Steel slag low-carbon concrete and preparation method thereof

By using alternative materials such as steel slag, construction recycled aggregates and slag powder in concrete, the problem of carbon emissions and strength in concrete production is solved, low-carbon, high-performance concrete preparation is achieved, and environmental impact and production costs are reduced.

CN118745104APending Publication Date: 2024-10-08SHANGHAI MCC ENVIRONMENTAL ENG TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410733264.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

A large amount of carbon dioxide is emitted during the existing concrete production process, leading to environmental pollution and health damage. When clay is used to replace cement, the strength of concrete may be reduced and the durability affected.

Method used

Steel slag and construction recycled aggregate are used to replace natural sand and gravel, and slag powder, silica fume and desulfurized gypsum are used to replace part of the cement. Low-carbon concrete is prepared through specific proportions and mixing methods to improve compressive strength and reduce carbon emissions.

Benefits of technology

On the premise of ensuring compressive strength, it can significantly reduce carbon emissions, improve concrete performance, reduce production costs, and expand the comprehensive utilization rate of steel slag and slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745104A_ABST
    Figure CN118745104A_ABST
Patent Text Reader

Abstract

The invention provides steel slag low-carbon concrete. The low-carbon concrete is prepared from the following raw materials in parts by weight: 2260 to 2990 parts of electric furnace steel slag, 0 to 350 parts of building recycled aggregate, 200 to 320 parts of slag powder, 50 to 70 parts of silica fume, 0 to 30 parts of desulfurized gypsum, 10 to 120 parts of cement, 0 to 4 parts of sodium silicate and 180 to 200 parts of water, the preparation method comprises the following steps: (1) mixing the slag powder, the silica fume and the cement to obtain a mixture I; (2) mixing the mixture I obtained in the step (1) with part of water to obtain a mixture II; (3) mixing the mixture II obtained in the step (2) with electric furnace steel slag to obtain a mixture III; and (4) mixing the mixture III obtained in the step (3) with the residual water, and uniformly stirring to obtain the product. The concrete prepared by the invention is relatively good in compressive strength and relatively low in porosity and carbon emission.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to concrete, in particular to steel slag low-carbon concrete and a preparation method thereof. Background Art

[0002] Carbon dioxide is one of the most important greenhouse gases. Since the Industrial Revolution, global climate change caused by the sharp increase in greenhouse gas concentrations has become the focus of attention of all countries.

[0003] In addition to coal-fired power and steel industries, cement is the industrial sector with the largest CO2 emissions in the world. China is a major cement producer, so the cement industry has become one of China's largest sources of carbon emissions. In the industrial chain, the entire production capacity and output of cement are almost related to concrete. Concrete is made by mixing cement, sand, stone, water, etc. in a certain proportion, and then mixing, molding, and curing. It is the most widely used building material in the world and is widely used in infrastructure construction, including railways, highways, water conservancy, nuclear power, and construction. In recent years, my country's concrete production and consumption have reached more than 50% of the world's total consumption. A large amount of CO2 is emitted during the production and application of concrete. Among them, CO2 emissions from cement production account for about 44% of CO2 emissions in the building materials production stage. It takes 0.161 to 0.296 tons of coal to produce 1 ton of cement clinker, and coal combustion will produce 0.383 to 0.704 tons of CO2. In addition to the CO2 produced by the decomposition of calcium carbonate when producing clinker, 0.894 to 1.215 tons of CO2 will be emitted for every 1 ton of cement clinker produced. The emission of large amounts of carbon dioxide not only destroys the human living environment, but also greatly harms human health.

[0004] Based on the above description, the preparation of low-carbon concrete is an important research direction. At present, carbon emissions are generally reduced from concrete raw materials, product production and later applications. Among them, the effect of reducing carbon emissions from concrete raw materials is more significant.

[0005] From the perspective of concrete raw materials, the way to achieve low carbon is generally to replace cement with natural materials with cementitious properties. Natural materials with cementitious properties can be clay, volcanic ash, etc.

