Kaolin inorganic composite graphite polyphenyl granule insulation board and preparation method thereof

By combining kaolin, industrial waste residue and other materials with graphite polystyrene particles, a kaolin inorganic composite graphite polystyrene particle insulation board is prepared, which solves the problems of poor waterproof performance and unstable mechanical properties of insulation materials in the existing technology, and achieves high efficiency and Environmentally friendly insulation effect and improved production efficiency.

CN118745098APending Publication Date: 2024-10-08NINGXIA SHENGTE THERMAL INSULATION MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410750427.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing all-inorganic insulation materials such as rock wool boards have poor waterproof performance, are easy to peel off, and will emit toxic and harmful substances during production and use, affecting the environment and human health; thermosetting composite polystyrene insulation boards have poor sheet integrity and poor mechanical properties. Unstable.

Method used

Kaolin, industrial waste residue, construction rubber powder, short fibers, admixtures and graphite polystyrene particles are combined to form an inorganic slurry that is evenly mixed with graphite polystyrene particles. Through precise metering, two-stage feeding, high-speed mixing, mold pressing and molding, Kaolin inorganic composite graphite polystyrene particle insulation board is prepared through automated cutting and other processes.

Benefits of technology

It achieves good thermal insulation effect, fire resistance and mechanical properties, improves production efficiency and economic benefits, reduces personnel consumption, has a solid product structure, has good practical value and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745098A_ABST
    Figure CN118745098A_ABST
Patent Text Reader

Abstract

The invention discloses a kaolin inorganic composite graphite polyphenyl granule insulation board, which comprises inorganic slurry and graphite polyphenyl granules, and the use amount of the inorganic slurry is 90-110 kg / m < 3 >; the graphite polyphenyl particles are 10-15 Kg / m < 3 >, and the inorganic slurry uniformly coats the graphite polyphenyl particles. The preparation method comprises the steps of raw material proportioning, two-stage feeding, stirring, mold compression molding, curing, demolding, secondary curing, cutting, inspection and packaging and delivery. The kaolin inorganic composite graphite polyphenyl granule insulation board is excellent in insulation effect and good in fireproof performance and mechanical property, the preparation method saves personnel consumption in the production process, the structure of the kaolin inorganic composite graphite polyphenyl granule insulation board is firmer, the quality and the bearing capacity are improved, and good practical value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of thermal insulation boards, and in particular relates to a kaolin inorganic composite graphite polyphenyl particle thermal insulation board and a preparation method thereof. Background Art

[0003] The existing all-inorganic thermal insulation materials are mainly rock wool boards, but rock wool is made of cotton yarns woven and pressed, with poor waterproof performance and easy to delaminate and peel off. If it is directly used in the external wall insulation project in the form of adhesive anchors, it is easy to cause the insulation layer to fall off as a whole, and the external wall surface is very likely to cause mildew and other phenomena after water seepage. In response to this, many manufacturers add water repellents to rock wool products. Since the water repellent has chemical failure, the rock wool insulation layer is more likely to crack and absorb water and fall off over time. The rock wool insulation used in external wall insulation on the market will emit toxic, harmful and radioactive substances during both the production process and the use process, which will pollute the environment and cause harm to the human body. In addition, the cutting of rock wool products during the construction process will cause continuous and severe skin damage to the construction workers, and the flying silk mineral powder caused by the cutting products can be easily inhaled into the human respiratory tract, leading to a serious occupational disease - silicosis.

[0004] Inorganic and organic composite insulation materials are made by combining the fireproof properties of inorganic slurry and the good thermal insulation properties of organic insulation materials. They are favored by customers for their advantages such as light weight, good thermal insulation effect and good fireproof performance. At present, the common composite insulation materials on the market are thermosetting composite polystyrene insulation boards, but the production process of this product adopts a vacuum suction cup infiltration process. Since the pore size cannot be guaranteed during the molding of the substrate, there is uneven infiltration during the infiltration process, and the requirements for the fineness of the inorganic slurry raw materials are very strict, which makes the thermosetting composite polystyrene insulation board produced have poor integrity and unstable mechanical properties, which are subject to certain restrictions in engineering applications. Summary of the invention

[0005] The object of the present invention is to provide a kaolin inorganic composite graphite polyphenyl particle insulation board and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a kaolin inorganic composite graphite polyphenyl particle insulation board, comprising

[0007] Inorganic slurry and graphite polystyrene particles, the dosage is: Inorganic sizing material: 90-110Kg / m 3 ;Graphite polystyrene particles 10-15Kg / m 3 ;

[0008] The inorganic slurry uniformly coats the graphite polyphenyl particles.

