and method known to those skilled in the art can be used, and can also be adjusted according to the actual process, for example, it can be air drying, vacuum drying, oven drying or freeze drying, or a combination of different methods.

[0093] In a third aspect, the present invention provides a positive electrode material, which includes the positive electrode active material prepared by coating the carbon nanotube-doped precursor as described in the first aspect.

[0094] The positive electrode material prepared in the third aspect of the present invention has excellent electrochemical properties and can improve the cycle performance and rate performance of the battery.

[0095] The present invention has no limitation on the structure of the positive electrode material and other materials, and any structure and other materials that can be used for the positive electrode material and are known to those skilled in the art can be used.

[0096] Preferably, the molar ratio of the sum of nickel, cobalt and manganese to lithium in the positive electrode material is 1:(1-1.1), for example, it can be 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1.1, etc.

[0097] Preferably, the method for preparing the positive electrode material comprises: mixing a carbon nanotube-coated doping precursor and a lithium source to obtain a mixture, and sintering the mixture to obtain the positive electrode material.

[0098] Preferably, the molar ratio of nickel, cobalt and manganese contained in the carbon nanotube-coated doping precursor to lithium in the lithium source is 1:(1-1.1), for example, it can be 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09 or 1:1.1, etc.

[0099] Preferably, the sintering comprises a first sintering stage and a second sintering stage:

[0100] Preferably, the temperature of the first sintering stage is 400-700°C, for example, it can be 400°C, 434°C, 467°C, 500°C, 534°C, 567°C, 600°C, 634°C, 667°C or 700°C, the time is 3-6h, for example, it can be 3h, 3.4h, 3.7h, 4h, 4.4h, 4.7h, 5h, 5.4h, 5.7h or 6h, and the heating rate is 2-6°C / min, for example, it can be 2°C / min, 2.5°C / min, 2.9°C / min, 3.4°C / min, 3.8°C / min, 4.3°C / min, 4.7°C / min, 5.2°C / min, 5.6°C / min or 6°C / min, etc.

[0101] Preferably, the temperature of the second sintering stage is 700-1000°C, for example, it can be 700°C, 734°C, 767°C, 800°C, 834°C, 867°C, 900°C, 934°C, 967°C or 1000°C, the time is 10-20h, for example, it can be 10h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h or 20h, and the heating rate is 2-6°C / min, for example, it can be 2°C / min, 2.5°C / min, 2.9°C / min, 3.4°C / min, 3.8°C / min, 4.3°C / min, 4.7°C / min, 5.2°C / min, 5.6°C / min or 6°C / min, etc.

[0102] Compared with the prior art, the present invention has at least the following beneficial effects:

[0103] (1) The carbon nanotube-coated doped precursor provided by the present invention has an internal core with a doped metal M and an external carbon nanotube coating, and has the advantages of both. The core and the carbon nanotube coating layer cooperate with each other, which can effectively improve the surface structure of the precursor, and can improve the rate performance and cycle performance of the battery. Under preferred conditions, after the carbon nanotube-coated doped precursor is prepared to form a lithium-ion battery, the 0.2C first discharge capacity is above 212.2mAh / g, the 0.2C first efficiency reaches above 91.4%, and the 100-cycle capacity retention rate reaches above 86.3%. The battery has excellent rate performance, the 1C first discharge capacity is above 201.5mAh / g, and the 1C first efficiency reaches above 88.2%;

[0104] (2) The method for preparing the carbon nanotube-coated doped precursor provided by the present invention adopts a co-precipitation method, which is simple and easy to operate, low in cost, and controls the preparation of the core first and spray pyrolysis to form an oxide core, and then prepares the carbon nanotube coating layer, which can strictly control the particle size of the carbon nanotube-coated doped precursor and improve the electrochemical performance;

[0105] (3) The preparation method of the carbon nanotube-coated doped precursor provided by the present invention preferably adopts four stages in the coprecipitation process, and combines the pulping, sand milling and spray pyrolysis processes, which can improve the distribution uniformity of the doped metal M and ultimately improve the rate performance and cycle performance of the battery;

[0106] (4) The positive electrode material provided by the present invention has excellent performance and can be used in batteries to better improve the rate performance and cycle performance of the battery, and has broad application prospects; BRIEF DESCRIPTION OF THE DRAWINGS

[0107] Figure 1 This is a surface SEM image of the carbon nanotube-coated doped precursor provided in Example 1 of the present invention.

[0108] Figure 2 This is the electron probe image corresponding to Ce doping in the carbon nanotube-coated doping precursor provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0109] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0110] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0111] Example 1

[0112] This embodiment provides a carbon nanotube coated doping precursor, which includes a core and a carbon nanotube coating layer coated on the outside of the core; the core includes nickel oxide, cobalt oxide and manganese oxide.

[0113] The doped metal M in the core includes doped metal M atoms attached to the carbon nanotube coating layer; the molar ratio of nickel, cobalt and manganese in the core is 80:10:10; the doped metal M in the core accounts for 0.5% of the total molar percentage of nickel, cobalt and manganese; the content of carbon nanotubes in the carbon nanotube coating doped precursor is 1wt%; the density of the carbon nanotube coating layer is 100m 2 / g; the doping metal M is cerium. The size of the core is 4.5 μm; the particle distribution span of the core is 1.0-1.5; the distribution uniformity of the doping metal M in the core is to form a uniformly dispersed distribution ring; the thickness of the carbon nanotube coating layer is 5 nm; the particle size range of the carbon nanotube-coated doping precursor is 4-5 μm.