[0006] The above method has improved the problem of high carbon content in concrete to a certain extent, but the addition of clay may form "air spaces" in the concrete, causing the strength of the concrete to decrease and affecting the durability of the concrete. Summary of the invention

[0007] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a steel slag low-carbon concrete and a preparation method thereof, so as to ensure the compressive strength of the concrete while reducing carbon emissions.

[0008] To achieve the above objectives and other related objectives, the present invention is achieved through the following technical solutions.

[0009] The first aspect of the present invention is to provide a steel slag low-carbon concrete, which includes the following raw materials in parts by weight: 2260-2990 parts of electric furnace steel slag, 0-350 parts of building recycled aggregate, 200-320 parts of slag powder, 50-70 parts of silica fume, 0-30 parts of desulfurized gypsum, 10-120 parts of cement, 0-4 parts of sodium silicate, and 180-200 parts of water.

[0010] The second aspect of the present invention is to provide a method for preparing steel slag low-carbon concrete, comprising the following steps:

[0011] (1) mixing slag powder, silica fume and cement to obtain a mixture 1;

[0012] (2) mixing the mixed material 1 obtained in step (1) with a portion of water to obtain a mixed material 2;

[0013] (3) mixing the mixed material 2 obtained in step (2) with electric furnace slag to obtain a mixed material 3;

[0014] (4) Mix the mixture obtained in step (3) with the remaining water and stir evenly to obtain a product.

[0015] In some embodiments of the present invention, the mixing and stirring time in step (3) is 2-3 minutes.

[0016] As described above, the steel slag low-carbon concrete and the preparation method thereof of the present invention have the following beneficial effects:

[0017] (1) The steel slag low-carbon concrete of the present invention uses solid waste electric furnace steel slag and construction recycled aggregates to replace natural sand and gravel as coarse and fine aggregates of concrete, and uses slag powder, silica fume, desulfurized gypsum, etc. to replace part of the cement. It has better compressive strength and lower porosity and carbon emissions.

[0018] (2) The steel slag low-carbon concrete of the present invention can be used in road engineering concrete, indoor and outdoor field concrete, and municipal concrete prefabricated products to not only improve the performance of concrete and reduce carbon emissions, but also increase the comprehensive utilization rate of steel slag and slag while reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It shows the performance improvement rate of the steel slag low-carbon concrete of the present invention. DETAILED DESCRIPTION

[0020] In order to make the purpose of the invention, technical solutions and beneficial technical effects of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. People familiar with this technology can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0021] The extended part of this application and the effect description of the extended part, including but not limited to subsequent data analysis, mechanism description, etc.

[0022] The first aspect of the present invention is to provide a steel slag low-carbon concrete, which includes the following raw materials in parts by weight: 2260-2990 parts of electric furnace steel slag, 0-350 parts of building recycled aggregate, 200-320 parts of slag powder, 50-70 parts of silica fume, 0-30 parts of desulfurized gypsum, 10-120 parts of cement, 0-4 parts of sodium silicate, and 180-200 parts of water.

[0023] On the one hand, the concrete of the present invention uses electric furnace steel slag and building recycled aggregate to replace natural sand and gravel resources, which alleviates the shortage of sand and gravel resources to a certain extent and avoids carbon emissions generated during the mining process; on the other hand, slag powder is mainly used, and a small amount of desulfurized gypsum, silica fume and other solid wastes are used to form slag powder low-carbon cementitious materials to replace more than 70% of cement, which has a significant effect on carbon reduction. In addition, steel slag and slag are relatively cheap as solid wastes in metallurgical processes. The use of steel slag low-carbon concrete in road engineering concrete, indoor and outdoor field concrete, and municipal concrete prefabricated products can not only improve the performance of concrete and reduce carbon emissions, but also reduce production costs while expanding the comprehensive utilization rate of steel slag and slag.

