Method for producing polyaluminum ferric sulfate water purifying agent by using red gypsum

Through the mixing and oxidation treatment of red gypsum and activated clay wastewater, a polymerized aluminum ferric sulfate water purifier is prepared, which solves the pollution problem of activated clay production wastewater and gypsum slag, achieves efficient sewage treatment and resource recovery, and reduces environmental impact and production cost.

CN118745033APending Publication Date: 2024-10-08GUANGXI LONGAN RUIFENG IND TRADING CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410827888.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The high-concentration sulfuric acid wastewater and by-product gypsum residue generated during the production of activated clay cause environmental pollution, and resource and high-value utilization are insufficient. New ways need to be developed to reduce production costs and environmental impact.

Method used

Red gypsum and activated clay production wastewater are used to stir and mix. By adjusting the pH value and oxidation treatment, a polymeric aluminum iron sulfate water purifier is prepared. The modified material is used for microwave modification to generate an efficient water purifier to treat sewage.

Benefits of technology

It significantly improves sewage turbidity and COD removal rate, achieves rapid generation of large flocs, reduces environmental pollution, improves resource recycling value and production efficiency, and complies with national emission standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745033A_ABST
    Figure CN118745033A_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing a polyaluminum ferric sulfate water purifying agent by using red gypsum, which comprises the following steps: (1) stirring and mixing the red gypsum and activated clay production wastewater, adjusting the pH value of the mixed solution, and carrying out filter pressing treatment to obtain primary filtrate; (2) stirring and mixing the primary filtrate and red gypsum for the second time, adjusting the pH value of the mixed solution, adjusting the composition of ferric oxide, aluminum oxide and sulfur trioxide in the liquid, and then carrying out filter pressing treatment to obtain a secondary filtrate; (3) carrying out oxidation treatment on the secondary filtrate to prepare liquid polyaluminum ferric sulfate; and (4) adding a modification material into the liquid polyaluminum ferric sulfate for modification treatment to prepare the polyaluminum ferric sulfate water purifying agent. The polyaluminum ferric sulfate water purifier product produced by the invention is a chemical product with high economic value, realizes recycling of resources, effective emission reduction in production and reduction of the influence on the environment, is low in production cost and short in period, improves the comprehensive economic benefits of enterprises, and promotes the development of circular economy.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the field of wastewater treatment produced by activated clay and preparation of a water purifier, and in particular to a method for producing a polyaluminium ferric sulfate water purifier by using red gypsum. [Background technology]

[0002] Activated clay is mainly used for decolorization and refining of mineral oil, vegetable oil and animal fat. It is an important raw material for petrochemical and daily chemical industry. Activated clay is made of bentonite as raw material, and is mainly processed by wet acidification process. Its production process includes: bentonite hydration, sulfuric acid activation, water washing, drying and crushing. Because the product contains a large amount of acid, it needs to be repeatedly washed to reduce the acid content to less than 0.2% to meet the requirements of HG / T2569-2007 product standard. Depending on the method, the amount of wastewater generated in the washing process varies, but the amount of wastewater generated by producing 1t of activated clay is generally not less than 30-40t. The wastewater mainly contains aluminum sulfate and unreacted sulfuric acid produced by the bentonite acidification reaction. If it is discharged directly, it will not only waste a lot of resources, but also cause serious pollution to the environment.

[0003] In industry, activated clay by-product gypsum slag is a by-product of lime and wastewater produced after the production of activated clay. Usually, about 1.6 tons of gypsum slag will be produced for every ton of activated clay produced. The output of activated clay by-product gypsum slag is large, and its surface is acidic, which is easy to pollute the environment. Therefore, it is imperative to accelerate its resource utilization and high-value utilization. Industrial by-product gypsum slag is mostly used in construction production, such as cement retarders, fillers, etc., and a small part is used in agricultural production and other fields. Among them, activated clay by-product gypsum slag is mainly used for brick making and storage. There are many shortcomings such as low resource utilization and high environmental pollution. It is urgent to develop new ways of high-value utilization. At present, there are few reports on the resource utilization and high-value utilization of activated clay by-product gypsum slag.