[0114] This embodiment also provides a method for preparing the above carbon nanotube-coated doped precursor, the preparation method comprising the following steps:

[0115] Ternary salt solution: a mixed acetate solution in which the molar ratio of Ni, Co and Mn is 80:10:10, wherein the concentration of the solute is 80 g / L.

[0116] Doped cerium salt solution: 30g / L cerium trichloride solution.

[0117] Precipitating agent: 30 wt% sodium hydroxide solution; complexing agent: 12 wt% ammonia water.

[0118] (1) Prepare the base solution: 3 Add 670L of pure water and a certain amount of NaOH solution and ammonia water into the reactor, and 3 / h rate of nitrogen gas into the bottom liquid, stirring at a speed of 100r / min to make it evenly mixed, and then raising the temperature to 55 ° C, controlling the pH value to 11.3, the ammonia concentration to 5.5g / L, and the total alkalinity to 18g / L.

[0119] (2) First reaction: The reaction temperature is controlled at 60°C, the stirring speed is 300 r / min, the pH is 11-12, the ammonia value is 7-9 g / L, the flow rates of ammonia water, alkali solution, ternary salt solution, and doped cerium salt solution are adjusted, and the following stage reactions are carried out to form a preliminary core.

[0120] The first stage reaction: the complexing agent, precipitant, ternary salt solution and doped cerium salt solution are introduced into the reactor at the same time, so that the total molar percentage of cerium in the ternary elements of Ni, Co and Mn is 0.5%, the pH is stabilized at 11-11.3, and the first stage reaction is completed when the internal nucleation is completed and the stable growth is 3.5 μm; in the first stage reaction, the flow rate of the complexing agent is controlled to be 700 ml / L, the flow rate of the precipitant is 1.4 L / h, the flow rate of the ternary salt solution is 4 L / h, the flow rate of the doped metal salt solution is 200 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.0-11.3;

[0121] Second stage reaction: raise the reaction pH to 11.4-11.6. During the second stage reaction, the particle span is about 1.5-2 and fine particles are observed to be uniformly dispersed around the large particles. When D50 drops to about 2.5-3 μm, the second stage reaction ends. In the second stage reaction, the flow rate of the complexing agent is controlled to be 700 ml / L, the flow rate of the precipitant is 1.7 L / h, the flow rate of the ternary salt solution is 6 L / h, the flow rate of the doped metal salt solution is 400 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.4-11.6.

[0122] The third stage reaction: aging the materials in the reactor and extracting small particles (with a particle size range of <1 μm) to obtain aged materials; extracting the first particles in the aged materials, and performing seed-stable growth on the first particles to 1.0-1.5 μm to obtain grown particles; and putting the grown particles into the aged materials to continue the subsequent fourth stage reaction;

[0123] According to the ratio of water to the first particle being 3.5 L / kg, the process of stable seed growth includes: mixing water and the first particle, then introducing a doped cerium salt solution, a ternary salt solution, a precipitant and a complexing agent to perform stable seed growth, and then aging, filtering and washing to obtain grown particles; during the stable seed growth, the flow rate of the complexing agent is controlled to be 400 ml / L, the flow rate of the precipitant is controlled to be 1.0 L / h, the flow rate of the ternary salt solution is controlled to be 3 L / h, and the flow rate of the doped cerium salt solution is controlled to be 300 ml / h, the temperature is controlled to be 55° C., and the stirring speed is controlled to be 350 rpm;

[0124] Fourth stage reaction: continue the fourth stage reaction in the reactor until the finished product is 4-5 μm, and then stop the reaction after the finished product weighing reaches the target value; in the fourth stage reaction, the flow rate of the complexing agent is controlled to be 900 ml / L, the flow rate of the precipitant is controlled to be 2.8 L / h, the flow rate of the ternary salt solution is controlled to be 9 L / h, the flow rate of the doped cerium salt solution is controlled to be 300 ml / h, the ammonia concentration is controlled to be 5-7 g / L, and the pH is controlled to be 10.2-10.5.

[0125] (3) washing and drying the obtained system containing the preliminary core, wherein the washing is performed by water washing five times, and the drying is performed by drying at a temperature of 90° C. to obtain a core powder.

[0126] (4) The core powder is transferred into a slurry kettle for slurry treatment, the solid content of the slurry is 30%, and then sand-milled with a 0.5 mm zirconium ball for 8 hours to obtain a sand-milled material; the sand-milled material is pumped into the feed port of a spray dryer for spray pyrolysis, the inlet temperature is controlled at 250° C., and the outlet temperature is controlled at 100° C. to obtain an oxide core.

[0127] (5) Activating the multi-walled carbon nanotubes to obtain a suspension containing carbon nanotubes at a concentration of 5 g / L, adding the oxide cores prepared in step (4), stirring and ultrasonicating at 1.2 kW for 20 min, filtering, washing three times with clean water, and drying in an oven at 100° C. to obtain a carbon nanotube-coated doped precursor.

[0128] This embodiment also provides a method for preparing a positive electrode material, the preparation method comprising:

[0129] The carbon nanotube coated doped precursor and lithium hydroxide are batch mixed in a high-speed mixer, the molar ratio of the sum of Ni, Co and Mn elements in the carbon nanotube coated doped precursor to lithium in lithium hydroxide is 1:1.05, and the obtained mixture is sintered in a box furnace, and the sintering includes a first stage sintering and a second stage sintering, the first stage sintering temperature is 450°C, the time is 5h, and the heating rate is 4°C / min, the second stage sintering temperature is 850°C, the time is 20h, and the heating rate is 3.5°C / min. The sintered material is cooled, crushed and sieved to obtain the positive electrode material.

