Preparation method of EP-grade extra-pure platinum tetrachloride
By controlling the reaction of Ag+ and Cl-, platinum tetrachloride is prepared, which solves the problems of low purity and large number of by-products in the existing technology, and achieves efficient and controllable platinum tetrachloride production, which is suitable for industrialization.
Patent Information
- Application Number
- CN202410888888.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-08
AI Technical Summary
Existing platinum tetrachloride production methods have problems such as low purity, high by-product content, and complex process steps, making it difficult to obtain efficient, controllable, and high-purity platinum tetrachloride products.
Through the extremely easy precipitation characteristics of Ag+ and Cl-, the Cl/Pt molar ratio in the solution is controlled so that [PtCl6]2- loses Cl- and is converted into PtCl4. The AgCl precipitate is separated by filtration, NO3- is removed, and then concentrated, crystallized and dried to avoid Pt4+ is reduced to obtain EP grade extra pure platinum tetrachloride.
The preparation of high-purity platinum tetrachloride is achieved, the production of by-products of PtCl2 and PtCl3 is avoided, the process flow is simplified, the cost is reduced, and it is suitable for industrial production.
Smart Images

Figure BDA0004926861860000051 
Figure BDA0004926861860000061 
Figure BDA0004926861860000072
Abstract
Description
Technical Field
[0001] The present application relates to the field of inorganic compound preparation methods, and specifically to a preparation method of EP-grade extra-pure platinum tetrachloride. Background Art
[0002] Platinum tetrachloride is an inorganic substance with the chemical formula PtCl4. It is a dark brown powder, easily soluble in water, ethanol, hydrochloric acid and acetone, and slightly soluble in acetic acid, ammonia and chloroform. It can generate hexachloroplatinic acid (chloroplatinic acid) when dissolved in hydrochloric acid. It absorbs moisture in the air and turns into yellow PtCl4·5H2O. Platinum tetrachloride is widely used in electroplating, catalysts and other fields.
[0003] At present, the production of platinum tetrachloride is mainly prepared by the method of thermal decomposition of chloroplatinic acid. Patent CN200910070646.6 reports a method for preparing platinum tetrachloride by gradually heating up and thermally decomposing chloroplatinic acid under the action of chlorine. However, this method uses highly toxic chlorine, which is costly and causes serious environmental pollution. In addition, when chloroplatinic acid is thermally decomposed, by-products such as PtCl2 and PtCl3 are inevitably produced, and it is difficult to obtain a high-purity platinum tetrachloride product with a Cl / Pt molar ratio of 4. Patent CN202011417786.9 discloses a method for preparing platinum tetrachloride by vacuum rotary evaporation of chloroplatinic acid liquid. However, since Pt-Cl belongs to a strong coordination bond, the breaking of the Pt-Cl bond requires a higher reaction temperature. Therefore, the vacuum rotary evaporation process will not only cause the loss of platinum, but also inevitably produce by-products such as PtCl2 and PtCl3. In addition, Semenova et al. of Russia reported a method for preparing platinum tetrachloride by high-pressure reaction of platinum powder and chlorine (Thermodynamic characteristics of thermal dissociation of platinum tetrachloride. Russian Chemical Bulletin, International Edition, 53, 10, 2117-2120), but the production efficiency was too low and it required continuous reaction for 5 days, which was not industrially feasible.
[0004] It can be seen from the above patent disclosure documents or literature that the existing platinum tetrachloride production method has many problems such as low purity, high by-product content, and complicated method steps. Developing an efficient and controllable method for preparing high-purity platinum tetrachloride is an urgent problem to be solved in the real industry. Summary of the invention
[0005] The present application provides a method for preparing EP grade ultra-pure platinum tetrachloride. + and Cl - The characteristic of easy precipitation is to control the Ag +The amount of Cl / Pt in the solution is controlled by the amount of Cl / Pt in the solution, so that [PtCl6] 2- Loss of Cl - Then it is converted into PtCl4. The AgCl precipitate and platinum tetrachloride solution are separated by filtration. Heat the solution to remove NO3 - Decompose, remove, and finally concentrate, crystallize, and dry to obtain platinum tetrachloride product. The AgCl precipitate produced in the process can be roasted to generate silver powder, which can be dissolved in nitric acid to prepare AgNO3 solution for recycling. The wet precipitation dechlorination method adopted by the present invention can accurately control the Cl / Pt molar ratio and will not cause Pt 4+ The reduction will not generate by-products such as PtCl2 and PtCl3, and EP grade ultra-pure platinum tetrachloride product will be obtained.