[0004] Using activated clay to produce wastewater containing high-concentration sulfuric acid to dissolve iron and aluminum in gypsum, and using the effective ingredients to prepare polyaluminum sulfate iron water purifier for sewage treatment will greatly reduce production costs, and can also effectively treat activated clay production wastewater, achieve effective production emission reductions, reduce impacts on the environment, and promote the development of a circular economy. [Summary of the invention]

[0005] The present invention provides a method for producing polyaluminium ferric sulfate water purifier by using red gypsum, so as to solve the practical technical problem of how to use activated clay to produce wastewater containing high-concentration sulfuric acid to dissolve iron and aluminium in gypsum, and to optimize the process for preparing the water purifier, so as to significantly improve the wastewater turbidity removal rate and COD removal rate.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0008] (1) mixing red gypsum and activated clay production wastewater for the first time, adjusting the pH value of the mixed solution, and performing filter press treatment to obtain a primary filtrate;

[0009] (2) stirring and mixing the primary filtrate obtained in step (1) with the newly added red gypsum for a second time, adjusting the pH of the mixed solution, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing a filter press treatment to obtain a secondary filtrate;

[0010] (3) subjecting the secondary filtrate obtained in step (2) to oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0011] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), and then performing a modification treatment under controlled microwave power, temperature, rotation speed and stirring time to obtain a polyaluminum ferric sulfate water purifier.

[0012] Preferably, the first stirring and mixing in step (1) is carried out at room temperature.

[0013] Preferably, the pH in step (1) is 1.0-1.5.

[0014] Preferably, the second stirring and mixing in step (1) is carried out at room temperature.

[0015] Preferably, the pH in step (2) is 2.0-2.5.

[0016] Preferably, in step (3), the secondary filtrate is oxidized by using oxygen or hydrogen peroxide.

[0017] Preferably, the microwave power in step (4) is 100-300W.

[0018] Preferably, the temperature in step (4) is 40-50°C.

[0019] Preferably, the rotation speed in step (4) is 200-400 r / min.

[0020] Preferably, the stirring time in step (4) is 30-60 min.

[0021] Compared with the prior art, the present invention has the following technical advantages:

[0022] (1) A large amount of red gypsum by-product is generated during the production process of activated clay. The present invention adopts an acid leaching method to further extract the effective components aluminum and iron from the red gypsum component, and studies the production and application of using the activated clay by-product solid red gypsum to produce a water purifier. In the process of producing polyaluminum ferric sulfate from red gypsum, the reaction pH value, polymerization degree, main component content, modified material ratio, etc. are controlled to finally produce a polyaluminum ferric sulfate water purifier. The water purifier is used to treat sewage, and the sewage turbidity removal rate reaches more than 93.2% and the COD removal rate reaches more than 96.1%. Large floccules are generated within 2.5 minutes. This shows that the use of the water purifier of the present invention to treat sewage has good effects such as rapid generation of large floccules, low turbidity of the supernatant after flocculation, and high sewage COD removal rate (in line with the national discharge standard of more than 93%).

[0023] (2) The physical and chemical indicators of the polyaluminum ferric sulfate water purifier product produced by the present invention are as follows: ① the mass fraction of aluminum oxide ≥ 8.0%, ② the mass fraction of total iron ≥ 1.5%, ③ the mass fraction of ferrous iron ≤ 0.2%. The product is a chemical product with high economic value, realizes the recycling of resources, effectively reduces wastewater discharge by more than 10%, reduces the impact on the environment, has low production cost, short cycle, is easy to operate production activities, can achieve new production goals, improve the comprehensive economic benefits of enterprises, and promote the development of circular economy.

Brief Description of the Drawings

[0024] Figure 1 This is a picture of the gypsum products produced by the applicant itself.

