Preparation method of water-resistant reinforcing agent and phosphogypsum-based artificial aggregate
By using water-resistant enhancers in phosphogypsum-based artificial aggregates, combined with phosphogypsum, slag and cement kiln dust, the problems of phosphogypsum storage and environmental pollution are solved, achieving efficient water resistance and reducing the heavy metal ion leaching rate, meeting the requirements Standards for gravel used in construction.
Patent Information
- Application Number
- CN202410957269.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-08
AI Technical Summary
The accumulation of phosphogypsum causes land occupation, environmental pollution and safety hazards, and its use in the field of building materials is limited by water resistance and leaching toxicity issues.
Design a water-resistant enhancer, including a waterproofing agent, an early strength agent, an active activator, a passivating agent, a thickener and a water-reducing agent, to form an efficient phosphogypsum base by combining with phosphogypsum, slag and cement kiln dust Artificial aggregate, improves its early strength and water resistance, and reduces the leaching rate of heavy metal ions such as fluorine and phosphorus.
It significantly improves the early strength and water resistance of phosphogypsum-based artificial aggregate, reduces the leaching rate of heavy metal ions, meets the standards for construction gravel, and alleviates the environmental pollution and accumulation problems of phosphogypsum.
Smart Images

Figure CN118745092A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phosphogypsum materials, and in particular to a method for preparing a water-resistant enhancer and a phosphogypsum-based artificial aggregate. Background Art
[0002] Phosphogypsum is a solid waste byproduct produced by the action of sulfuric acid on phosphate rock during the wet process of phosphoric acid production. The wet process produces about 5 to 6 tons of phosphogypsum for every ton of phosphoric acid (measured in P2O5). Phosphogypsum is mainly composed of calcium sulfate dihydrate (CaSO4·2H2O), containing about 5-6% of impurities such as phosphorus, fluorine, heavy metals and residual acid, making it difficult to use directly. At present, the global stockpile of phosphogypsum has reached 8 billion tons, and it is still increasing at a rate of 150 million tons per year. China is the world's largest producer of phosphate fertilizers and the largest by-producer of phosphogypsum. The stockpile of phosphogypsum has reached more than 400 million tons, and it is still increasing at a rate of about 50 million tons per year.
[0003] There are three main ways to use phosphogypsum in my country: building materials, chemical products, and soil conditioners. ① Building materials mainly include gypsum building materials, cement retarders, etc., but there are problems such as small dosage, unstable quality, and low user acceptance in the use of these products; ② Chemical products mainly include sulfuric acid co-production of cement, ammonium sulfate co-production of calcium carbonate, etc., but there are problems such as large investment, many problems after installation, high cost, and difficult clinker processing; ③ Soil conditioners mainly use the acidic phosphorus and fluorine in phosphogypsum to adjust the acidity of the soil and improve soil quality, but given the characteristics of my country's soil being acidic in the south and alkaline in the north, and phosphogypsum being mainly concentrated in the south of the Yangtze River, there are problems such as a small scope of use of phosphogypsum as a soil conditioner.
[0004] Therefore, at present, most phosphogypsum is still disposed of in the form of slag dumps. The storage of huge amounts of phosphogypsum has the following problems: first, it occupies a large amount of arable land; second, dry-stacked phosphogypsum is in powder form, which is prone to form dust after long-term exposure to the sun, affecting the atmospheric environment; third, the stacked phosphogypsum becomes a fluid object after being drenched by rain, and various harmful impurities such as water-soluble P2O5 and F salts are easy to flow out or overflow and enter surface water, groundwater or soil, causing irreversible water, soil and plant pollution; fourth, the long-term storage of phosphogypsum will also bring safety hazards such as dam breach. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention proposes a method for preparing a water-resistant enhancer and a phosphogypsum-based artificial aggregate, so that after adding the water-resistant enhancer, the early strength of the phosphogypsum-based artificial aggregate is greatly improved, the water resistance is significantly improved, the leaching rate of heavy metal ions such as fluorine and phosphorus is greatly reduced, the softening coefficient is as high as 0.85, and the water absorption rate of the aggregate is reduced by 25-30% compared with that without adding the water-resistant enhancer, meeting the standards for crushed stone for construction, and can be widely used in C30-C60 grade concrete and highway roadbed materials.
[0006] To achieve the above purpose, the present invention is designed to provide a water resistance enhancer, which is special in that, based on 100 parts by weight of the total weight of the water resistance enhancer, the water resistance enhancer includes the following components: 60-70 parts by weight of a waterproofing agent, 3-5 parts by weight of an early strength agent, 10-20 parts by weight of an active stimulant, 10-15 parts by weight of a passivator, 2-5 parts by weight of a thickener, and 0.1-20 parts by weight of a water reducer.
[0007] Furthermore, the waterproofing agent is composited by one or more of 1%-5% by weight of sodium metasilicate pentahydrate, 5%-10% by weight of nano silicon dioxide, 30%-40% by weight of polyaluminium chloride, 20%-30% by weight of polyaluminium ferric chloride, 1%-5% by weight of potassium trimethylsilanol, 10%-20% by weight of methyl aluminium silicate, 1%-5% by weight of polyacrylate and 5%-10% by weight of silicone.