[0024] The electric furnace slag in the concrete of the present invention plays a skeleton role in the concrete and inhibits the shrinkage of cement; cement and water form cement paste, which wraps around the surface of coarse and fine aggregates and fills the gaps between aggregates; silica fume can improve the performance of hardened cement paste and concrete to a great extent, mainly because silica fume has strong volcanic ash activity and its smaller particle size and larger specific surface area. The influence of silica fume on the microstructure of hardened cement paste is generally reflected in the following aspects: (1) improving the hydration degree of cement and reacting with Ca(OH)2 for secondary hydration, increasing the amount of CSH gel in hardened cement paste, and improving the performance of traditional CSH gel, thereby improving the performance of hardened cement paste; (2) silica fume and its secondary hydration products fill the harmful pores in hardened cement paste, the macroscopic macropores and capillary pores in cement stone are reduced, and the gel pores and transition pores are increased, so that the pore size distribution changes greatly, the pores are reduced, the small pores are increased, and the distribution is uniform, thereby changing the pore structure of hardened cement paste.

[0025] The building recycled aggregate added in the present invention is combined with electric furnace steel slag, which contains almost no free calcium oxide. Compared with other types of steel slag, it is safer to use and is convenient for improving the performance of concrete. The particle size of slag powder is small, which is convenient for filling fine pores in concrete, increasing the fluidity of concrete and reducing the viscosity of concrete. The slag powder is mainly composed of chemical components such as silicate, aluminate and calcium salt, among which silicate is the most important chemical component of slag powder. Active silicate can react with hydroxide ions in water to form hydrated silicate gel. The gel is convenient for filling the pore space in concrete and improving the density of concrete. properties, thereby improving the strength of concrete; desulfurized gypsum is a product of flue gas desulfurization in coal-fired power plants. Its main component is calcium sulfate dihydrate. Slag powder has volcanic ash effect, morphological effect and filling effect. Desulfurized gypsum has an excitation effect and crystallization effect on sulfate activity. Under the action of desulfurized gypsum stimulating volcanic ash activity and its own crystallization effect, as the various effects of slag powder are strengthened, secondary hydration reactions begin to appear. More hydrates are produced and filled through the stimulation and crystallization of desulfurized gypsum, thereby improving the compressive strength of concrete; sodium silicate can form colloid SiO2·nH2O during cement hydration, and this colloid can block capillaries. When water is lost, the colloid forms a film attached to the capillary wall; when water enters again, the colloid will expand again to play an anti-seepage role. Active SiO3 introduced into cement paste 2- It can react with Ca(OH)2 formed by cement hydration to generate calcium silicate cementitious products and block cold pores to play an anti-seepage role. It uses cementitious materials mainly composed of slag powder and a small amount of desulfurized gypsum, silica fume and other solid waste to replace part of the cement, thereby reducing carbon emissions while ensuring the strength of the concrete.

[0026] In some embodiments of the present invention, the low-carbon concrete includes the following raw materials in parts by weight: 2260-2990 parts of electric furnace slag, 0-350 parts of building recycled aggregate, 200-320 parts of slag powder, 50-70 parts of silica fume, 0-30 parts of desulfurized gypsum, 10-120 parts of cement, 0-4 parts of sodium silicate, and 180-200 parts of water.

[0027] In some specific embodiments of the present invention, the weight proportion of the electric furnace slag can be 2260-2460 parts, 2460-2660 parts, 2660-2860 parts, 2860-2990 parts; typically but not limiting, for example, 2400 parts, 2500 parts, 2600 parts, 2700 parts, 2800 parts.

[0028] In some specific embodiments of the present invention, the weight proportion of the slag powder may be 200-240 parts, 240-270 parts, 270-300 parts, 300-320 parts; typically but not limiting, for example, 200 parts, 240 parts, 270 parts, 300 parts, 320 parts.

[0029] In some specific embodiments of the present invention, the weight proportion of the silica fume may be 50-55 parts, 55-60 parts, 60-65 parts, 65-70 parts; typically but not limiting, for example, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts.