[0025] Figure 2 The comparison diagram is before and after flocculation of turbid sewage in a river in Nanning City treated with the polyaluminium ferric sulfate water purifier produced in Example 3, wherein the left picture is a picture before treatment, and the right picture is a picture after treatment. [Specific implementation method]

[0026] In order to facilitate a better understanding of the present invention, the following examples are used to illustrate the present invention. These examples belong to the protection scope of the present invention, but do not limit the protection scope of the present invention.

[0027] The red gypsum with high aluminum and iron content used in the embodiments and comparative examples of the present invention is gypsum produced by the applicant himself, see Figure 1 The production process can be seen in Example 1 of the invention previously applied by the applicant, "A method for producing mother liquor and co-producing alum and gypsum using activated white clay (publication number: CN105293797A)". The gypsum was dried, ground and sieved, and then chemically analyzed using an X-ray fluorescence spectrometer. Its main chemical composition is as follows: SO3 is 35.23%, CaO is 32.18%, Al2O3 is 9.47%, Fe2O3 is 7.05%, MgO is 2.69%, and SiO2 is 0.91%.

[0028] In an embodiment of the present invention, a method for producing a polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0029] (1) mixing red gypsum with high aluminum and iron content with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH of the mixed solution to 1.0-1.5, and performing filter press treatment to obtain a primary filtrate;

[0030] (2) mixing the primary filtrate obtained in step (1) with the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH of the mixed solution to 2.0-2.5, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0031] (3) subjecting the secondary filtrate obtained in step (2) to oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0032] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is (100-200):(6.2-12.3):(4.1-7.4):(1.5-3.6), and then stirring for 30-60 min at a microwave power of 100-300 W, a temperature of 40-50° C., and a rotation speed of 200-400 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0033] In order to make the disclosure of the present invention more complete, the present invention is described below through more specific embodiments.

[0034] Example 1

[0035] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0036] (1) mixing red gypsum with high aluminum and iron contents with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.1, and performing filter press treatment to obtain a primary filtrate;

[0037] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.4, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0038] (3) subjecting the secondary filtrate obtained in step (2) to oxygen oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0039] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 103:6.4:4.5:1.6, and then stirring for 60 minutes at a microwave power of 100 W, a temperature of 40° C., and a rotation speed of 200 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0040] Example 2

[0041] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0042] (1) mixing red gypsum with high aluminum and iron content with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.0, and performing filter press treatment to obtain a primary filtrate;

[0043] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.2, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0044] (3) subjecting the secondary filtrate obtained in step (2) to an oxidation treatment with hydrogen peroxide to obtain liquid polyaluminum ferric sulfate;

[0045] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 120:7:4.8:2, and then stirring for 50 minutes at a microwave power of 160 W, a temperature of 42° C., and a rotation speed of 250 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0046] Example 3

[0047] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0048] (1) mixing red gypsum with high aluminum and iron content with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.3, and performing filter press treatment to obtain a primary filtrate;

[0049] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.3, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0050] (3) subjecting the secondary filtrate obtained in step (2) to oxygen oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0051] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 152:9.5:6:2.4, and then stirring for 46 minutes at a microwave power of 200 W, a temperature of 46° C., and a rotation speed of 30 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0052] Example 4

[0053] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0054] (1) mixing red gypsum with high aluminum and iron contents with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.2, and performing filter press treatment to obtain a primary filtrate;

[0055] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.1, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0056] (3) subjecting the secondary filtrate obtained in step (2) to an oxidation treatment with hydrogen peroxide to obtain liquid polyaluminum ferric sulfate;

[0057] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 163:10.1:6.3:2.8, and then stirring for 48 minutes at a microwave power of 200 W, a temperature of 43° C., and a rotation speed of 260 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0058] Example 5

[0059] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0060] (1) mixing red gypsum with high aluminum and iron contents with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.5, and performing filter press treatment to obtain a primary filtrate;

[0061] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.3, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0062] (3) subjecting the secondary filtrate obtained in step (2) to oxygen oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0063] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 185:10.2:6.4:3.1, and then stirring for 40 minutes at a microwave power of 250 W, a temperature of 43° C., and a rotation speed of 300 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0064] Example 6

[0065] A method for producing polyaluminium ferric sulfate water purifier using red gypsum comprises the following steps:

[0066] (1) mixing red gypsum with high aluminum and iron contents with activated clay production wastewater for the first time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 1.4, and performing filter press treatment to obtain a primary filtrate;

[0067] (2) stirring and mixing the primary filtrate obtained in step (1) and the newly added red gypsum for a second time, adjusting the acidity of the mixed solution to adjust the pH value of the mixed solution to 2.4, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing filter press treatment to obtain a secondary filtrate;

[0068] (3) subjecting the secondary filtrate obtained in step (2) to oxygen oxidation treatment to obtain liquid polyaluminum ferric sulfate;

[0069] (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), wherein the modified material consists of citric acid, L-arabinose, and palmitoyl tetrapeptide, and the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide is 196:11.8:7.2:3.5, and then stirring for 30 minutes at a microwave power of 300 W, a temperature of 50° C., and a rotation speed of 400 r / min to obtain a polyaluminum ferric sulfate water purifier.

[0070] Comparative Example 1

[0071] The method for preparing the water purifier is the same as that in Example 3, except that the obtained liquid polyaluminum ferric sulfate is not subjected to the treatment of step (4), that is, the raw materials for preparing the water purifier lack citric acid, L-arabinose, and palmitoyl tetrapeptide, and the missing mass is supplemented with purified water to maintain the total mass unchanged.

[0072] Comparative Example 2

[0073] The method for preparing the water purifier is the same as that in Comparative Example 1, except that more citric acid is added to the raw materials for preparing the water purifier, and the missing mass is supplemented with pure water to maintain the total mass unchanged.

[0074] Comparative Example 3

[0075] The method for preparing the water purifier is the same as that in Comparative Example 1, except that more L-arabinose is added to the raw materials for preparing the water purifier, and the missing mass is supplemented with pure water to maintain the total mass unchanged.

[0076] Comparative Example 4

[0077] The method for preparing the water purifier is the same as that in Comparative Example 1, except that more palmitoyl tetrapeptide is added to the raw materials for preparing the water purifier, and the missing mass is supplemented with purified water to maintain the total mass unchanged.

[0078] Comparative Example 5

[0079] The method for preparing the water purifier is the same as that in Example 3, except that the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide in the raw materials for preparing the water purifier is 230:15:2:1.

[0080] Comparative Example 6

[0081] The method for preparing the water purifier is the same as that in Example 3, except that the mass ratio of the liquid polyaluminum ferric sulfate, citric acid, L-arabinose, and palmitoyl tetrapeptide in the raw materials for preparing the water purifier is 50:5:10:7.

[0082] Comparative Example 7

[0083] The polyaluminum sulfate ferric water purifier was prepared by the process of Example 1 in the Chinese patent document "A method for producing polyaluminum sulfate ferric water purifier and silica gel using iron tailings (patent number: ZL201911285365.2)".

[0084] Turbid sewage (slightly odorous, water temperature 26°C) from a river in Nanning was used for flocculation test. The water purifiers in Examples 1-6 and Comparative Examples 1-7 were used for flocculation, and the flocculation phenomenon was observed. The turbidity of the turbid sewage before and after flocculation and the COD removal rate of the sewage were measured. The test results are shown in the table below, where the turbidity was measured using an XZ-0101B turbidity detector, and the COD determination method is as follows:

[0085] (1) Take 20.00 mL of sewage and place it in a 250 mL ground-mouth reflux conical flask. Add 10.00 mL of potassium dichromate standard solution and several small zeolites accurately. Shake the conical flask to mix the solution. Heat and reflux for 2 hours (starting from the beginning of boiling).

[0086] (2) After cooling, rinse the condenser tube wall with 90 mL of water and remove the conical flask. The total volume of the solution must not be less than 140 mL, otherwise the titration endpoint will not be obvious due to the high acidity.

[0087] (3) After the solution is cooled again, add 3 drops of ferrocyanine indicator solution and titrate with ammonium ferrous sulfate standard solution. The end point is when the color of the solution changes from yellow to blue-green to reddish brown. Record the amount of ammonium ferrous sulfate standard solution used.