[0008] Furthermore, the early strength agent is composed of one or more of 20%-30% by weight of Glauber's salt, 30%-40% by weight of Sodium Sulfate, 1%-2% by weight of Trihydroxyethanolamine, and 10%-30% by weight of Sodium Thiosulfonate.
[0009] Furthermore, the active activator is composited by one or more of 40%-60% by weight of slag, 10%-30% by weight of silica fume, and 20%-30% by weight of cement.
[0010] Furthermore, the passivator is composited by one or more of 10%-20% by weight of petroleum coke desulfurization ash, 20%-40% by weight of carbide slag, 20%-30% by weight of calcium formate, 20%-30% by weight of sodium lignosulfonate, 20%-30% by weight of diatomaceous earth, and 5%-10% by weight of polyacrylic acid resin.
[0011] Furthermore, the thickener is composited by one or more of 40%-50% by weight of xanthan gum, 10%-30% by weight of xylitol mother liquor, and 40%-50% by weight of hydroxybutyl methylcellulose.
[0012] Furthermore, the water reducer is compounded by one or more of 1%-10% by weight of sodium humate, 1%-30% by weight of aminosulfonic acid ammonia, 5%-30% by weight of sodium xylene sulfonate, and 40%-50% by weight of naphthalene-based water reducer.
[0013] The present invention also provides a method for preparing phosphogypsum-based artificial aggregate, which is particularly characterized in that the method uses the water-resistant enhancer as described above, and comprises the following steps:
[0014] S1) drying the original phosphogypsum and grinding it to obtain ground phosphogypsum; drying the original slag and grinding it to obtain ground slag powder; calcining cement kiln dust at high temperature, cooling it to room temperature, and then grinding it to obtain ground cement kiln dust;
[0015] S2) setting a feeding angle of the granulator, first adding the ground phosphogypsum into the granulator and rotating it for 5 to 10 seconds, then adding a mixture of ground slag powder and ground cement kiln dust, and a water-resistant enhancer into the granulator for artificial granulation, and adding water during the granulation process to obtain phosphogypsum-based artificial aggregate;
[0016] Based on 100 parts by weight of the dry total weight of the phosphogypsum-based artificial aggregate, the phosphogypsum-based artificial aggregate comprises the following components: 80-85 parts by weight of ground phosphogypsum, 8-12 parts by weight of ground slag powder, 5-9 parts by weight of ground cement kiln dust, and 0.1-5 parts by weight of a water-resistant enhancer;
[0017] The water accounts for 18% to 23% of the total dry weight of the phosphogypsum-based artificial aggregate;
[0018] S3) discharging the phosphogypsum-based artificial aggregate in step S3) and setting a discharging angle of a granulator;
[0019] S4) performing moisture-curing on the unloaded phosphogypsum-based artificial aggregate, and controlling the relative humidity during the curing period.
[0020] Further, in S1), the ground phosphogypsum is prepared by neutralizing the original phosphogypsum with quicklime to a pH value of 7.5-8, standing for 20-24 hours, drying at 50-60° C., and ball milling in a ball mill for 60-80 minutes until the specific surface area is greater than or equal to 450 m 2 / kg of phosphogypsum;
[0021] The ground slag powder is obtained by drying the original slag at 50-60°C, and ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 500m 2 / kg of slag powder;
[0022] The ground cement kiln dust is obtained by calcining the original cement kiln dust at a high temperature of 500-700°C for 1-2 hours, cooling it to room temperature, and then ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 330 m 2 / kg of cement kiln dust.
[0023] Furthermore, in S2), the feeding angle of the granulator is set to 44° to 51°, and the discharging angle of the granulator is set to 68° to 80°.