[0009] Preferably, the graphite polyphenylene particles are connected to each other on all sides by an inorganic adhesive to form an organizational structure in the shape of a molecular connection.

[0010] Preferably, in any of the above solutions, the graphite polyphenylene particles and the inorganic slurry form a honeycomb structure.

[0011] In any of the above schemes, preferably, the inorganic slurry comprises kaolin, industrial waste residue, building glue powder, short fibers, admixtures and water.

[0012] Preferably, in any of the above schemes, the graphite polyphenylene particles are spherical particles in appearance.

[0013] Preferably, in any of the above schemes, the graphite polyphenylene particles have a diameter of 3-5 mm and a bulk density of 8-15 kg / m3.

[0014] The present invention also provides a method for preparing a kaolin inorganic composite graphite polyphenyl particle insulation board, comprising the following steps:

[0015] S1: Raw material ratio: The raw material ratio measurement adopts a single-portion measurement system. The single portion means that the materials poured into each mold box are individually measured at the raw material end and then stirred and mixed. The measurement accuracy of the raw materials is controlled within 1%, so that the bulk density of each mold is uniform and accurate. The difficulty in achieving the above requirements is that the measurement system must be both fast and accurate. Once the measurement speed is too slow, it will directly affect the production efficiency. The use of high-precision measurement modules imported from Germany, combined with the combination logic control program compiled by the company, perfectly solves the above bottlenecks.

[0016] S2: Two-stage loading: The first-stage loading is to put the measured water and powder into the mixer one by one, which is realized in a fully closed state. In this way, the generation of dust is avoided in the process of the entire mixing system. After the slurry is evenly stirred, the measured graphite polystyrene particles are filled in through the secondary loading port.

[0017] S3: Mixing: The first stage of mixing is to use a high-speed mixer to make a slurry with measured water and powder, and then the slurry enters the secondary horizontal mixer and is mixed with polystyrene particles.

[0018] S4: Mold pressing: There will be a lot of gaps after the mixed material enters the mold box. The computer-controlled film pressing system can change the pressure curve at any time according to needs and vibrate at high frequency to compact the material and control the product bulk density.

[0019] S5: Curing: The product is naturally cured for 4 hours after injection molding.

[0020] S6: Demolding: The product can be demoulded 4 hours after injection molding. The realization of automatic demoulding can effectively avoid the heavy work of demoulding and assembling the mold, especially the removal and transportation of the cover plate, and also greatly save time and manpower.

[0021] S7: Secondary curing: The semi-finished products after demoulding are transported to the curing workshop for curing (natural curing).

[0022] S8: Cutting: Cutting is done by a fully automatic multi-layer band saw closed cutting machine. According to customer requirements, the computer controls the high-precision automatic adjustment of the band saw spacing. The thickness of the cut plate is controlled within ±1mm, and the diagonal size is controlled within 1mm.

[0023] S9: Inspection and packaging: Products that have passed the inspection are packaged on the packaging machine and stacked in the finished product warehouse. The packaging machine adopts a roller-type continuous film feeding packaging method, eliminating the need for manual bagging.

[0024] S10: Delivery: The packaged products are loaded and shipped out of the factory for sale after acceptance.