[0088] (4) While measuring the wastewater, take 20.00 mL of double distilled water and perform a blank test according to the same operating steps. Record the amount of ammonium ferrous sulfate standard solution used in the blank titration.

[0089] (5) Calculation

[0090] CODCr(O2, mg / L)=(V0-V1)×C×8×1000 / V

[0091] Where: C——concentration of ammonium ferrous sulfate standard solution, mol / L;

[0092] V0——the amount of ammonium ferrous sulfate standard solution used in the blank titration, ml;

[0093] V1——the amount of ammonium ferrous sulfate standard solution used in the titration of sewage, ml;

[0094] V——volume of sewage, ml;

[0095] 8——Molar mass of oxygen (1 / 2O), g / mol.

[0096]

[0097]

[0098] It can be seen from the above table that: (1) From the data of Examples 1-6, it can be seen that when the water purifier of Examples 1-6 is used to treat sewage, the sewage turbidity removal rate reaches more than 93.2% and the COD removal rate reaches more than 96.1%, and large floccules are generated within 2.5 minutes, indicating that the use of the water purifier of the present invention to treat sewage has good effects such as rapid generation of large floccules, low turbidity of the supernatant after flocculation, and high sewage COD removal rate (in line with the national discharge standard of more than 93%). Among them, Example 3 is the best example. The comparison diagram before and after flocculation of turbid sewage in a river in Nanning City treated with the water purifier of this example is shown in Figure 2 It can be seen that after being treated with the water purifier of the present invention, the sewage becomes clear and flocculation is significant.

[0099] (2) From the sewage turbidity removal rate and COD removal rate data of Example 3 and Comparative Examples 1-4, it can be calculated that the sewage turbidity removal rate effect value generated when polyaluminum ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide are used together is 27.5% higher than the effect value of the sewage turbidity removal rate generated by the superposition of polyaluminum ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide when used separately, which is greater than 10%; it can also be calculated that the COD removal rate effect value generated when polyaluminum ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide are used together is 35.0% higher than the effect value of the COD removal rate generated by the superposition of polyaluminum ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide when used separately, which is greater than 10%. It can be seen that polyaluminum ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide play a synergistic role in the preparation of water purifiers, and synergistically improve the sewage turbidity removal rate and COD removal rate, because:

[0100] As a highly efficient flocculant, polyaluminium ferric sulfate can quickly react with suspended particles and colloidal substances in sewage to form larger floccules. Its unique polymer structure gives it a higher charge density and adsorption capacity in water, and can significantly and effectively remove turbidity substances in sewage, not only improving the sewage turbidity removal rate, but also improving the COD removal rate.

[0101] As an organic acid, citric acid plays an important synergistic role in sewage treatment. On the one hand, citric acid can react with metal ions in sewage to reduce the impact of metal ions on the flocculation effect of polyaluminum ferric sulfate; on the other hand, citric acid can also adjust the pH value of sewage, creating more favorable environmental conditions for the flocculation of polyaluminum ferric sulfate, and further promote the improvement of sewage turbidity removal rate and COD removal rate. In addition, citric acid combines with the hydroxyl group of L-arabinose through hydrogen bonding, thereby improving the dispersibility of L-arabinose and enhancing the flocculation effect.

[0102] As a natural polysaccharide, L-arabinose has a highly branched structure that can chelate dissolved organic matter in sewage with hydrogen bonds and has a good adsorption effect, thus having a good coagulant effect in sewage treatment. It can interact with organic matter in sewage, promote the decomposition and transformation of organic matter in sewage, and improve the removal rate of COD. In addition, it can also enhance the adsorption capacity of polyaluminium ferric sulfate, further improve the flocculation effect, and increase the removal rate of sewage turbidity and COD.

[0103] As a bioactive peptide, palmitoyl tetrapeptide plays a reinforcing role in sewage treatment. It can form a stable complex with organic matter in sewage and improve the removal rate of COD. Palmitoyl tetrapeptide forms a complex with L-arabinose, which promotes the flocculation effect. In addition, palmitoyl tetrapeptide also has certain biological activity, which can promote the degradation of organic matter by microorganisms and further improve the removal rate of sewage turbidity.