[0024] The principle that the water-resistant enhancer designed in the present invention can make the phosphogypsum-based artificial aggregate reach the standard of crushed stone for construction is as follows:
[0025] 1. The present invention dries the original phosphogypsum (the main material in the artificial aggregate) and then grinds it. Under the combined action of the physical excitation method of grinding the phosphogypsum in a ball mill and the active activator (including the active activator in the water-resistant enhancer, and the ground slag powder and the ground cement kiln dust in the artificial aggregate), the phosphogypsum volcanic ash activity is fully activated, and the ground phosphogypsum is fully hydrated to generate a large amount of hydrated calcium silicate, hydrated calcium aluminate, and calcium hydroxide;
[0026] 2. The early strength agent in the water-resistant enhancer (compounded by one or more of Glauber's salt, sodium sulfate, trihydroxyethanolamine, and sodium thiosulfonate) increases the alkalinity of the system and increases the early strength of the solid waste group aggregate by promoting the formation of calcium hydroxide, calcium sulfate, calcium carbonate, and calcium aluminate hydrate;
[0027] 3. The waterproofing agent in the water-resistant enhancer (composite of one or more of sodium silicate pentahydrate, nano-silicon dioxide, polyaluminum chloride, polyaluminum chloride iron, potassium trimethylsilanolate, methyl aluminum silicate, polyacrylate, silicone) combines with the hydroxide in the solution to generate a large amount of colloid substances that are difficult to dissolve in water, such as iron hydroxide and aluminum hydroxide colloids, which stimulate the hydrated calcium aluminate produced by the phosphogypsum to further react and generate calcium sulfoaluminate crystals with certain expansion. These colloids and crystals fill the capillaries formed in the aggregate during the hardening process, improve the density of the aggregate, and thus improve the waterproof effect; at the same time, the hydrolysis of silicone forms water-soluble silanol, which reacts with polyacrylate and forms a layer of mesh-like hydrophobic siloxane film that is not easy to penetrate water on the surface of the phosphogypsum aggregate, thereby improving the waterproof effect;
[0028] 4. The theoretical water-to-paste ratio of phosphogypsum is only about 18%, but in actual production, due to the requirement of fluidity, the actual water consumption often reaches 60% to 80%. The excess water overflows or evaporates from the slurry during the hardening process of phosphogypsum, leaving a large number of micropores and cracks inside the hardened body. The water reducing agent in the water-resistant enhancer (compounded by one or more of sodium humate, aminosulfonic acid, sodium xylene sulfonate, and naphthalene-based water reducing agent) can reduce the water consumption and increase the strength. At the same time, the higher strength can effectively prevent cracks and help improve the long-term effectiveness of the waterproof effect.
[0029] 5. The thickener in the water-resistant enhancer (composite of one or more of xanthan gum, xylitol mother liquor, and hydroxybutyl methylcellulose) has gelling properties, which can bind the phosphogypsum particles together and fill the gaps between the phosphogypsum particles, thereby reducing the porosity and increasing the strength. However, it is easily eroded by water. At this time, the methyl aluminum silicate in the waterproofing agent reacts with carbon dioxide and water to form a hydrophobic film on the surface of the xanthan gum, which reduces the erosion by water and increases the strength of the aggregate.
[0030] 6. The passivator in the water-resistant enhancer (composite of one or more of petroleum coke desulfurization ash, carbide slag, calcium formate, sodium lignosulfonate, diatomaceous earth, and polyacrylic resin) can provide calcium ions, which react with soluble phosphorus and fluorine in phosphogypsum to generate calcium phosphate and calcium fluoride precipitates, thereby reducing the phosphorus and fluorine content in phosphogypsum.
[0031] The advantages of the present invention are:
[0032] 1. The water-resistant enhancer of the present invention is added to the phosphogypsum aggregate, and the components work synergistically to improve the compressive strength and water resistance of the phosphogypsum aggregate, and reduce the leaching toxicity, thereby improving the performance of the phosphogypsum aggregate and reducing its pollution to the environment;
[0033] 2. The phosphogypsum-based artificial aggregate in the present invention is prepared by directly mixing a variety of powder ingredients, with a simple production process, low cost, and easy packaging and transportation;
[0034] 3. The phosphogypsum content in the phosphogypsum-based artificial aggregate of the present invention is large and has a high utilization rate, which can effectively alleviate the problem of large-scale accumulation of phosphogypsum.
[0035] The water-resistant enhancer and the preparation method of the phosphogypsum-based artificial aggregate of the present invention enable the phosphogypsum-based artificial aggregate to have greatly improved early strength and significantly improved water resistance after adding the water-resistant enhancer, and to have greatly reduced leaching rates of heavy metal ions such as fluorine and phosphorus, thereby meeting the standards for crushed stone for construction, and can be widely used in C30-C60 grade concrete and highway subgrade materials, effectively alleviating the environmental pollution and large-scale accumulation problems of phosphogypsum. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1This is a schematic diagram of the phosphogypsum-based artificial aggregate prepared by the present invention. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0038] Although phosphogypsum has strong volcanic ash activity, its activity needs to be fully stimulated. The present invention greatly improves the water resistance of the aggregate by adding a water-resistant enhancer to the phosphogypsum-based artificial aggregate.
[0039] The water resistance enhancer comprises the following components based on 100 parts by weight of the total weight of the water resistance enhancer: 60-70 parts by weight of a waterproofing agent, 3-5 parts by weight of an early strength agent, 10-20 parts by weight of an active stimulant, 10-15 parts by weight of a passivator, 2-5 parts by weight of a thickener, and 0.1-20 parts by weight of a water reducer.
[0040] Preferably, the waterproofing agent is 65-70 parts by weight, the early strength agent is 3-5 parts by weight, the active stimulant is 15-20 parts by weight, the passivator is 10-15 parts by weight, the thickener is 3-5 parts by weight, and the water reducing agent is 0.1-15 parts by weight.
[0041] Specifically, the waterproofing agent is composed of one or more of 1%-5% by weight of sodium metasilicate pentahydrate, 5%-10% by weight of nano silicon dioxide, 30%-40% by weight of polyaluminium chloride, 20%-30% by weight of polyaluminium ferric chloride, 1%-5% by weight of potassium trimethylsilanol, 10%-20% by weight of methyl aluminium silicate, 1%-5% by weight of polyacrylate and 5%-10% by weight of silicone.