[0030] In some specific embodiments of the present invention, the weight proportions of the cement may be 10-35 parts, 35-50 parts, 50-80 parts, 80-120 parts; typically but not limiting, for example, 10 parts, 35 parts, 50 parts, 80 parts, 120 parts.

[0031] In some specific embodiments of the present invention, the weight proportion of water may be 180-190 parts, 190-200 parts; typically but not limiting, for example, 180 parts, 190 parts, 200 parts.

[0032] In some specific embodiments of the present invention, the weight proportions of recycled building aggregate can be 0-50 parts, 50-100 parts, 100-150 parts, 150-200 parts, 200-250 parts, 250-300 parts, 300-350 parts; typical but non-limiting, for example, 20 parts, 50 parts, 80 parts, 130 parts, 170 parts, 240 parts, 290 parts, 320 parts, 350 parts.

[0033] In some specific embodiments of the present invention, the weight proportion of the desulfurized gypsum can be 0-10 parts, 10-20 parts, 20-30 parts; typically but not limiting, for example, 10 parts, 16 parts, 25 parts, 30 parts.

[0034] In some specific embodiments of the present invention, the weight proportion of the sodium silicate can be 0-1 parts, 1-2 parts, 2-3 parts, 3-4 parts; typically but not limiting, for example, 1 part, 1.5 parts, 2 parts, 3 parts.

[0035] In some embodiments of the invention:

[0036] 1) The particle size of the recycled building aggregate is 5-15 mm;

[0037] 2) The moisture content of the desulfurized gypsum is ≤3%;

[0038] 3) The modulus of the sodium silicate is 1.0-1.6.

[0039] In some specific embodiments of the present invention, the moisture content of the desulfurized gypsum may be 1-2%, 2-3%; typically but not limiting, for example, 1%, 2%, 3%.

[0040] In some specific embodiments of the present invention, the modulus of the sodium silicate may be 1.0-1.2, 1.2-1.3, 1.3-1.4, 1.4-1.5, 1.5-1.6; typically but not limiting, for example, 1.0, 1.2, 1.3, 1.4, 1.5, 1.6.

[0041] In some embodiments of the present invention, the electric furnace slag is blended with particle sizes of 0-1 mm, 1-5 mm and 5-20 mm.

[0042] The electric furnace steel slag with a particle size of 5-20 mm and the building recycled aggregate with a particle size of 5-15 mm play the role of a skeleton in concrete. The electric furnace steel slag with a particle size of 1-5 mm and the electric furnace steel slag with a particle size of 0-1 mm cooperate with each other and fill the pores in the concrete molding process, thereby reducing the porosity of the concrete and improving the compressive strength of the concrete.

[0043] In some embodiments of the present invention, the electric furnace slag is composed of particles with a diameter of 0-1 mm, a diameter of 1-5 mm, and a diameter of 5-20 mm in a mass ratio of (400-512): (710-830): (1150-1650).

[0044] In some embodiments of the invention:

[0045] a1) The apparent density of the electric furnace slag is ≥3600 kg / m 3 ;

[0046] a2) the particle size of the slag powder is less than 0.075 mm;

[0047] a3) The cement is silicate cement.

[0048] In some embodiments of the invention:

[0049] b1) the screening content of 5-15 mm particles in the electric furnace slag with a particle size of 5-20 mm is ≥ 85%;

[0050] b2) the screening content of particles <1mm in the electric furnace slag with a particle size of 1-5mm is less than 5%, and the screening content of particles >5mm is less than 5%;

[0051] b3) The screening content of particles with a diameter of 0-1 mm in the electric furnace slag>1 mm is less than 5%.

[0052] The second aspect of the present invention is to provide a method for preparing steel slag low-carbon concrete, comprising the following steps:

[0053] (1) Mixing slag powder, silica fume and cement to obtain a mixture 1;

[0054] (2) mixing the mixed material 1 obtained in step (1) with a portion of water to obtain a mixed material 2;

[0055] (3) mixing the mixed material 2 obtained in step (2) with electric furnace slag to obtain a mixed material 3;

[0056] (4) Mix the mixture obtained in step (3) with the remaining water and stir evenly to obtain a product.