[0104] The present invention synergistically improves the sewage turbidity removal rate and COD removal rate through an innovative design of a combination of polyaluminium ferric sulfate, citric acid, L-arabinose and palmitoyl tetrapeptide.

[0105] (3) It can be seen from the data of Comparative Examples 5 and 6 that when the mass ratio of the liquid polyaluminum sulfate ferric, citric acid, L-arabinose, and palmitoyl tetrapeptide is not within the range of (100-200):(6.2-12.3):(4.1-7.4):(1.5-3.6), the sewage turbidity removal rate and COD removal rate obtained by the prepared water purifier are significantly different from the sewage turbidity removal rate and COD removal rate obtained by the water purifier prepared in Example 3, which further illustrates that the process of the present invention needs to strictly control the mass ratio of polyaluminum sulfate ferric, citric acid, L-arabinose and palmitoyl tetrapeptide, so that polyaluminum sulfate ferric, citric acid, L-arabinose and palmitoyl tetrapeptide can better synergistically improve the sewage turbidity removal rate and COD removal rate.

[0106] (4) It can be seen from the phenomena and data of Examples 1-6 and Comparative Example 7 (prior art) that the flocculation rate of the water purifier prepared in Examples 1-6 is comparable to that of the water purifier prepared in Comparative Example 7, the sewage turbidity removal rate of the water purifier prepared in Examples 1-6 is 4.5%-8.5% higher than that of the water purifier prepared in Comparative Example 7, and the COD removal rate of the water purifier prepared in Examples 1-6 is 1.4%-4.2% higher than that of the water purifier prepared in Comparative Example 7. In addition, the process for preparing the water purifier of the present invention is simpler than that of the water purifier prepared in Comparative Example 7, is easier to operate, and has a lower preparation cost. It can be seen that the technology of the present invention is significantly improved over the prior art.

[0107] The above content cannot be used to determine that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, they can make several simple deductions or substitutions without departing from the concept of the present invention, which should be regarded as belonging to the scope of patent protection of the present invention determined by the submitted claims.

Claims

1. A method for producing polyaluminium ferric sulfate water purifier using red gypsum, characterized in that: The following steps are involved: (1) mixing red gypsum and activated clay production wastewater for the first time, adjusting the pH value of the mixed solution, and performing filter press treatment to obtain a primary filtrate; (2) stirring and mixing the primary filtrate obtained in step (1) with the newly added red gypsum for a second time, adjusting the pH of the mixed solution, adjusting the composition of iron oxide, aluminum oxide, and sulfur trioxide in the liquid, and then performing a filter press treatment to obtain a secondary filtrate; (3) subjecting the secondary filtrate obtained in step (2) to oxidation treatment to obtain liquid polyaluminum ferric sulfate; (4) adding a modified material to the liquid polyaluminum ferric sulfate obtained in step (3), and then performing a modification treatment under controlled microwave power, temperature, rotation speed and stirring time to obtain a polyaluminum ferric sulfate water purifier.

2. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The first stirring and mixing in step (1) is carried out at room temperature.

3. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The pH in step (1) is 1.0-1.

5.

4. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The second stirring and mixing in step (1) is carried out at room temperature.

5. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The pH in step (2) is 2.0-2.

5.

6. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: In step (3), the secondary filtrate is oxidized by using oxygen or hydrogen peroxide.

7. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The microwave power in step (4) is 100-300W.

8. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The temperature in step (4) is 40-50°C.

9. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The rotation speed in step (4) is 200-400r / min.

10. The method for producing polyaluminium ferric sulfate water purifier using red gypsum according to claim 1, characterized in that: The stirring time in step (4) is 30-60 min.

Citation Information

Cited By

  • Liquid polyaluminum ferric sulfate flocculant, preparation process and application of liquid polyaluminum ferric sulfate flocculant in wastewater treatment

    CN120247193A