[0025] The technical effects and advantages of the present invention: the kaolin inorganic composite graphite polystyrene particle insulation board and the preparation method thereof have excellent insulation effect, good fireproof performance and good mechanical properties, and solve the technical problems in the prior art that organic insulation materials have poor fireproof performance, inorganic insulation materials have poor thermal insulation performance and organic and inorganic composite insulation materials have poor mechanical properties. An inorganic slurry is prepared by mixing kaolin, industrial waste residue, building glue powder, short fibers, admixtures and water. The inorganic slurry and graphite polystyrene particles are uniformly stirred. The processes of raw material proportioning, two-stage feeding, stirring, mold pressing, curing, demoulding, secondary curing, cutting and inspection and packaging are adopted to greatly improve the production efficiency and economic benefits, save personnel consumption in the production process, make the structure of the kaolin inorganic composite graphite polystyrene particle insulation board more solid, improve the quality and load-bearing capacity, and have good practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a structural schematic diagram of the thermal insulation board of the present invention;

[0027] Figure 2 The present invention is a flow chart for preparing the thermal insulation board.

[0028] In the figure: 1. Inorganic slurry; 2. Graphite polystyrene particles. DETAILED DESCRIPTION

[0029] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0031] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features.

[0032] The present invention provides Figure 1 The kaolin inorganic composite graphite polyphenylene particle insulation board shown comprises, by weight, an inorganic slurry 1 and graphite polyphenylene particles 2;

[0033] The inorganic slurry 1 uniformly covers the graphite polyphenylene particles 2.

[0034] The graphite polyphenylene particles 2 are connected to each other on all sides through the inorganic adhesive 1 to form a molecular connection-shaped organizational structure.

[0035] The graphite polyphenylene particles 2 and the inorganic slurry 1 form a honeycomb structure.

[0036] The inorganic slurry 1 comprises kaolin, industrial waste residue, building glue powder, short fibers, admixtures and water.

[0037] The graphite polyphenylene particles 2 have a spherical particle shape.

[0038] The diameter of the graphite polystyrene particles 2 is 3-5 mm, and the bulk density is 8-15 kg / m3.

[0039] The present invention also provides Figure 2 The method for preparing a kaolin inorganic composite graphite polyphenyl particle insulation board shown comprises the following steps:

[0040] S1: Raw material ratio: The raw material ratio measurement adopts a single-portion measurement system. The single portion means that the materials poured into each mold box are individually measured at the raw material end and then stirred and mixed. The measurement accuracy of the raw materials is controlled within 1%, so that the bulk density of each mold is uniform and accurate. The difficulty in achieving the above requirements is that the measurement system must be both fast and accurate. Once the measurement speed is too slow, it will directly affect the production efficiency. The use of high-precision measurement modules imported from Germany, combined with the combination logic control program compiled by the company, perfectly solves the above bottlenecks.

[0041] S2: Two-stage loading: The first-stage loading is to put the measured water and powder into the mixer one by one, which is realized in a fully closed state. In this way, the generation of dust is avoided in the process of the entire mixing system. After the slurry is evenly stirred, the measured graphite polystyrene particles are filled in through the secondary loading port.

[0042] S3: Mixing: The first stage of mixing is to use a high-speed mixer to make a slurry with measured water and powder, and then the slurry enters the secondary horizontal mixer and is mixed with polystyrene particles.

[0043] S4: Mold pressing: There will be a lot of gaps after the mixed material enters the mold box. The computer-controlled film pressing system can change the pressure curve at any time according to needs and vibrate at high frequency to compact the material and control the product bulk density.

[0044] S5: Curing: The product is naturally cured for 4 hours after injection molding.

[0045] S6: Demolding: The product can be demoulded 4 hours after injection molding. The realization of automatic demoulding can effectively avoid the heavy work of demoulding and assembling the mold, especially the removal and transportation of the cover plate, and also greatly save time and manpower.

[0046] S7: Secondary curing: The semi-finished products after demoulding are transported to the curing workshop for curing (natural curing).

[0047] S8: Cutting: Cutting is done by a fully automatic multi-layer band saw closed cutting machine. According to customer requirements, the computer controls the high-precision automatic adjustment of the band saw spacing. The thickness of the cut plate is controlled within ±1mm, and the diagonal size is controlled within 1mm.

[0048] S9: Inspection and packaging: Products that have passed the inspection are packaged on the packaging machine and stacked in the finished product warehouse. The packaging machine adopts a roller-type continuous film feeding packaging method, eliminating the need for manual bagging.