[0006] A method for preparing EP-grade extra-pure platinum tetrachloride comprises the following steps:
[0007] Step (1): using chloroplatinic acid as a raw material, adding water to prepare a chloroplatinic acid solution of a specific concentration;
[0008] Step (2): The chloroplatinic acid solution is kept at a constant temperature, the chloroplatinic acid solution is kept in a stirring state, and a silver nitrate solution of a certain stoichiometric ratio is slowly added dropwise to the chloroplatinic acid solution. The reaction formula of chloroplatinic acid and silver nitrate is as follows:
[0009] H2PtCl6+2AgNO3→PtCl4+2HNO3+2AgCl↓ (1)
[0010] Step (3): filtering the liquid after the reaction in step (2) is completed, and then removing the nitrate to obtain a platinum tetrachloride aqueous solution, wherein the reaction formula for removing the nitrate is as follows:
[0011] 4HNO3→4NO2↑+O2↑+2H2O (2)
[0012] Step (4): Concentrate and crystallize the platinum tetrachloride aqueous solution in step (3) to obtain platinum tetrachloride crystals, and finally dry the platinum tetrachloride crystals in an oven to obtain an EP grade ultra-pure platinum tetrachloride product.
[0013] In step (1), the chloroplatinic acid raw material is commercial chloroplatinic acid with a platinum content of 38 wt%.
[0014] In step (1), the platinum content of the chloroplatinic acid solution is 0.1wt% to 15wt%, preferably 0.1wt% to 5wt%, and more preferably 0.1wt% to 0.5wt%.
[0015] In a preferred embodiment, the platinum content of the chloroplatinic acid solution in step (1) is 0.2 wt%.
[0016] In step (2), the constant temperature (i.e., reaction temperature) of the chloroplatinic acid solution is 0 to 50°C, preferably 0 to 20°C, and more preferably 0 to 10°C.
[0017] In a preferred embodiment, the constant temperature (i.e., reaction temperature) of the chloroplatinic acid solution in step (2) is 5°C.
[0018] In step (2), the stirring speed of the chloroplatinic acid solution is 50 to 1000 rpm, preferably 500 rpm.
[0019] In step (2), the silver nitrate dropping speed is 0.5 to 2 drops / s, preferably 1 drop / s.
[0020] In step (2), after the silver nitrate is added, the reaction needs to be continued for a certain period of time to promote the reaction of Ag. + The conversion is complete and the reaction time is 0.5 to 5 h, preferably 1 to 3 h, and more preferably 2 to 3 h.
[0021] In a preferred embodiment, after the dropwise addition in step (2) is completed, the reaction is continued for 2.5 hours.
[0022] In step (2), the silver content of the silver nitrate solution is 0.1 to 10 wt %, preferably 0.1 to 3 wt %, and more preferably 0.1 to 0.3 wt %.
[0023] In a preferred embodiment, the silver content of the silver nitrate solution in step (2) is 0.2 wt %.
[0024] In step (2), the molar amount of the silver nitrate added dropwise is twice the molar amount of chloroplatinic acid.
[0025] In step (3), the temperature of removing nitrate is 80-150°C, and the time of removing nitrate is 1-6 hours. The higher the temperature of removing nitrate is, the shorter the time of removing nitrate is. Preferably, the temperature of removing nitrate is 120-150°C, and the time of removing nitrate is 1-4 hours. More preferably, the temperature of removing nitrate is 130-140°C, and the time of removing nitrate is 2-3 hours.
[0026] In step (4), the platinum tetrachloride solution is concentrated by negative pressure rotary evaporation, the concentration temperature is 30-70° C., and the concentration vacuum is -0.1 MPa.
[0027] In step (4), the platinum tetrachloride crystals are dried in a blast oven at a temperature of 80 to 130° C. for a drying time of 2 to 4 hours.