[0042] Specifically, the early strength agent is composed of one or more of 20%-30% by weight of Glauber's salt, 30%-40% by weight of Sodium Sulfate, 1%-2% by weight of Trihydroxyethanolamine, and 10%-30% by weight of Sodium Thiosulfonate.
[0043] Specifically, the active activator is composited from one or more of 40%-60% by weight of slag, 10%-30% by weight of silica fume, and 20%-30% by weight of cement.
[0044] Specifically, the passivator is composited by one or more of 10%-20% by weight of petroleum coke desulfurization ash, 20%-40% by weight of carbide slag, 20%-30% by weight of calcium formate, 20%-30% by weight of sodium lignosulfonate, 20%-30% by weight of diatomaceous earth, and 5%-10% by weight of polyacrylic acid resin.
[0045] Specifically, the thickener is composited from one or more of 40%-50% by weight of xanthan gum, 10%-30% by weight of xylitol mother liquor, and 40%-50% by weight of hydroxybutyl methylcellulose.
[0046] Specifically, the water reducer is compounded by one or more of 1%-10% by weight of sodium humate, 1%-30% by weight of aminosulfonic acid ammonia, 5%-30% by weight of sodium xylene sulfonate, and 40%-50% by weight of naphthalene-based water reducer.
[0047] The present invention also provides a method for preparing phosphogypsum-based artificial aggregate, using the above-mentioned water-resistant enhancer, comprising the following steps:
[0048] S1) drying the original phosphogypsum and then grinding it to obtain ground phosphogypsum; drying the original slag and then grinding it to obtain ground slag powder; calcining cement kiln dust at high temperature, cooling it to room temperature, and then grinding it to obtain ground cement kiln dust.
[0049] The original phosphogypsum used in this embodiment was taken from the phosphogypsum yard, and its appearance was gray and fine powder. The slag had a white and fine powder appearance. The cement was ordinary Portland cement (model P·O42.5). The chemical composition of the main raw materials of the phosphogypsum-based artificial aggregate was as shown in the following table.
[0050] Table 1 Chemical composition of main raw materials of phosphogypsum-based artificial aggregate (wt / %)
[0051]
[0052] Phosphogypsum is a solid waste in the phosphoric acid production process. Its main component is calcium sulfate dihydrate. Traditional phosphogypsum aggregate has poor water resistance and slow setting. After being soaked in water, the internal structure is destroyed, the strength is greatly reduced, and the leaching rate of heavy metal ions such as fluorine and phosphorus in the phosphogypsum is increased. This makes it difficult to use phosphogypsum in large quantities in the building materials field.
[0053] Specifically, the ground phosphogypsum is prepared by neutralizing the original phosphogypsum with quicklime to a pH value of 7.5-8, standing for 20-24 hours, drying at 50-60° C., and ball milling in a ball mill for 60-80 minutes until the specific surface area is greater than or equal to 450 m 2 / kg of phosphogypsum.
[0054] The ground slag powder is obtained by drying the original slag at 50-60°C, and ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 500m 2 / kg of slag powder.
[0055] The ground cement kiln dust is obtained by calcining the original cement kiln dust at a high temperature of 500-700°C for 1-2 hours, cooling it to room temperature, and then ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 330 m 2 / kg of cement kiln dust.
[0056] In addition, the moisture content, fluorine content and phosphorus content of the original phosphogypsum need to be tested before grinding.
[0057] S2) Setting the feeding angle of the granulator, firstly adding the ground phosphogypsum into the granulator and rotating it for 5-10 seconds, then adding the mixture of ground slag powder and ground cement kiln dust, and water-resistant enhancer into the granulator for artificial granulation, and adding water during the granulation process to obtain phosphogypsum-based artificial aggregate.
[0058] The present invention dries the original phosphogypsum (the main material in the artificial aggregate) and then grinds it. Under the combined action of the physical excitation method of grinding the ground phosphogypsum in a ball mill and an active activator (including the active activator in the water-resistant enhancer, and the ground slag powder and ground cement kiln dust in the artificial aggregate), the volcanic ash activity of the phosphogypsum is fully stimulated, and the ground phosphogypsum is fully hydrated to generate a large amount of hydrated calcium silicate, hydrated calcium aluminate, and calcium hydroxide. These hydration products provide a certain strength for the artificial aggregate.