[0130] Figure 1 This is a surface SEM image of the carbon nanotube-coated doped precursor in Example 1 of the present application. Figure 1 The morphology of uniform distribution of large and small particles is obtained, which is beneficial to improve the tap density of the material while taking into account the electrochemical cycle performance and capacity of the material. Figure 2 This is the electron probe image corresponding to Ce doping in the carbon nanotube-coated doping precursor. Figure 2It can be seen that the cerium element is uniformly doped inside the particles and the general outline of the particles can be observed, indicating that relatively uniform doping is achieved during the reaction process.

[0131] Example 2

[0132] This embodiment provides a carbon nanotube coated doping precursor, which includes a core and a carbon nanotube coating layer coated on the outside of the core; the core includes nickel oxide, cobalt oxide and manganese oxide.

[0133] The doped metal M in the core includes doped metal M atoms attached to the carbon nanotube coating layer; the molar ratio of nickel, cobalt and manganese in the core is 88:10:2; the doped metal M in the core accounts for 5% of the total molar percentage of nickel, cobalt and manganese; the content of carbon nanotubes in the carbon nanotube coating doped precursor is 1.5wt%; the density of the carbon nanotube coating layer is 200m 2 / g; the doped metal M is cerium. The size of the core is 4.0 μm; the particle distribution span of the core is 1.0-1.5; the distribution uniformity of the doped metal M in the core is to form a uniformly dispersed distribution ring; the thickness of the carbon nanotube coating layer is 1 nm; the particle size range of the carbon nanotube-coated doped precursor is 4.5-5 μm.

[0134] This embodiment also provides a method for preparing the above carbon nanotube-coated doped precursor, the preparation method comprising the following steps:

[0135] Ternary salt solution: a mixed acetate solution in which the molar ratio of Ni, Co and Mn is 88:10:2, wherein the concentration of the solute is 120 g / L.

[0136] Doped cerium salt solution: 50g / L cerium nitrate solution.

[0137] Precipitating agent: 32 wt% sodium hydroxide solution; complexing agent: 13 wt% ammonia water.

[0138] (1) Prepare the base solution: 3 Add 650L of pure water and a certain amount of NaOH solution and ammonia water into the reactor, and 3 / h rate of nitrogen gas into the bottom liquid, stirring at a speed of 200r / min to make it evenly mixed, and then raising the temperature to 40 ° C, controlling the pH value to 10.2, the ammonia concentration to 4.2g / L, and the total alkalinity to 19.5g / L.

[0139] (2) First reaction: The reaction temperature is controlled at 45°C, the stirring speed is 250 r / min, the pH is 11-12, the ammonia value is 7-9 g / L, the flow rates of ammonia water, alkali solution, ternary salt solution, and doped cerium salt solution are adjusted, and the following stage reactions are carried out to form a preliminary core.

[0140] The first stage reaction: the complexing agent, the precipitating agent, the ternary salt solution and the doped cerium salt solution are introduced into the reactor at the same time, so that the total molar percentage of cerium in the ternary elements of Ni, Co and Mn is 3.5%, the pH is stabilized at 11.1-11.4, and the first stage reaction ends when the internal nucleation is completed and the stable growth reaches 3.0 μm; in the first stage reaction, the flow rate of the complexing agent is controlled to be 600 ml / L, the flow rate of the precipitating agent is controlled to be 1.2 L / h, the flow rate of the ternary salt solution is controlled to be 3 L / h, the flow rate of the doped cerium salt solution is controlled to be 100 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.12-11.3;

[0141] The second stage reaction: the reaction pH is raised to 11.4-11.6. During the second stage reaction, the particle span is about 1.5-2 and fine particles are observed to be uniformly dispersed around the large particles. When the D50 drops to about 2.5-2.8 μm, the second stage reaction ends. In the second stage reaction, the flow rate of the complexing agent is controlled to be 800 ml / L, the flow rate of the precipitant is 2.0 L / h, the flow rate of the ternary salt solution is 8 L / h, the flow rate of the doped cerium salt solution is 500 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.3-11.6.

[0142] The third stage reaction: aging the materials in the reactor and extracting small particles (with a particle size range of <1 μm) to obtain aged materials; extracting the first particles in the aged materials, and performing seed-stable growth on the first particles to 1.0-1.5 μm to obtain grown particles; and putting the grown particles into the aged materials to continue the subsequent fourth stage reaction;

[0143] According to the ratio of water to the first particles being 5 L / kg, the process of stable seed growth comprises: mixing water and the first particles, then introducing a doped metal salt solution, a ternary salt solution, a precipitant and a complexing agent to perform stable seed growth, and then aging, filtering and washing to obtain grown particles; during the stable seed growth, the flow rate of the complexing agent is controlled to be 500 ml / L, the flow rate of the precipitant is controlled to be 1.2 L / h, the flow rate of the ternary salt solution is controlled to be 5 L / h, the flow rate of the doped cerium salt solution is controlled to be 500 ml / h, the temperature is controlled to be 60° C., and the stirring speed is controlled to be 300 rpm;

[0144] Fourth stage reaction: continue the fourth stage reaction in the reactor until the finished product is 4.5-5 μm, and then stop the reaction after the finished product weighing reaches the target value; in the fourth stage reaction, the flow rate of the complexing agent is controlled to be 800 ml / L, the flow rate of the precipitant is controlled to be 2.5 L / h, the flow rate of the ternary salt solution is controlled to be 8 L / h, the flow rate of the doped metal salt solution is controlled to be 100 ml / h, the ammonia concentration is controlled to be 5-7 g / L, and the pH is controlled to be 10.2-10.5.