[0028] The beneficial effects that the present invention can produce include:
[0029] 1) In the present invention, platinum tetrachloride is prepared by a wet precipitation dechlorination method, using Ag + With Cl- The characteristics of the generated precipitation remove the excess Cl- in chloroplatinic acid, making the Cl / Pt molar ratio in the liquid phase system 4, and obtaining EP-grade ultra-pure platinum tetrachloride, which completely avoids the Pt 4+ Reduction leads to the production of byproducts such as PtCl2 and PtCl3. High-purity platinum tetrachloride has high economic value in the fields of platinum plating solution configuration, supported catalysts, and benchmark reagents.
[0030] 2) The method for preparing platinum tetrachloride provided by the present invention does not require high temperature roasting and high pressure reaction, and the production process is simple and the production cost is low. The preparation method of the present invention can solve the problem that the product of the traditional roasting route is uncontrollable and the product purity is low, and the whole process flow is simple. After the AgCl precipitation is roasted, nitric acid can be added to re-make it into a silver nitrate solution for recycling, which has low overall cost, high economy, and is suitable for industrial production.
[0031] 3) The method for preparing platinum tetrachloride provided by the present invention is easy for large-scale industrial continuous automated production, and is easy to accurately control the purity and yield of the product. DETAILED DESCRIPTION
[0032] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0033] If not otherwise specified, the chloroplatinic acid used in the present invention was purchased from Guiyan Platinum Co., Ltd.; silver nitrate and 68% concentrated nitric acid were purchased from China National Pharmaceutical Group Corporation.
[0034] The analysis method in the examples of this application is as follows:
[0035] The impurity elements and platinum content of the product were determined using a NexIon 300Q inductively coupled plasma mass spectrometer (ICP for short) from PE Company of the United States.
[0036] The chlorine and nitrate content of the product was detected using the ELEMENTRAC ONH-P 2 oxygen and nitrogen analyzer and the Dionex ICS3000 ion chromatograph from the German ELTRA company.
[0037] Example 1 Preparation of EP grade extra pure platinum tetrachloride-1
[0038] Preparation of platinum tetrachloride solution: Weigh 100g of chloroplatinic acid to make a solution with a platinum content of 0.2wt%, and weigh 66.18g of silver nitrate to make a solution with a silver content of 0.2wt%. After the chloroplatinic acid solution is heated to 10°C in a water bath, silver nitrate is added dropwise, the stirring speed of the chloroplatinic acid liquid is maintained at 500rmp, and the silver nitrate dropping speed is 1 drop / s. After the silver nitrate is added dropwise, the reaction is continued for 2.5h. Filter to remove the silver chloride, heat the filtrate to 130°C, cover the surface with a watch glass, and remove the nitrate for 3h. After removing the nitrate, transfer the liquid to a rotary evaporator.
[0039] Preparation of platinum tetrachloride solid product: maintain the vacuum degree of rotary evaporation at -0.1MPa and the temperature at 30°C, and concentrate the liquid. When a large amount of platinum tetrachloride crystals appear, continue to concentrate to completely evaporate the water in the rotary evaporation. Remove the platinum tetrachloride crystals from the rotary evaporation and dry them in a blast oven at 80°C for 4 hours to obtain 63.41g of the final platinum tetrachloride solid product.
[0040] The platinum tetrachloride was tested for platinum and impurity content, and the results are shown in the following table.
[0041] Table 1 Platinum tetrachloride product platinum and other impurity content (wt%)
[0042]
[0043] Example 2 Preparation of EP grade extra pure platinum tetrachloride-2
[0044] Preparation of silver nitrate solution: Take 100g of AgCl precipitate, put it in a quartz crucible, heat it to 1000℃ in a muffle furnace and roast it for 2h to obtain silver powder. Take 42.03g of silver powder, add 100g of 68% concentrated nitric acid, and heat until the silver powder is completely dissolved. Add deionized water to make the silver nitrate solution 420.3g to obtain a silver nitrate solution with a silver content of 10wt%.
[0045] Preparation of platinum tetrachloride solution: Weigh 100g of chloroplatinic acid to make a solution with a platinum content of 15wt%. Keep the chloroplatinic acid solution in a water bath at a constant temperature of 50°C and then add silver nitrate. Keep the stirring speed of the chloroplatinic acid liquid at 1000rmp and the silver nitrate dropping speed at 2 drops / s. After the silver nitrate is added, continue the reaction for 0.5h. Filter to remove the silver chloride, heat the filtrate to 150°C, cover the surface with a watch glass, and remove the nitrate for 1h. After removing the nitrate, transfer the liquid to a rotary evaporator.