[0059] The early strength agent in the water-resistant enhancer (compounded by one or more of Glauber's salt, sodium sulfate, trihydroxyethanolamine, and sodium thiosulfonate) increases the alkalinity of the system and increases the early strength of the solid waste group aggregate by promoting the formation of calcium hydroxide, calcium sulfate, calcium carbonate, and hydrated calcium aluminate;
[0060] The waterproofing agent in the water-resistant enhancer (composite of one or more of sodium silicate pentahydrate, nano-silicon dioxide, polyaluminum chloride, polyaluminum chloride iron, potassium trimethylsilanolate, methyl aluminum silicate, polyacrylate, silicone) combines with the hydroxide in the solution to generate a large amount of colloid substances that are difficult to dissolve in water, such as iron hydroxide and aluminum hydroxide colloid, which stimulate the further reaction of calcium aluminate hydrate produced by phosphogypsum to generate calcium sulfoaluminate crystals with certain expansion. These colloids and crystals fill the capillaries formed in the aggregate during the hardening process, improve the density of the aggregate, and thus improve the waterproof effect; at the same time, the hydrolysis of silicone forms water-soluble silanol, which reacts with polyacrylate and forms a layer of mesh-like hydrophobic siloxane film that is not easy to penetrate water on the surface of the phosphogypsum aggregate, thereby improving the waterproof effect;
[0061] The theoretical water-to-paste ratio of phosphogypsum is only about 18%, but in actual production, due to the requirement of fluidity, the actual water consumption often reaches 60% to 80%. The excess water overflows or evaporates from the slurry during the hardening process of phosphogypsum, leaving a large number of micropores and cracks inside the hardened body. The water reducing agent in the water-resistant enhancer (compounded by one or more of sodium humate, aminosulfonic acid, sodium xylene sulfonate, and naphthalene-based water reducing agent) reduces the water consumption, thereby increasing the strength. At the same time, the higher strength can effectively prevent cracks and help improve the long-term effectiveness of the waterproof effect.
[0062] The thickener in the water-resistant enhancer (composite of one or more of xanthan gum, xylitol mother liquor, and hydroxybutyl methylcellulose) has gelling properties, which can bind the phosphogypsum particles together and fill the gaps between the phosphogypsum particles, thereby reducing the porosity and increasing the strength. However, it is easily eroded by water bodies. At this time, the methyl aluminum silicate in the waterproofing agent reacts with carbon dioxide and water to form a hydrophobic film on the surface of the xanthan gum, which reduces erosion by water bodies and increases the strength of the aggregate.
[0063] The passivator in the water-resistant enhancer (composite of one or more of petroleum coke desulfurization ash, carbide slag, calcium formate, sodium lignosulfonate, diatomaceous earth, and polyacrylic resin) can provide calcium ions, which react with soluble phosphorus and fluorine in phosphogypsum to generate calcium phosphate and calcium fluoride precipitates, thereby reducing the phosphorus and fluorine content in phosphogypsum.
[0064] Based on 100 parts by weight of the dry total weight of the phosphogypsum-based artificial aggregate, the phosphogypsum-based artificial aggregate includes the following components: 80-85 parts by weight of ground phosphogypsum, 8-12 parts by weight of ground slag powder, 5-9 parts by weight of ground cement kiln dust, and 0.1-5 parts by weight of a water-resistant enhancer.
[0065] Water accounts for 18% to 23% of the total dry weight of the phosphogypsum-based artificial aggregate.
[0066] S3) discharging the phosphogypsum-based artificial aggregate in step S3) and setting a discharging angle of the granulator.
[0067] Specifically, the feeding angle of the granulator is set to 44° to 51°, and the discharging angle of the granulator is set to 68° to 80°.
[0068] S4) performing moisture-curing on the unloaded phosphogypsum-based artificial aggregate, and controlling the relative humidity during the curing period.
[0069] Specifically, the aggregate after unloading is subjected to moisture-maintaining curing for 28 days, and the relative humidity in the curing room is controlled to be above 90%.
[0070] Example 1
[0071] The original phosphogypsum was dried and then ball-milled in a ball mill for 60 minutes. The specific surface area of the phosphogypsum after ball milling was 450m 2 / kg. After drying, the slag was ball-milled in a ball mill for 30 minutes. The specific surface area of the slag after ball milling was 500m 2 / kg. Cement kiln dust is calcined at 500℃-700℃ for 2h, cooled to room temperature and then ball milled in a ball mill for 30min. The specific surface area of the cement after ball milling is 330m 2 / kg.
[0072] Take 80.5kg of ground phosphogypsum, 12kg of ground slag, 7.5kg of ground cement kiln dust, 1kg of water-resistant enhancer, and the mixed moisture content is 23.0kg.
[0073] The water-resistant enhancer consists of 0.65kg of composite waterproofing agent, 0.05kg of early strength agent, 0.1kg of active stimulant, 0.1kg of passivator, 0.05kg of thickener and 0.05kg of water reducer.
[0074] The waterproofing agent is compounded by 0.0325kg of sodium metasilicate pentahydrate, 0.065kg of nano silicon dioxide, 0.2275kg of polyaluminium chloride, 0.13kg of polyaluminium ferric chloride, 0.0325kg of potassium trimethylsilanol, 0.065kg of methyl aluminium silicate, 0.0325kg of polyacrylate and 0.065kg of silicone.
[0075] The early strength agent is compounded by 0.015kg of mirabilite, 0.0225kg of glauber's salt, 0.001kg of trihydroxyethanolamine and 0.0115kg of sodium thiosulfonate.
[0076] The active activator is compounded from 0.06kg of slag, 0.01kg of silica fume and 0.03kg of cement.
[0077] The passivating agent is compounded from 0.01kg of petroleum coke desulfurization ash, 0.02kg of carbide slag, 0.02kg of calcium formate, 0.02kg of sodium lignosulfonate, 0.02kg of diatomaceous earth and 0.01kg of polyacrylic acid resin.