[0145] (3) washing and drying the obtained system containing the preliminary core, wherein the washing is performed by water washing five times, and the drying is performed by drying at a temperature of 90° C. to obtain a core powder.

[0146] (4) The core powder is transferred into a slurry kettle for slurry treatment, the solid content of the slurry is 20%, and then sand-milled with a 1.0 mm zirconium ball for 10 hours to obtain a sand-milled material; the sand-milled material is pumped into the feed port of a spray dryer for spray pyrolysis, the inlet temperature is controlled at 200° C., and the outlet temperature is controlled at 80° C. to obtain an oxide core.

[0147] (5) Activating the multi-walled carbon nanotubes to obtain a suspension containing carbon nanotubes at a concentration of 25 g / L, adding the oxide cores prepared in step (4), stirring and ultrasonicating at 2 kW for 35 min, filtering and washing four times with clean water, and then drying in an oven at 120° C. to obtain a carbon nanotube-coated doped precursor.

[0148] This embodiment also provides a method for preparing a positive electrode material, the preparation method comprising:

[0149] The carbon nanotube coated doped precursor and lithium hydroxide are batch mixed in a high-speed mixer, the molar ratio of the sum of Ni, Co and Mn elements in the carbon nanotube coated doped precursor to lithium in lithium hydroxide is 1:1.1, and the obtained mixture is sintered in a box furnace, and the sintering includes a first stage sintering and a second stage sintering, the first stage sintering temperature is 700°C, the time is 6h, and the heating rate is 2°C / min, the second stage sintering temperature is 1000°C, the time is 10h, and the heating rate is 2.0°C / min. The sintered material is cooled, crushed and sieved to obtain the positive electrode material.

[0150] Example 3

[0151] This embodiment provides a carbon nanotube coated doping precursor, which includes a core and a carbon nanotube coating layer coated on the outside of the core; the core includes nickel oxide, cobalt oxide and manganese oxide.

[0152] The doped metal M in the core includes doped metal M atoms attached to the carbon nanotube coating layer; the molar ratio of nickel, cobalt and manganese in the core is 70:20:10; the doped metal M in the core accounts for 0.25% of the total molar percentage of nickel, cobalt and manganese; the content of carbon nanotubes in the carbon nanotube coating doped precursor is 2.5wt%; the density of the carbon nanotube coating layer is 250m 2 / g; the doped metal M is cerium. The size of the core is 4.8 μm; the particle distribution span of the core is 1.2 to 1.5; the distribution uniformity of the doped metal M in the core is to form a uniformly dispersed distribution ring; the thickness of the carbon nanotube coating layer is 6 nm; the particle size range of the carbon nanotube-coated doped precursor is 4.2 to 4.8 μm.

[0153] This embodiment also provides a method for preparing the above carbon nanotube-coated doped precursor, the preparation method comprising the following steps:

[0154] Ternary salt solution: a mixed acetate solution in which the molar ratio of Ni, Co and Mn is 70:20:10, wherein the concentration of the solute is 50 g / L.

[0155] Doped cerium salt solution: 10g / L cerium sulfate solution.

[0156] Precipitating agent: 28 wt% sodium hydroxide solution; complexing agent: 10 wt% ammonia water.

[0157] (1) Prepare the base solution: 3 500L of pure water and a certain amount of NaOH solution and ammonia water were added to the reactor. 0.5 m 3 / h rate of nitrogen gas into the bottom liquid, stirring at a speed of 150r / min to make it evenly mixed, and then raising the temperature to 60 ° C, controlling the pH value to 11.2, the ammonia concentration to 5.5g / L, and the total alkalinity to 15.5g / L.

[0158] (2) First reaction: The reaction temperature is controlled at 60°C, the stirring speed is 380 r / min, the pH is 11-12, the ammonia value is 7-9 g / L, the flow rates of ammonia water, alkali solution, ternary salt solution, and doped cerium salt solution are adjusted, and the following stage reactions are carried out to form a preliminary core.

[0159] The first stage reaction: the complexing agent, the precipitating agent, the ternary salt solution and the doped cerium salt solution are introduced into the reactor at the same time, so that the cerium accounts for 0.1% of the total molar percentage of the ternary elements of Ni, Co and Mn, the pH is stabilized at 11.2-11.4, and the first stage reaction is completed when the internal nucleation is completed and the stable growth is 4.0 μm; in the first stage reaction, the flow rate of the complexing agent is controlled to be 800 ml / L, the flow rate of the precipitating agent is controlled to be 1.6 L / h, the flow rate of the ternary salt solution is controlled to be 6 L / h, the flow rate of the doped cerium salt solution is controlled to be 500 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.02-11.28;

[0160] The second stage reaction: the reaction pH is raised to 11.5-12. During the second stage reaction, the particle span is about 1.5-2 and fine particles are observed to be uniformly dispersed around the large particles. When the D50 drops to about 2.5-2.8 μm, the second stage reaction ends. In the second stage reaction, the flow rate of the complexing agent is controlled to be 600 ml / L, the flow rate of the precipitant is controlled to be 1.6 L / h, the flow rate of the ternary salt solution is controlled to be 4 L / h, the flow rate of the doped cerium salt solution is controlled to be 400 ml / h, the ammonia concentration is controlled to be 7-9 g / L, and the pH is controlled to be 11.3-11.6.