[0057] The present invention, through the preparation method, is easy to match with the raw materials and raw material ratios of concrete, thereby reducing the carbon emission in the concrete and improving the performance of the concrete.

[0058] In some embodiments of the present invention, the preparation method further comprises:

[0059] (11) adding desulfurized gypsum in step (1);

[0060] (21) The amount of water added in step (2) is 1 / 3-2 / 3 of the total amount of water;

[0061] (31) adding recycled building aggregate in step (3);

[0062] (41) The mixing in step (4) does not exceed 3 minutes.

[0063] In some specific embodiments of the present invention, the mixing time in step (4) is 1-2 min, 2-3 min; typically but not limiting, for example, it can be 1 min, 2 min, 3 min.

[0064] In some specific embodiments of the present invention, the amount of water added in step (2) can be 1 / 3-5 / 12, 5 / 12-7 / 12, 7 / 12-2 / 3 of the total amount of water; typically but not limiting, for example, it can be 1 / 3, 5 / 12, 7 / 12, 2 / 3.

[0065] In some specific embodiments of the present invention, when the cement content is lower than 10% of the cementitious material, sodium silicate is added in step (1), and the solid content of the sodium silicate aqueous solution is 30-50%. The cementitious material is the mixture 1 corresponding to step (1).

[0066] In some specific embodiments of the present invention, the solid content of the sodium silicate aqueous solution can be 30-35%, 35-40%, 40-45%, 45-50%; typically but not limiting, for example, it can be 30%, 35%, 40%, 45%, 50%.

[0067] The present invention is further described below by way of examples, but the scope of the present invention is not limited thereto.

[0068] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. If specific conditions are not specified in the embodiment, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for all reagents or instruments, they are conventional products that can be purchased commercially. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any method, equipment, and material of the prior art similar or equivalent to the method, equipment, and material in the embodiments of the present invention can also be used to realize the present invention.

[0069] The building recycled aggregate of the present invention meets the Class I grade of GB / T 25177 "Recycled coarse aggregate for concrete" and has a particle size of 5-15 mm.

[0070] The slag powder of the present invention complies with the S95 grade of GB / T 18046 "Granulated blast furnace slag powder for cement, mortar and concrete".

[0071] The desulfurized gypsum of the present invention complies with GB / T 21371 "Industrial by-product gypsum used in cement".

[0072] The silica fume of the present invention complies with the SF90 grade of GB / T 27690 "Silica fume for mortar and concrete".

[0073] The screening content of particles with a diameter of 5-15 mm in the electric furnace steel slag of the present invention is greater than 85%; the screening content of particles with a diameter of 1-5 mm in the electric furnace steel slag of less than 1 mm is less than 5%, and the screening content of particles with a diameter of >5 mm is less than 5%; the screening content of particles with a diameter of 0-1 mm in the electric furnace steel slag of more than 1 mm is less than 5%.

[0074] Table 1 Ratio of raw material components of concrete of Examples 1-4 and Comparative Examples 1-2

[0075] Raw material kg Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Electric furnace slag (5-20mm) 1200 1600 1600 1600 / / Electric furnace slag (1-5mm) 740 740 740 740 / / Electric furnace slag (0-1mm) 460 460 460 320 / / Recycled aggregates for construction 350 / / / / / Slag powder 200 200 300 320 / / Desulfurization gypsum 30 30 5 / / / cement 120 120 35 20 400 400 water 200 200 193 181 180 188 Silica Fume 50 50 60 70 / / Sodium silicate / / 2.5 4 / / Stone / / / / 1300 1400 yellow sand / / / / 550 500