[0078] The thickener is compounded from 0.0225 kg of xanthan gum, 0.0125 kg of xylitol mother liquor and 0.015 kg of hydroxybutyl methylcellulose.
[0079] The water reducing agent is compounded by 0.005 kg of sodium humate, 0.0125 kg of ammonia sulfamic acid, 0.0125 kg of sodium xylene sulfonate, and 0.02 kg of naphthalene-based water reducing agent.
[0080] According to the following processing method, a highly water-resistant phosphogypsum-based artificial aggregate is prepared.
[0081] S1) The moisture content, fluorine content and phosphorus content of the original phosphogypsum were tested. The free phosphorus content in the original phosphogypsum was 5.2 mg / L, and the free fluoride ion content was 329 mg / L.
[0082] S2) The feeding angle of the granulator is set to 44° to 51°, the ground phosphogypsum is first added to the granulator and rotated for 5 to 10 seconds, and then the mixture of ground slag powder and ground cement kiln dust and water-resistant enhancer are added to the granulator for granulation. Water is added during the granulation process, and the water accounts for 18% to 23% of the total dry raw material.
[0083] S3) The aggregate granulated in step S2) is unloaded, and the unloading angle of the granulator is set to 68° to 80°.
[0084] S4) The aggregate after unloading is subjected to moisture-curing curing for 28 days, and the relative humidity in the curing room is controlled to be above 90%.
[0085] The test results of artificial aggregates show that:
[0086] Cylinder pressure strength 6.07MPa, water absorption 6.7%, softening coefficient 0.84, loose bulk density 1066.3kg / m 3 , meeting the requirements of Class II crushed stone in GBT 14685-2011 construction crushed stone and gravel standard and JTG TF50-2011 highway bridge and culvert construction technical specifications, and can be used for the preparation of concrete with strength grade C30-C60 and requirements for frost resistance, impermeability or other requirements;
[0087] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 1.01 mg / L and the total phosphorus was 0.12 mg / L, which met the requirements of Class V water body standards in the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0088] Example 2
[0089] The difference between Example 2 and Example 1 is that: 80.5 kg of ground phosphogypsum, 12 kg of ground slag, 7.5 kg of ground cement kiln dust, and a mixed moisture content of 23.0 kg are taken; in step S2 of preparing highly water-resistant phosphogypsum-based artificial aggregate, the feeding angle of the granulator is set to 44°~51°, the ground phosphogypsum is first added to the granulator and rotated for 5~10 seconds, and then the mixture of ground slag powder and ground cement kiln dust is added to the granulator for granulation, and water is added during the granulation process, and the water accounts for 18%~23% of the total amount of dry raw materials.
[0090] The test results of artificial aggregates show that:
[0091] Cylinder pressure strength 2.85MPa, water absorption 23%, softening coefficient 0.65, loose bulk density 1032.3kg / m 3 , which cannot meet the requirements of Class II crushed stone in GBT 14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction;
[0092] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry Method" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 2.2 mg / L and the total phosphorus was 0.56 mg / L, which could not meet the Class V water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0093] Example 3
[0094] The difference between Example 3 and Example 1 is that 83 kg of ground phosphogypsum, 12 kg of ground slag, 5 kg of ground cement kiln dust, and 1 kg of water resistance enhancer are taken, and the mixed moisture content is 23.0 kg.
[0095] The test results of artificial aggregates show that:
[0096] Cylinder pressure strength 5.95MPa, water absorption 6.6%, softening coefficient 0.82, loose bulk density 1060.3kg / m 3 , meeting the requirements of Class II crushed stone in GBT 14685-2011 construction crushed stone and gravel standard and JTG TF50-2011 highway bridge and culvert construction technical specifications, and can be used for the preparation of concrete with strength grade C30-C60 and requirements for frost resistance, impermeability or other requirements;
[0097] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 1.03 mg / L and the total phosphorus was 0.14 mg / L, which met the requirements of Class V water body standards in the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0098] Example 4
[0099] The difference between Example 4 and Example 1 is that: 83 kg of ground phosphogypsum, 12 kg of ground slag, and 5 kg of ground cement kiln dust are taken, and the mixed moisture content is 23.0 kg; step S2 of preparing highly water-resistant phosphogypsum-based artificial aggregate) The feeding angle of the granulator is set to 44°~51°, the ground phosphogypsum is first added to the granulator and rotated for 5~10s, and then the mixture of ground slag powder and ground cement kiln dust is added to the granulator for granulation, and water is added during the granulation process, and the water accounts for 18%~23% of the total amount of dry raw materials.
[0100] The test results of artificial aggregates show that:
[0101] Cylinder pressure strength 2.70MPa, water absorption 24%, softening coefficient 0.63, loose bulk density 1029.3kg / m 3 , which cannot meet the requirements of Class II crushed stone in GBT 14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction;
[0102] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry Method" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 2.5 mg / L and the total phosphorus was 0.72 mg / L, which could not meet the Class V water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0103] Example 5
[0104] The difference between Example 5 and Example 1 is that 85 kg of ground phosphogypsum, 10 kg of ground slag, 5 kg of ground cement kiln dust, and 1 kg of water resistance enhancer are taken, and the mixed moisture content is 23.0 kg.