[0161] The third stage reaction: aging the materials in the reactor and extracting small particles (with a particle size range of <1 μm) to obtain aged materials; extracting the first particles in the aged materials, and performing seed-stable growth on the first particles to 1.0-1.5 μm to obtain grown particles; and putting the grown particles into the aged materials to continue the subsequent fourth stage reaction;

[0162] According to the ratio of water to the first particles being 3 L / kg, the process of stable seed growth comprises: mixing water and the first particles, then introducing a doped metal salt solution, a ternary salt solution, a precipitant and a complexing agent to perform stable seed growth, and then aging, filtering and washing to obtain grown particles; during the stable seed growth, the flow rate of the complexing agent is controlled to be 300 ml / L, the flow rate of the precipitant is controlled to be 0.8 L / h, the flow rate of the ternary salt solution is controlled to be 2 L / h, and the flow rate of the doped cerium salt solution is controlled to be 100 ml / h, the temperature is controlled to be 50° C., and the stirring speed is controlled to be 400 rpm;

[0163] Fourth stage reaction: continue the fourth stage reaction in the reactor until the finished product is 4.0-4.3 μm, and then start to receive the finished product, and stop the reaction after the finished product weighing reaches the target value; in the fourth stage reaction, the flow rate of the complexing agent is controlled to be 1000 ml / L, the flow rate of the precipitant is controlled to be 3.0 L / h, the flow rate of the ternary salt solution is controlled to be 10 L / h, the flow rate of the doped metal salt solution is controlled to be 500 ml / h, the ammonia concentration is controlled to be 5-7 g / L, and the pH is controlled to be 10.2-10.5.

[0164] (3) washing and drying the obtained system containing the preliminary core, wherein the washing is performed by water washing five times, and the drying is performed by drying at a temperature of 90° C. to obtain a core powder.

[0165] (4) The core powder is transferred into a slurrying kettle for slurrying treatment, the solid content of the slurry is 40%, and then sand-milled with a 0.8 mm zirconium ball for 6 hours to obtain a sand-milled material; the sand-milled material is pumped into the feed port of a spray dryer for spray pyrolysis, the inlet temperature is controlled at 300° C., and the outlet temperature is controlled at 150° C. to obtain an oxide core.

[0166] (5) Activating the multi-walled carbon nanotubes to obtain a suspension containing carbon nanotubes at a concentration of 50 g / L, adding the oxide cores prepared in step (4), stirring and ultrasonicating at 3 kW for 40 min, filtering and washing three times with clean water, and then drying in an oven at 80° C. to obtain a carbon nanotube-coated doped precursor.

[0167] This embodiment also provides a method for preparing a positive electrode material, the preparation method comprising:

[0168] The carbon nanotube coated doped precursor and lithium hydroxide are batch mixed in a high-speed mixer, the molar ratio of the sum of Ni, Co and Mn elements in the carbon nanotube coated doped precursor to the lithium in the lithium hydroxide is 1:1, and the obtained mixture is sintered in a box furnace, and the sintering includes a first stage sintering and a second stage sintering, the first stage sintering temperature is 400°C, the time is 6h, and the heating rate is 2.5°C / min, the second stage sintering temperature is 700°C, the time is 20h, and the heating rate is 6°C / min. The sintered material is cooled, crushed and sieved to obtain a positive electrode material.

[0169] Example 4

[0170] The only difference between this embodiment and embodiment 1 is that the molar percentage of cerium in the total molar percentage of the ternary elements Ni, Co and Mn is 0.05%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0171] Example 5

[0172] The only difference between this embodiment and embodiment 1 is that the molar percentage of cerium in the total molar percentage of the ternary elements Ni, Co and Mn is 0.1%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0173] Example 6

[0174] The only difference between this embodiment and embodiment 1 is that the molar percentage of cerium in the total molar percentage of the ternary elements Ni, Co and Mn is 1%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0175] Example 7

[0176] The only difference between this embodiment and embodiment 1 is that the molar percentage of cerium in the total molar percentage of the ternary elements Ni, Co and Mn is 5%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0177] Example 8

[0178] The only difference between this embodiment and embodiment 1 is that the third stage reaction is not carried out, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0179] Example 9

[0180] The only difference between this embodiment and embodiment 1 is that the pH of the first stage reaction is 11.4-11.6, which is the same as the pH of the second stage reaction, and the flow rate of the precipitant in the first stage reaction is increased accordingly. Other conditions and parameters are exactly the same as those in embodiment 1.

[0181] Example 10

[0182] The only difference between this embodiment and embodiment 1 is that the pH of the first stage reaction is 11.7-12, that is, greater than the pH of the second stage reaction, and the flow rate of the precipitant in the first stage reaction is increased accordingly. Other conditions and parameters are exactly the same as those in embodiment 1.

[0183] Embodiment 11

[0184] The only difference between this embodiment and the first embodiment is that the first particles are subjected to seed-stable growth to 3.0-3.5 μm alone, and the other conditions and parameters are exactly the same as those in the first embodiment.