[0046] Preparation of platinum tetrachloride solid product: maintain the vacuum degree of rotary evaporation at -0.1MPa and the temperature at 70°C, and concentrate the liquid. Continue to concentrate when a large amount of platinum tetrachloride crystals appear, so that the water in the rotary evaporation is completely volatilized. Remove the platinum tetrachloride crystals from the rotary evaporation, place them in a blast oven and dry them at a drying temperature of 130°C for 2 hours to obtain 63.40g of the final platinum tetrachloride solid product.
[0047] The platinum tetrachloride was tested for platinum and impurity content, and the results are shown in the following table.
[0048] Table 2 Platinum tetrachloride product platinum and other impurity content (wt%)
[0049]
[0050]
[0051] Example 3 Preparation of EP grade extra pure platinum tetrachloride-3
[0052] Preparation of platinum tetrachloride solution: Weigh 100g of chloroplatinic acid to make a solution with a platinum content of 0.1wt%, and weigh 66.18g of silver nitrate to make a solution with a silver content of 0.1wt%. Keep the chloroplatinic acid solution in a water bath at a constant temperature of 0°C, then drop silver nitrate, keep the stirring speed of the chloroplatinic acid liquid at 50rmp, and the silver nitrate drop speed at 0.5 drops / s. After the silver nitrate is added, continue the reaction for 5h. Filter to remove the silver chloride, heat the filtrate to 80°C, cover the surface with a watch glass, and remove the nitrate for 6h. After removing the nitrate, transfer the liquid to a rotary evaporator.
[0053] Preparation of platinum tetrachloride solid product: maintain the vacuum degree of rotary evaporation at -0.1MPa and the temperature at 50°C, and concentrate the liquid. Continue to concentrate when a large amount of platinum tetrachloride crystals appear to completely evaporate the water in the rotary evaporation. Remove the platinum tetrachloride crystals from the rotary evaporation and dry them in a blast oven at a drying temperature of 100°C for 3 hours to obtain 63.38g of the final platinum tetrachloride solid product.
[0054] The platinum tetrachloride was tested for platinum and impurity content, and the results are shown in the following table.
[0055] Table 3 Platinum tetrachloride product platinum and other impurity content (wt%)
[0056]
[0057] Example 4 Preparation of EP grade extra pure platinum tetrachloride-4
[0058] Preparation of platinum tetrachloride solution: weigh 100g of chloroplatinic acid to make a solution with a platinum content of 0.5wt%, weigh 66.18g of silver nitrate to make a solution with a silver content of 0.3wt%. After the chloroplatinic acid solution is heated to 20°C in a water bath, silver nitrate is added dropwise, the stirring speed of the chloroplatinic acid liquid is maintained at 500rmp, and the silver nitrate dropping speed is maintained at 0.5 drops / s. After the silver nitrate is added dropwise, the reaction is continued for 2.5h. Filter to remove the silver chloride, heat the filtrate to 130°C, cover the surface with a watch glass, and remove the nitrate for 3h. After removing the nitrate, transfer the liquid to a rotary evaporator.
[0059] Preparation of platinum tetrachloride solid product: maintain the vacuum degree of rotary evaporation at -0.1MPa and the temperature at 30°C, and concentrate the liquid. Continue to concentrate when a large amount of platinum tetrachloride crystals appear, so that the water in the rotary evaporation is completely volatilized. Remove the platinum tetrachloride crystals from the rotary evaporation, place them in a blast oven and dry them at a drying temperature of 80°C for 4 hours to obtain 63.40g of the final platinum tetrachloride solid product.
[0060] The platinum tetrachloride was tested for platinum and impurity content, and the results are shown in the following table.