[0105] The test results of artificial aggregates show that:
[0106] Cylinder pressure strength 5.85MPa, water absorption 6.4%, softening coefficient 0.80, loose bulk density 1056.3kg / m 3 , meeting the requirements of Class II crushed stone in GBT 14685-2011 construction crushed stone and gravel standard and JTG TF50-2011 highway bridge and culvert construction technical specifications, and can be used for the preparation of concrete with strength grade C30-C60 and requirements for frost resistance, impermeability or other requirements;
[0107] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 1.05 mg / L and the total phosphorus was 0.17 mg / L, which met the requirements of Class V water body standards in the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0108] Example 6
[0109] The difference between Example 6 and Example 1 is that: 85 kg of ground phosphogypsum, 10 kg of ground slag, and 5 kg of ground cement kiln dust are taken, and the mixed moisture content is 23.0 kg; step S2 of preparing highly water-resistant phosphogypsum-based artificial aggregate) The feeding angle of the granulator is set to 44°~51°, the ground phosphogypsum is first added to the granulator and rotated for 5~10s, and then the mixture of ground slag powder and ground cement kiln dust is added to the granulator for granulation, and water is added during the granulation process, and the water accounts for 18%~23% of the total amount of dry raw materials.
[0110] The test results of artificial aggregates show that:
[0111] Cylinder pressure strength 2.50MPa, water absorption 28%, softening coefficient 0.62, loose bulk density 1015.6kg / m 3 , which cannot meet the requirements of Class II crushed stone in GBT 14685-2011 Standard for Construction Crushed Stone and Pebbles and JTG TF50-2011 Technical Specifications for Highway Bridge and Culvert Construction;
[0112] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry Method" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 2.8 mg / L and the total phosphorus was 0.98 mg / L, which could not meet the Class V water body standard requirements of the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0113] Example 7
[0114] The difference between Example 7 and Example 1 is that 85 kg of ground phosphogypsum, 10 kg of ground slag, 5 kg of ground cement kiln dust, 2 kg of water resistance enhancer are taken, and the mixed moisture content is 23.0 kg.
[0115] The test results of artificial aggregates show that:
[0116] Cylinder pressure strength 6.52MPa, water absorption 5.5%, softening coefficient 0.85, loose bulk density 1064.3kg / m 3 , meeting the requirements of Class II crushed stone in GBT 14685-2011 construction crushed stone and gravel standard and JTG TF50-2011 highway bridge and culvert construction technical specifications, and can be used for the preparation of concrete with strength grade C30-C60 and requirements for frost resistance, impermeability or other requirements;
[0117] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 0.98 mg / L and the total phosphorus was 0.12 mg / L, which met the requirements of Class V water body standards in the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0118] Example 8
[0119] The difference between Example 8 and Example 1 is that 85 kg of ground phosphogypsum, 10 kg of ground slag, 5 kg of ground cement kiln dust, 0.5 kg of water resistance enhancer are taken, and the mixed moisture content is 23.0 kg.
[0120] The test results of artificial aggregates show that:
[0121] Cylinder pressure strength 7.65MPa, water absorption 4.6%, softening coefficient 0.87, loose bulk density 1072.3kg / m 3 , meeting the requirements of Class II crushed stone in GBT 14685-2011 construction crushed stone and gravel standard and JTG TF50-2011 highway bridge and culvert construction technical specifications, and can be used for the preparation of concrete with strength grade C30-C60 and requirements for frost resistance, impermeability or other requirements;
[0122] After 28 days, the artificial aggregate was used to prepare the leachate according to the "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method" (HJ 557-2010). The total phosphorus content in the leachate was tested according to the "Solid Waste Total Phosphorus Determination Ammonium Metamolybdate Spectrophotometry" (HJ 712-2014), and the fluoride ion content was tested according to the "Solid Waste Fluoride Determination Ion Selective Electrode Method" (GB / T15555.11-1995). The fluoride ion concentration of the leachate was 0.82 mg / L and the total phosphorus was 0.10 mg / L, which met the requirements of Class V water body standards in the "Surface Water Environmental Quality Standard" (GB 3838-2002).
[0123] Therefore, in summary, after adding water-resistant enhancer, the early strength of phosphogypsum-based artificial aggregate is greatly improved, the water resistance is significantly improved, the leaching rate of heavy metal ions such as fluorine and phosphorus is greatly reduced, and it meets the standards for crushed stone for construction. It can be widely used in C30-C60 grade concrete and highway subgrade materials, effectively alleviating the environmental pollution and large-scale accumulation problems of phosphogypsum.
[0124] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A water resistance enhancer, characterized in that: Based on the total weight of the water resistance enhancer being 100 parts by weight, the water resistance enhancer includes the following components: 60-70 parts by weight of waterproofing agent, 3-5 parts by weight of early strength agent, 10-20 parts by weight of active stimulant, 10-15 parts by weight of passivator, 2-5 parts by weight of thickener, and 0.1-20 parts by weight of water reducer.