[0185] Example 12

[0186] The only difference between this embodiment and the first embodiment is that the first particles are subjected to seed-stable growth to a size of 0.5 to 0.95 μm. Other conditions and parameters are exactly the same as those in the first embodiment.

[0187] Example 13

[0188] The only difference between this embodiment and embodiment 1 is that the cerium trichloride solution is replaced by yttrium chloride solution, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0189] Embodiment 14

[0190] The only difference between this embodiment and embodiment 1 is that the cerium trichloride solution is replaced by a zirconium chloride solution, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0191] Comparative Example 1

[0192] This comparative example provides a method for preparing a precursor. The specific steps can refer to Example 1, except that step (5) is not performed.

[0193] Comparative Example 2

[0194] This comparative example provides a method for preparing a precursor. The specific steps can refer to Example 1, except that step (4) is not performed, and the core powder is directly mixed with the suspension containing carbon nanotubes and step (5) is performed.

[0195] Comparative Example 3

[0196] This comparative example provides a method for preparing a precursor. The specific steps can refer to Example 1, except that the spray pyrolysis in step (4) is not performed, and the sand-milled material is directly mixed with the suspension containing carbon nanotubes and step (5) is performed.

[0197] Comparative Example 4

[0198] This comparative example provides a method for preparing a precursor. The specific steps can refer to Example 1, except that the sand grinding in step (4) is not performed, and the slurry treated with slurry is directly subjected to spray pyrolysis.

[0199] Comparative Example 5

[0200] This comparative example provides a method for preparing a precursor. The specific steps can refer to Example 1, except that no doped cerium salt solution is added in the first reaction.

[0201] Performance Test:

[0202] The positive electrode material obtained in the above embodiments and comparative examples is used as a positive electrode active material, and is mixed with conductive carbon and PVDF in a ratio of 94:3:3, and then the mixture is dispersed in methyl pyrrolidone (NMP) as a solvent to obtain a positive electrode slurry, which is evenly coated on an aluminum foil. After coating, the current collector is punched to obtain a coin-shaped electrode, and the positive electrode is obtained after vacuum drying at 120°C overnight. Metal lithium is selected as the negative electrode, and 1.0M LiPF6 is injected into ethylene carbonate (EC) / methyl carbonate (EMC) (1:2 vol%) electrolyte. The positive electrode, the negative electrode, and the separator are wound to prepare a battery cell, and then a lithium-ion battery is assembled through packaging, liquid injection, formation, and capacity division.

[0203] The prepared lithium-ion battery was subjected to electrochemical performance tests at a test voltage of 3.0 to 4.3 V. The first discharge capacity and first efficiency were measured at 0.2C and 1C. The discharge capacity of the battery at the first cycle and the discharge capacity at the 100th cycle were tested at 1C to obtain the capacity retention rate after 100 cycles. The test results are shown in Table 1.

[0204] Table 1

[0205]

[0206] Referring to Table 1, we can draw the following conclusions:

[0207] (1) It can be seen from Examples 1 to 3 that after the carbon nanotube-coated doped precursor provided by the present invention is prepared into a lithium-ion battery, the 0.2C first discharge capacity is above 212.2 mAh / g, the 0.2C first efficiency reaches above 91.4%, and the 100-cycle capacity retention rate reaches above 86.3%. The battery has excellent rate performance, the 1C first discharge capacity is above 201.5 mAh / g, and the 1C first efficiency reaches above 88.2%, and the application prospect is broad;

[0208] (2) It can be seen from Example 1 and Examples 4 to 7 that the doping metal M is doped in the range of 0.05 to 5% by molar ratio, preferably in the range of 0.15 to 4.5%, which refines the grains, shortens the distance of lithium ion transmission, improves the rate performance and cycle performance of the material, stabilizes the crystal structure, and improves the safety during the electrochemical reaction;

[0209] (3) Combining Example 1 and Example 8, it can be seen that in Example 1, the first reaction is carried out in four stages. After the positive electrode material of Example 1 is prepared into a lithium ion battery, the first discharge capacity at 0.2C is 212.2 mAh / g, and the cycle efficiency of 100 weeks is 86.3%; the first discharge capacity at 1C is 201.5 mAh / g, and the first efficiency of 1C is 88.4%. In Example 8, the third stage reaction is not carried out, and the fourth stage reaction is directly carried out to grow to the precursor of the corresponding particle size. Finally, the first discharge capacity at 0.2C is 191.5 mAh / g, and the cycle efficiency of 100 weeks is 80.2%; the first discharge capacity at 1C is 182.8 mAh / g, and the first efficiency of 1C is 76.9%. This shows that the present invention performs the first reaction in four preferred stages, and in the third stage, the small particles are separately seeded, which is more conducive to improving the uniformity of the precursor particle distribution and the doping uniformity of the doped metal M, and the electrochemical performance of the final material is better;

[0210] (4) Combining Example 1 and Examples 9 to 10, it can be seen that the pH of the first stage reaction in Example 1 is less than the pH of the second stage reaction. After the positive electrode material of Example 1 is prepared into a lithium ion battery, the first discharge capacity at 0.2C is 212.2mAh / g, and the cycle efficiency of 100 weeks is 86.3%; the first discharge capacity at 1C is 201.5mAh / g, and the first efficiency at 1C is 88.4%. In Examples 9 to 10, the pH of the first stage reaction is controlled to be equal to the pH of the second stage reaction and the pH of the first stage reaction is greater than the pH of the second stage reaction. In Examples 9 to 10, the cycle efficiency of 100 weeks at 0.1C is only 84.9% and 84.1%, respectively, and the first discharge capacity and first efficiency at 0.1C and 1C are also significantly reduced. This shows that the present invention can improve the distribution uniformity of particles and avoid agglomeration of secondary particles on the surface by preferably controlling the pH of the first stage reaction to be less than the pH of the second stage reaction, and finally further improve the rate performance, cycle performance and first discharge capacity of the material.