[0076] Example 1

[0077] The steel slag low-carbon concrete of this embodiment has a raw material composition ratio as shown in Table 1. Among them, the building recycled aggregate comes from Xinwei Holding Group, with a particle size of 5-15mm; the desulfurized gypsum comes from Guizhou Zongyi Environmental Protection Technology Co., Ltd., with a moisture content of ≤3%; the sodium silicate comes from Shandong Lianke Technology Co., Ltd., with a modulus of 1.4; the electric furnace slag comes from Baoshan Iron and Steel, with an apparent density of ≥3600kg / m 3The slag powder comes from Shanghai Baotian New Building Materials Co., Ltd., and its particle size is less than 0.075 mm; the cement comes from Anhui Conch Cement Co., Ltd., and is ordinary silicate P.O42.5 cement; the screening content of 5-15 mm in the electric furnace slag with a particle size of 5-20 mm is 85%.

[0078] The method for preparing the steel slag low-carbon concrete of this embodiment comprises the following steps:

[0079] (1) mixing slag powder, silica fume, cement and desulfurized gypsum in a concrete mixer to obtain a mixture 1;

[0080] (2) Mixing the mixed material 1 obtained in step (1) and part of the water in a mixer to obtain a mixed material 2; wherein the amount of the part of the water added is 1 / 3 of the total amount of the water;

[0081] (3) Mixing the mixture 2 obtained in step (2) with electric furnace slag and building recycled aggregate in a mixer and stirring for 2 minutes to obtain a mixture 3;

[0082] (4) Mix the mixture obtained in step (3) with the remaining water and stir for 2 minutes.

[0083] Example 2

[0084] The steel slag low-carbon concrete of this embodiment has a raw material composition ratio as shown in Table 1. The difference from Example 1 is that no building recycled aggregate is added, and the amount of electric furnace steel slag (5-20 mm) added is different from that in Example 1.

[0085] The method for preparing the steel slag low-carbon concrete of this embodiment comprises the following steps:

[0086] (1) mixing slag powder, silica fume, cement and desulfurized gypsum in a concrete mixer to obtain a mixture 1;

[0087] (2) Mixing the mixed material 1 obtained in step (1) and part of the water in a mixer to obtain mixed material 2; wherein the amount of the part of the water added is 1 / 3 of the total amount of the water;

[0088] (3) Mixing the mixed material 2 obtained in step (2) with electric furnace steel slag in a mixer and stirring for 2 minutes to obtain a mixed material 3;

[0089] (4) Mix the mixture obtained in step (3) with the remaining water and stir for 2 minutes.

[0090] Example 3

[0091] The steel slag low-carbon concrete of this embodiment has a raw material composition ratio as shown in Table 1. The difference from Embodiment 1 is that sodium silicate is added and the composition ratios of the raw material components are different.

[0092] The method for preparing the steel slag low-carbon concrete of this embodiment comprises the following steps:

[0093] (1) mixing slag powder, silica fume, cement, desulfurized gypsum and sodium silicate in a concrete mixer to obtain a mixture 1; wherein the sodium silicate is an aqueous solution with a solid content of 40%;

[0094] (2) Mixing the mixed material 1 obtained in step (1) and part of the water in a mixer to obtain a mixed material 2; wherein the amount of the part of the water added is 1 / 3 of the total amount of the water;

[0095] (3) Mixing the mixed material 2 obtained in step (2) with electric furnace steel slag in a mixer and stirring for 2 minutes to obtain a mixed material 3;

[0096] (4) Mix the mixture obtained in step (3) with the remaining water and stir for 2 minutes.

[0097] Example 4

[0098] The steel slag low-carbon concrete of this embodiment has a raw material composition ratio as shown in Table 1. The difference from Embodiment 3 is that no desulfurized gypsum is added and the composition ratios of the raw material compositions are different.

[0099] The method for preparing the steel slag low-carbon concrete of this embodiment comprises the following steps:

[0100] (1) mixing slag powder, silica fume, cement and sodium silicate in a concrete mixer to obtain a mixture 1; wherein the sodium silicate is an aqueous solution with a solid content of 40%;

[0101] (2) Mixing the mixed material 1 obtained in step (1) and part of the water in a mixer to obtain a mixed material 2; wherein the amount of the part of the water added is 1 / 3 of the total amount of the water;

[0102] (3) Mixing the mixed material 2 obtained in step (2) with electric furnace steel slag in a mixer and stirring for 2 minutes to obtain a mixed material 3;

[0103] (4) Mix the mixture obtained in step (3) with the remaining water and stir for 2 minutes.