[0061] Table 4 Platinum tetrachloride product platinum and other impurity content (wt%)
[0062]
[0063] Example 5 Preparation of EP grade extra pure platinum tetrachloride-5
[0064] Preparation of platinum tetrachloride solution: Weigh 100g of chloroplatinic acid to make a solution with a platinum content of 5wt%, and weigh 66.18g of silver nitrate to make a solution with a silver content of 3wt%. Keep the chloroplatinic acid solution in a water bath at a constant temperature of 5°C, then add silver nitrate dropwise, keep the stirring speed of the chloroplatinic acid liquid at 500rmp, and the silver nitrate dropwise addition speed at 1 drop / s. After the silver nitrate is added dropwise, continue the reaction for 3h. Filter to remove the silver chloride, heat the filtrate to 140°C, cover the surface with a watch glass, and remove the nitrate for 2h. After removing the nitrate, transfer the liquid to a rotary evaporator.
[0065] Preparation of platinum tetrachloride solid product: maintain the vacuum degree of rotary evaporation at -0.1MPa and the temperature at 50°C, and concentrate the liquid. Continue to concentrate when a large amount of platinum tetrachloride crystals appear to completely evaporate the water in the rotary evaporation. Remove the platinum tetrachloride crystals from the rotary evaporation and dry them in a blast oven at a drying temperature of 100°C for 3 hours to obtain 63.39g of the final platinum tetrachloride solid product.
[0066] The platinum tetrachloride was tested for platinum and impurity content, and the results are shown in the following table.
[0067] Table 5 Platinum tetrachloride product platinum and other impurity content (wt%)
[0068]
[0069] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing EP grade extra pure platinum tetrachloride, characterized in that: The following steps are involved: Step (1): using chloroplatinic acid as a raw material, adding water to prepare a chloroplatinic acid solution of a specific concentration; Step (2): The chloroplatinic acid solution is kept at a constant temperature, the chloroplatinic acid solution is kept in a stirring state, and a silver nitrate solution of a certain stoichiometric ratio is slowly added dropwise to the chloroplatinic acid solution. The reaction formula of chloroplatinic acid and silver nitrate is as follows: H2PtCl6+2AgNO3→PtCl4+2HNO3+2AgCl↓ (1) Step (3): filtering the liquid after the reaction in step (2) is completed, and then removing the nitrate to obtain a platinum tetrachloride aqueous solution, wherein the reaction formula for removing the nitrate is as follows: 4HNO3→4NO2↑+O2↑+2H2O (2) Step (4): Concentrate and crystallize the platinum tetrachloride aqueous solution in step (3) to obtain platinum tetrachloride crystals, and finally dry the platinum tetrachloride crystals in an oven to obtain an EP grade ultra-pure platinum tetrachloride product.
2. The method for preparing EP-grade ultra-pure platinum tetrachloride according to claim 1, characterized in that: In step (1), the platinum content of the chloroplatinic acid is 38wt%, and the platinum content of the prepared chloroplatinic acid solution is 0.1wt% to 15wt%.
3. The method for preparing EP-grade ultra-pure platinum tetrachloride according to claim 1, characterized in that: In step (2), the constant temperature of the chloroplatinic acid solution is 0-50° C., the constant temperature of the chloroplatinic acid solution is the reaction temperature, the stirring speed is 50-1000 rpm, the silver nitrate dropping speed is 0.5-2 drops / s, and the reaction is continued for 0.5-5 hours after the dropping is completed.
4. The method for preparing EP-grade ultra-pure platinum tetrachloride according to claim 1, characterized in that: In step (2), the silver content of the silver nitrate solution is 0.1 to 10 wt %.
5. The method for preparing EP grade extra pure platinum tetrachloride according to claim 1, characterized in that: In step (3), the temperature of removing the nitrate is 80 to 150° C., and the time of removing the nitrate is 1 to 6 hours.
6. The method for preparing EP grade extra pure platinum tetrachloride according to claim 1, characterized in that: In step (4), the concentration method is rotary evaporation concentration, the concentration temperature is 30-70° C., and the concentration vacuum degree is -0.1 MPa.
7. The method for preparing EP grade extra pure platinum tetrachloride according to claim 1, characterized in that: In step (4), the oven drying temperature is 80 to 130° C., and the drying time is 2 to 4 hours.
8. The method for preparing EP grade extra pure platinum tetrachloride according to claim 1, characterized in that: In step (2), the molar amount of the silver nitrate added dropwise is twice the molar amount of chloroplatinic acid.