[0211] (5) Combining Example 1 and Examples 11 to 12, it can be seen that when the growth particle size of the seed in Example 11 is larger than the preferred range, the difference in particle size between large and small particles in the system will be reduced, and the compactness of the accumulation in the subsequent process of preparing the positive electrode by doping large and small particles is lower than that in Example 1. Finally, the energy density of Example 1 will be better than that of Example 11. However, when the growth particle size of the seed in Example 12 is too small, the growth rate of large and small particles is uneven due to the different surface areas, resulting in uneven particle size distribution, which ultimately leads to better rate performance and cycle performance in Example 1 than in Example 12. This shows that the present invention can be more conducive to improving the electrochemical performance of the material by controlling the particle size of the first particle after the seed growth in the third stage reaction within a reasonable range;

[0212] (6) It can be seen from Example 1 and Examples 13 to 14 that zirconium has better doping performance than other doping metals;

[0213] (7) It can be seen from Example 1 and Comparative Examples 1 to 5 that the coating (Comparative Example 1), slurry treatment, grinding (Comparative Example 4) and spray pyrolysis (Comparative Example 2, Comparative Example 3) of the carbon nanotubes in the present invention and the doping of the doped metal M are critical for ultimately obtaining a precursor with excellent electrochemical properties. These features are combined and cooperate with each other to ultimately improve the rate performance, cycle performance, first discharge capacity and first efficiency of the material.

[0214] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A carbon nanotube-coated doped precursor, characterized in that: The carbon nanotube-coated doped precursor comprises a core and a carbon nanotube coating layer coated outside the core; The core comprises a nickel-cobalt-manganese ternary precursor core containing a doping metal M; The doping metal M includes any one of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum, or a combination of at least two thereof.

2. The carbon nanotube-coated doped precursor according to claim 1, characterized in that: The core comprises nickel oxide, cobalt oxide and manganese oxide; Preferably, the doped metal M in the core comprises doped metal M atoms attached to the carbon nanotube coating layer; Preferably, the molar ratio of nickel, cobalt and manganese in the core is (60-90):(10-20):(0-20), preferably 80:10:10; Preferably, the doped metal M in the core accounts for 0.05 to 5% of the total molar percentage of nickel, cobalt and manganese; Preferably, the content of carbon nanotubes in the carbon nanotube-coated doping precursor is 0.1 to 10 wt %; Preferably, the density of the carbon nanotube coating is 100 to 1000 m 2 / g; Preferably, the doping metal M is cerium.

3. The carbon nanotube-coated doped precursor according to claim 1 or 2, characterized in that: The size of the core is 4 to 5 μm; Preferably, the core has a particle distribution span of 1.0 to 1.5; Preferably, the thickness of the carbon nanotube coating layer is 1 to 10 nm; Preferably, the particle size of the carbon nanotube-coated doping precursor is in the range of 4 to 5 μm.

4. A method for preparing a carbon nanotube-coated doped precursor according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: A base liquid containing ammonia is prepared, and then a doping metal salt solution, a ternary salt solution, a precipitant and a complexing agent are introduced into the base liquid to perform a first reaction to form a preliminary core; The preliminary core is aged and dried in sequence to obtain core powder; The core powder is sequentially slurried, ground and spray-pyrolyzed to obtain an oxide core; The oxide core is mixed with a suspension containing carbon nanotubes and dried to obtain the carbon nanotube-coated doping precursor.

5. The preparation method according to claim 4, characterized in that: The first reaction is carried out in a reaction atmosphere; Preferably, the reaction atmosphere comprises nitrogen; Preferably, the nitrogen introduction rate is 0.2 to 2 m 3 / h; Preferably, the precipitant comprises an alkaline solution, preferably the precipitant is a sodium hydroxide solution; Preferably, the concentration of the alkaline solution is 30-35wt%; Preferably, the complexing agent comprises aqueous ammonia; Preferably, the concentration of the ammonia water is 10-20wt%; Preferably, the ammonia concentration of the base solution is 4 to 10 g / L; Preferably, the pH of the base solution is 10 to 12; Preferably, the temperature of the base liquid is 40-60°C.