[0104] Comparative Example 1

[0105] The raw material composition ratio of the concrete of this comparative example is shown in Table 1. Among them, the yellow sand is medium sand with a particle size of 0.25-0.5mm; the particle size of the gravel is 5-20mm.

[0106] The preparation method of the concrete of this comparative example comprises the following steps: mixing and stirring water, cement, yellow sand and gravel to obtain the concrete.

[0107] Comparative Example 2

[0108] The concrete of this comparative example has a distribution ratio of raw material groups as shown in Table 1. The difference from comparative example 1 is that the sand ratio is different and the distribution ratio of each raw material group is different.

[0109] Performance Testing

[0110] Compressive strength performance test: The concrete prepared in Examples 1-4 and Comparative Examples 1-2 was tested for 7d and 28d compressive strength according to the test method in GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The compressive strength test results are shown in Table 2. The 28d compressive strength change rate is shown in Table 2. Figure 1 As shown, the 28d compressive strength change rate formula is as follows:

[0111] d%=(d 实施例x -d 对比例 ) / d 对比例 ×100%

[0112] Among them, d% is the change rate of compressive strength at 28 days, d 对比例 is the 28d compressive strength measured in the comparative example, d 对比例 =(d1+d2) / 2, d 实施例x The 28d compressive strength measured for different embodiments.

[0113] Porosity performance test: The porosity of the concrete prepared in Examples 1-4 and Comparative Examples 1-2 was tested by mercury intrusion porosimetry. The test results are shown in Table 2.

[0114] Carbon emission test: The concrete prepared in Examples 1-4 and Comparative Examples 1-2 was tested for carbon emission according to the test method in DB64 / T 1954-2023 "Calculation Method and Evaluation Standard for Carbon Emission of Concrete". The test results are shown in Table 2. The carbon emission change rate is shown in Table 2. Figure 1 As shown, the formula for the rate of change of carbon emissions is as follows:

[0115] c%=(c 实施例x -c 对比例 ) / c 对比例 ×100%

[0116] Among them, c% is the carbon emission change rate, c 对比例 is the carbon emission measured for the comparative example, c 对比例 =(c1+c2) / 2, c 实施例x Carbon emissions measured for different embodiments.

[0117] Table 2 Performance test results of steel slag low carbon concrete of Examples 1-4 and Comparative Examples 1-2

[0118] Serial number 7d compressive strength / MPa 28d compressive strength / MPa Porosity / % <![CDATA[Carbon emissions / (kg / m 3 )]]> Example 1 16.9 41.3 2.2 152 Example 2 17.1 45.7 1.9 122 Example 3 18.5 42.9 2.1 104 Example 4 15 40.7 2.4 89 Comparative Example 1 17.4 34.6 6.9 254 Comparative Example 2 16.5 32.2 6.2 253

[0119] Combined with Examples 1-4, and combined with Table 2 and Figure 1 It can be seen from the data that the 28d compressive strength of steel slag low-carbon concrete in Examples 1-4 exceeds that of ordinary concrete, and all reach the C40 level. Steel slag low-carbon concrete has a significant effect on carbon reduction, and can reduce carbon by more than 40% compared with ordinary concrete, and the highest carbon reduction can reach about 60%.