[0049] S10: Delivery: The packaged products are loaded and shipped out of the factory for sale after acceptance.

[0050] The kaolin inorganic composite graphite polyphenyl particle insulation board of the present invention has a product bulk density of ≤140Kg / m 3; Thermal conductivity ≤ 0.045W / (K·m); Combustion performance can reach A1 level; Compressive strength ≥ 200Kpa. All performance indicators are better than the current G-type thermosetting composite basic ethylene foam insulation board. The kaolin inorganic composite graphite polystyrene particle insulation board has both high-efficiency thermal insulation and fire retardancy, and has the characteristics of light weight, low thermal conductivity, low water absorption, and stable mechanical properties. The raw materials used are kaolin and industrial waste slag (silica ash and fly ash) which are relatively cheap and can be obtained locally, so as to reduce the production cost of the insulation board, utilize industrial waste, improve the performance of the insulation board, realize the recycling of industrial waste, and have good economic, social and ecological benefits.

[0051] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A kaolin inorganic composite graphite polystyrene particle insulation board, characterized in that: include Inorganic slurry (1) and graphite polyphenylene particles (2), the dosage of which is: Inorganic slurry (1): 90-110 kg / m 3 ; Graphite polyphenylene particles (2) 10-15Kg / m 3 ; The inorganic slurry (1) uniformly coats the graphite polyphenylene particles (2).

2. The kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 1, characterized in that: The four sides of the graphite polyphenylene particles (2) are connected to each other through the inorganic adhesive (1), forming an organizational structure in the shape of molecular connection.

3. The kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 2, characterized in that: The graphite polyphenyl particles (2) and the inorganic slurry (1) form a honeycomb structure.

4. The kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 1, characterized in that: The inorganic slurry (1) comprises kaolin, industrial waste residue, building glue powder, short fibers, additives and water.

5. The kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 1, characterized in that: The graphite polyphenylene particles (2) are spherical particles in appearance.

6. The kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 5, characterized in that: The graphite polyphenylene particles (2) have a diameter of 3-5 mm and a bulk density of 8-15 kg / m3.

7. A method for preparing the kaolin inorganic composite graphite polyphenyl particle insulation board according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Raw material ratio: The raw material ratio measurement adopts a single-portion measurement system. The single-portion means that the material poured into each mold box is stirred and mixed after being individually measured at the raw material end. The measurement accuracy of the raw materials is controlled within 1%, so that the bulk density of each mold is uniform and accurate; S2: Two-stage feeding: The first stage of feeding is to put the measured water and powder into the mixer one by one, which is achieved in a fully closed state. After the slurry is evenly stirred, the measured graphite polystyrene particles are charged through the second-stage feeding port; S3: stirring: the first stage of stirring is to use a high-speed stirring machine to make an inorganic slurry (1) with measured water and powder, and then the slurry enters a secondary horizontal stirrer and is mixed with graphite polystyrene particles (2); S4: Mold pressing and molding: Change the pressure curve at any time according to the needs and vibrate at high frequency to compact the material and control the bulk density of the product; S5: Curing: The product is naturally cured for 4 hours after injection molding; S6: Demolding: The product is automatically demoulded 4 hours after injection molding; S7: Secondary curing: The semi-finished products after demoulding are transported to the curing workshop for curing; S8: Cutting: Cutting is carried out by a fully automatic multi-layer band saw closed cutting machine. The thickness of the cut plate is controlled within ±1mm, and the diagonal size is controlled within 1mm; S9: Inspection and packaging: After the products pass the inspection, they are packaged on the packaging machine and stacked in the finished product warehouse. The packaging machine adopts the roller type continuous film feeding packaging method; S10: Delivery: The packaged products are loaded and shipped out of the factory for sale after acceptance.

8. The method for preparing a kaolin inorganic composite graphite polyphenyl particle insulation board according to claim 7, characterized in that: In step S7, the curing is natural curing.

Citation Information

Patent Citations

  • Composite fireproof insulation board

    CN103833324A

  • Silicon modified heat-insulating plate and manufacturing method

    CN106182350A

  • Homogeneous flexible fireproof insulation board

    CN108585637A