6. The preparation method according to claim 4 or 5, characterized in that: The ternary salt solution includes nickel salt, cobalt salt, manganese salt and doped metal salt; Preferably, the nickel salt comprises any one of nickel sulfate, nickel nitrate, nickel acetate or nickel chloride or a combination of at least two thereof, preferably nickel acetate; Preferably, the cobalt salt comprises any one of cobalt sulfate, cobalt nitrate, cobalt acetate or cobalt chloride, or a combination of at least two thereof, preferably cobalt acetate; Preferably, the manganese salt comprises any one of manganese sulfate, manganese nitrate, manganese acetate or manganese chloride, or a combination of at least two thereof, preferably manganese acetate; Preferably, the total concentration of Ni, Co and Mn in the ternary salt solution is 20 to 120 g / L; Preferably, the molar ratio of Ni, Co and Mn in the ternary salt solution is (60-90):(10-20):(0-20), preferably 80:10:10; The doping metal M in the doping metal salt solution includes any one or a combination of at least two of aluminum, titanium, niobium, zirconium, tungsten, vanadium, strontium, gallium, cerium, yttrium or lanthanum, and preferably the doping metal M is cerium; Preferably, the doping metal salt comprises any one of sulfate, nitrate, acetate or chloride, or a combination of at least two thereof; Preferably, when the doping metal M is cerium, the cerium source is any one of cerium sulfate, cerium nitrate, cerium acetate or cerium trichloride, or a combination of at least two thereof; Preferably, the doping metal M accounts for 0.05-5% of the total molar percentage of the ternary elements Ni, Co and Mn; Preferably, the concentration of the doped metal salt solution is 10-50 g / L.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The first reaction includes a first stage reaction, a second stage reaction, a third stage reaction and a fourth stage reaction performed sequentially; Preferably, in the first stage reaction, the flow rate of the complexing agent is controlled to be 600-800 ml / L, the flow rate of the precipitant is controlled to be 1.2-1.6 L / h, the flow rate of the ternary salt solution is controlled to be 3-6 L / h, and the flow rate of the doped metal salt solution is controlled to be 100-500 ml / h; Preferably, in the second stage reaction, the flow rate of the complexing agent is controlled to be 600-800 ml / L, the flow rate of the precipitant is controlled to be 1.6-2.0 L / h, the flow rate of the ternary salt solution is controlled to be 4-8 L / h, and the flow rate of the doped metal salt solution is controlled to be 100-500 ml / h; Preferably, the pH of the second stage reaction is greater than that of the first stage reaction; Preferably, the ammonia concentration in the first stage reaction is 7 to 9 g / L; Preferably, the pH in the first stage reaction is controlled to be 11 to 11.3; Preferably, the ammonia concentration in the second stage reaction is 7 to 9 g / L; Preferably, the pH in the second stage reaction is controlled to be 11.3 to 11.6; Preferably, the particle size of the particles after the first stage reaction is 3 to 4 μm; Preferably, the particle span after the second stage reaction is 1.5 to 2; Preferably, the third stage reaction comprises: aging the material after the second stage reaction to obtain an aged material; extracting first particles from the aged material, and performing seed-stable growth of the first particles alone to a first particle size range to obtain grown particles; and adding the grown particles to the aged material to continue the subsequent fourth stage reaction; the particle size range of the first particles is <1.0 μm; Preferably, the process of stable seed growth comprises: mixing water and the first particle, and then introducing a doped metal salt solution, a ternary salt solution, a precipitant and a complexing agent to perform stable seed growth; Preferably, the ratio of the water to the first particles is 3 to 5 L / kg; Preferably, during the stable growth of the seed crystal, the flow rate of the complexing agent is controlled to be 300-500 ml / L, the flow rate of the precipitant is controlled to be 0.8-1.2 L / h, the flow rate of the ternary salt solution is controlled to be 2-5 L / h, and the flow rate of the doped metal salt solution is controlled to be 100-500 ml / h; Preferably, the temperature at which the seed crystal grows stably is 50-60°C; Preferably, the stirring speed for stable growth of the seed crystal is 300-400 rpm; Preferably, the first particle size ranges from 1.0 to 1.5 μm; Preferably, in the fourth stage reaction, the flow rate of the complexing agent is controlled to be 800-1000 ml / L, the flow rate of the precipitant is controlled to be 2.5-3.0 L / h, the flow rate of the ternary salt solution is controlled to be 8-10 L / h, and the flow rate of the doped metal salt solution is controlled to be 100-500 ml / h; Preferably, the ammonia concentration in the fourth stage reaction is 5 to 7 g / L; Preferably, the pH in the fourth stage reaction is controlled at 10.2-10.

5.

8. The preparation method according to any one of claims 4 to 7, characterized in that: After the slurrying, a slurry is obtained, wherein the solid content of the slurry is 20 to 40 wt %; Preferably, the inlet temperature of the spray pyrolysis is 200°C to 300°C; Preferably, the outlet temperature of the spray pyrolysis is 80°C to 150°C.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The carbon nanotubes are single-walled carbon nanotubes and / or multi-walled carbon nanotubes, preferably multi-walled carbon nanotubes; Preferably, the concentration of carbon nanotubes in the carbon nanotube suspension is 0.1 to 100 g / L, preferably 5 g / L; Preferably, the ratio of the oxide core to the suspension containing carbon nanotubes is 20-100 g / L.

10. A positive electrode material, characterized in that: The positive electrode material comprises a positive electrode active material prepared by coating a carbon nanotube-doped precursor as claimed in any one of claims 1 to 3; Preferably, the molar ratio of the sum of nickel, cobalt and manganese to lithium in the positive electrode material is 1:(1-1.1).

Citation Information

Patent Citations

  • High-cycle positive electrode material precursor, preparation method thereof, positive electrode material and battery

    CN117276534A

  • Composite coated positive electrode material and preparation method thereof, positive electrode plate, secondary battery and electric device

    CN117543020A

  • High-nickel positive electrode material, preparation method thereof and lithium ion battery

    CN117613222A

Cited By

  • Bio-based carbon material modified ternary precursor as well as preparation method and application thereof

    CN119503911A