[0120] Combined with the embodiments and comparative examples, and combined with Table 2 and Figure 1 It can be seen from the data in that the 28d compressive strength of the concrete prepared in the embodiment is greater than the 28d compressive strength of the concrete prepared in the comparative example, the porosity of the concrete prepared in the embodiment is small, and the carbon emission is low. The difference between the embodiment and the comparative example is that the embodiment uses electric furnace steel slag and building recycled aggregate to replace the gravel and yellow sand in the comparative example, and at the same time, introduces slag powder, silica fume, and desulfurized gypsum to reduce the amount of cement added, so as to reduce the carbon emission in the concrete preparation process without reducing the strength of the concrete. In addition, steel slag and slag are relatively cheap as solid wastes in the metallurgical process, and can also reduce production costs while expanding the comprehensive utilization rate of steel slag and slag.

[0121] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A steel slag low-carbon concrete, characterized in that: The low-carbon concrete includes the following raw materials in parts by weight: 2260-2990 parts of electric furnace slag, 0-350 parts of building recycled aggregate, 200-320 parts of slag powder, 50-70 parts of silica fume, 0-30 parts of desulfurized gypsum, 10-120 parts of cement, 0-4 parts of sodium silicate, and 180-200 parts of water.

2. The steel slag low-carbon concrete according to claim 1, characterized in that: Also includes one or more of the following features: 1) The particle size of the recycled building aggregate is 5-15 mm; 2) The moisture content of the desulfurized gypsum is ≤3%; 3) The modulus of the sodium silicate is 1.0-1.

6.

3. The steel slag low-carbon concrete according to claim 1, characterized in that: The electric furnace slag is mixed with particle sizes of 0-1mm, 1-5mm and 5-20mm.

4. The steel slag low-carbon concrete according to claim 3, characterized in that: The electric furnace slag is composed of particle sizes of 0-1mm, 1-5mm and 5-20mm in the mass ratio of (400-512): (710-830): (1150-1650).

5. The steel slag low-carbon concrete according to claim 4, characterized in that: Also includes one or more of the following characteristics: a1) The apparent density of the electric furnace slag is ≥3600 kg / m 3 ; a2) the particle size of the slag powder is less than 0.075 mm; a3) The cement is ordinary Portland cement.

6. The steel slag low-carbon concrete according to claim 5, characterized in that: Also includes one or more of the following characteristics: b1) the screening content of 5-15 mm particles in the electric furnace slag with a particle size of 5-20 mm is ≥ 85%; b2) the screening content of particles <1mm in the electric furnace slag with a particle size of 1-5mm is less than 5%, and the screening content of particles >5mm is less than 5%; b3) The screening content of particles with a diameter of 0-1 mm in the electric furnace slag>1 mm is less than 5%.

7. A method for preparing steel slag low-carbon concrete according to any one of claims 1 to 6, characterized in that: The steps include: (1) mixing slag powder, silica fume and cement to obtain a mixture 1; (2) mixing the mixed material 1 obtained in step (1) with a portion of water to obtain a mixed material 2; (3) mixing the mixed material 2 obtained in step (2) with electric furnace slag to obtain a mixed material 3; (4) Mix the mixture obtained in step (3) with the remaining water and stir evenly to obtain a product.

8. The method for preparing steel slag low-carbon concrete according to claim 7, characterized in that: The preparation method also includes one or more of the following features: (11) adding desulfurized gypsum in step (1); (21) The amount of water added in step (2) is 1 / 3-2 / 3 of the total amount of water; (31) adding recycled building aggregate in step (3); (41) The mixing in step (4) does not exceed 3 minutes.

9. The method for preparing steel slag low-carbon concrete according to claim 8, characterized in that: When the cement content is lower than 10% of the cementitious material, sodium silicate is added in the step (1), and the solid content of the sodium silicate aqueous solution is 30-50%.

10. The method for preparing steel slag low-carbon concrete according to claim 8, characterized in that: The mixing and stirring time in step (3) is 2-3 minutes.

Citation Information

Patent Citations

  • Steel slag concrete

    CN107500635A

  • All-solid waste concrete taking hot-stewed converter steel slag as aggregate and preparation method of all-solid waste concrete

    CN113943142A

  • Low-carbon road concrete taking steel slag as aggregate and preparation method of low-carbon road concrete

    CN114591061A

  • AU2020101143A4