2. The water resistance enhancer according to claim 1, characterized in that: The waterproofing agent is composited by one or more of 1%-5% by weight of sodium metasilicate pentahydrate, 5%-10% by weight of nano silicon dioxide, 30%-40% by weight of polyaluminium chloride, 20%-30% by weight of polyaluminium ferric chloride, 1%-5% by weight of potassium trimethylsilanol, 10%-20% by weight of methyl aluminium silicate, 1%-5% by weight of polyacrylate and 5%-10% by weight of silicone.
3. The water resistance enhancer according to claim 2, characterized in that: The early strength agent is compounded from one or more of 20%-30% by weight of sodium sulfate, 30%-40% by weight of sodium sulfate, 1%-2% by weight of trihydroxyethanolamine, and 10%-30% by weight of sodium thiosulfonate.
4. The water resistance enhancer according to claim 3, characterized in that: The active activator is composited from one or more of 40% to 60% by weight of slag, 10% to 30% by weight of silica fume, and 20% to 30% by weight of cement.
5. The water resistance enhancer according to claim 4, characterized in that: The passivating agent is composited by one or more of 10%-20% by weight of petroleum coke desulfurization ash, 20%-40% by weight of carbide slag, 20%-30% by weight of calcium formate, 20%-30% by weight of sodium lignosulfonate, 20%-30% by weight of diatomaceous earth and 5%-10% by weight of polyacrylic acid resin.
6. The water resistance enhancer according to claim 5, characterized in that: The thickener is composited from one or more of 40% to 50% by weight of xanthan gum, 10% to 30% by weight of xylitol mother liquor, and 40% to 50% by weight of hydroxybutyl methylcellulose.
7. The water resistance enhancer according to claim 6, characterized in that: The water reducer is compounded from one or more of 1% to 10% by weight of sodium humate, 1% to 30% by weight of aminosulfonic acid ammonia, 5% to 30% by weight of sodium xylene sulfonate, and 40% to 50% by weight of naphthalene series water reducer.
8. A method for preparing phosphogypsum-based artificial aggregate, characterized in that: Using the water resistance enhancer as claimed in any one of claims 1 to 7 comprises the following steps: S1) drying the original phosphogypsum and grinding it to obtain ground phosphogypsum; drying the original slag and grinding it to obtain ground slag powder; calcining cement kiln dust at high temperature, cooling it to room temperature, and then grinding it to obtain ground cement kiln dust; S2) setting a feeding angle of the granulator, first adding the ground phosphogypsum into the granulator and rotating it for 5 to 10 seconds, then adding a mixture of ground slag powder and ground cement kiln dust, and a water-resistant enhancer into the granulator for artificial granulation, and adding water during the granulation process to obtain phosphogypsum-based artificial aggregate; Based on 100 parts by weight of the dry total weight of the phosphogypsum-based artificial aggregate, the phosphogypsum-based artificial aggregate comprises the following components: 80-85 parts by weight of ground phosphogypsum, 8-12 parts by weight of ground slag powder, 5-9 parts by weight of ground cement kiln dust, and 0.1-5 parts by weight of a water-resistant enhancer; Water accounts for 18% to 23% of the total dry weight of the phosphogypsum-based artificial aggregate; S3) discharging the phosphogypsum-based artificial aggregate in step S3) and setting a discharging angle of a granulator; S4) performing moisture-curing on the unloaded phosphogypsum-based artificial aggregate, and controlling the relative humidity during the curing period.
9. The method for preparing phosphogypsum-based artificial aggregate according to claim 8, characterized in that: In S1), the ground phosphogypsum is prepared by neutralizing the original phosphogypsum with quicklime to a pH value of 7.5-8, standing for 20-24 hours, drying at 50-60° C., and ball milling in a ball mill for 60-80 minutes until the specific surface area is greater than or equal to 450 m 2 / kg of phosphogypsum; The ground slag powder is obtained by drying the original slag at 50-60°C, and ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 500m 2 / kg of slag powder; The ground cement kiln dust is obtained by calcining the original cement kiln dust at a high temperature of 500-700°C for 1-2 hours, cooling it to room temperature, and then ball milling it in a ball mill for 25-35 minutes until the specific surface area is greater than or equal to 330 m 2 / kg of cement kiln dust.
10. The method for preparing phosphogypsum-based artificial aggregate according to claim 9, characterized in that: In S2), the feeding angle of the granulator is set to 44° to 51°, and the discharging angle of the granulator is set to 68° to 80°.
Citation Information
Patent Citations
Low-toxicity phosphogypsum-based high-strength artificial aggregate and preparation method thereof
CN111732356A
Gypsum-based unfired aggregate
CN113121138A
Phosphogypsum-based aggregate and preparation method thereof
CN113354376A
Energy storage phosphorus building gypsum aggregate and preparation method thereof
CN113402187A
All-solid waste phosphogypsum-based aggregate as well as preparation method and application thereof
CN118206349A