High-yield-ratio high-specific-strength aluminum rare earth alloy and preparation method thereof

By introducing Ce, Yb, Er and other rare earth elements into the Al-Mn-Mg-Zn base alloy, and through reasonable process processing, a multi-scale strengthening phase is formed, which solves the problem that existing aluminum alloys are difficult to meet high yield ratio and specific ratio at the same time. To solve the problem of strength, aluminum rare earth alloys with high yield-to-strength ratio and high specific strength have been achieved, which are suitable for industrial production.

CN118745542APending Publication Date: 2024-10-08CENT SOUTH UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410918191.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

It is difficult for existing aluminum alloys to meet the requirements of high yield ratio and specific strength at the same time, and there is also the problem of high cost of alloy raw materials.

Method used

Introduce Zn and rare earth elements Ce, Yb, and Er into the Al-Mn-Mg-Zn base alloy, adjust their proportions, and regulate the content and proportion of the main elements (Mg, Zn), aging treatment, soaking annealing, and rolling deformation. and solid solution treatment to form multi-scale strengthening phases to improve the yield ratio and specific strength of the alloy.

Benefits of technology

It is achieved that while maintaining high plastic toughness, the yield-to-strength ratio of the aluminum rare earth alloy is higher than 0.85, and the specific strength can reach 232.8kN·m/kg. The process operation is simple and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745542A_ABST
    Figure CN118745542A_ABST
Patent Text Reader

Abstract

The invention discloses a high-yield-ratio high-specific-strength aluminum rare earth alloy and a preparation method thereof. The alloy is prepared from the following components in percentage by mass: 4 to 6 percent of Mg, 2 to 4 percent of Zn, 0.05 to 0.3 percent of Zr, 0.05 to 0.3 percent of Mn, 0.01 to 0.2 percent of Ce, 0.01 to 0.2 percent of Yb, 0.01 to 0.2 percent of Er, 1 to 3 percent of Mg / Zn and the balance of Al and inevitable impurity elements. According to the invention, Zn and rare earth alloys Ce, Yb and Er are introduced into an Al-Mn-Mg-Zn base alloy, and the proportions of the Zn and the rare earth alloys Ce, Yb and Er are regulated and controlled, so that the aluminum rare earth alloy keeps high plasticity and toughness, the yield ratio is higher than 0.85, and compared with alloys with similar alloying degrees and alloying elements, the aluminum rare earth alloy also can keep higher specific strength. Meanwhile, the preparation method is simple and convenient in process operation, simple in step and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-yield ratio and high-specific-strength aluminum rare earth alloy and a preparation method thereof, and belongs to the technical field of aluminum alloy material preparation. Background Art

[0002] High-quality structural materials should have high specific strength and yield strength ratio to achieve the weight reduction requirements and excellent structural reliability of aerospace structural parts. Compared with commercial Al-Mg alloys, high-magnesium content Al-Mg-Zn-based alloys can not only significantly improve the alloy's aging hardening potential by precipitating T phase, but also significantly improve the alloy's yield strength ratio (ratio of yield strength to tensile strength), while maintaining high specific strength (ratio of tensile strength to density) and plastic processing capabilities. Although high-strength Al-Zn-Mg-Cu aluminum alloys have high specific strength (180-208MPa.cm 3 / g) and yield strength ratio, but compared with Al-Mg-Zn based alloys, it has a higher tendency to hot cracking and stress corrosion cracking. The existing Al-Li alloy has excellent specific strength (180~220MPa.cm 3 / g) and yield strength ratio, but the production cost is high. Therefore, low-cost age-hardened Al-Mg-Zn-based alloys may be a suitable choice to replace other lightweight structural materials in the future, but their specific strength and yield strength ratio need to be further improved, so that the yield strength ratio reaches that of Al-Zn-Mg-Cu alloys, and the specific strength reaches that of Al-Li alloys.

[0003] Grain refinement can simultaneously improve the specific strength and yield strength ratio of the material without damaging the plastic toughness of the material. In production, increasing the cooling rate of the ingot and micro-alloying are often used to refine the grains of the ingot. Adding certain rare earth elements to aluminum alloys can have a significant effect on grain refinement. Cerium is almost not dissolved in aluminum (less than 0.01at%) and the eutectic temperature (645℃) is close to the melting point of aluminum. A tetragonal structure Al is formed in the early stage of solidification. 11 Ce3 phase, as the nucleation point of grains, is affected by Al distributed along the grain boundaries during grain growth. 11 The addition of Ce to aluminum alloys has a significant effect of refining the grains due to the hindrance of Ce3 phase.

[0004] Some rare earth elements can precipitate dispersion-strengthened nanoparticles in aluminum alloys, obtain significant dispersion-strengthening effects, and further improve the strength of aluminum alloys without losing plastic toughness. For example, Sc can form a rare earth element of a coherent L12 structure nano-precipitation phase in aluminum alloys. For example, the Chinese patent CN116949307A provides an Al-Mg-Zn (-Sc) (-Zr) alloy containing rare earth Sc and a preparation method. Sc plays a role in refining grains in the alloy, produces a dispersion-strengthening effect, and promotes the precipitation of T phase, thereby further enhancing intergranular corrosion performance. Although the specific strength of the alloy can be improved by adding Sc to the alloy, the rare earth Sc is expensive, which limits its application in production, and the patent must contain Cu, Sc and Zr at the same time to enhance the strength of the alloy by solid solution strengthening, and multiple deformation heat treatments are required, and the process is cumbersome. Most importantly, the technical solution cannot simultaneously improve the specific strength of the alloy. Summary of the invention

[0005] In view of the problems that aluminum alloys in the prior art cannot simultaneously meet the requirements of yield ratio and specific strength, and the high cost of alloy raw materials, the first object of the present invention is to provide a high yield ratio and high specific strength aluminum rare earth alloy. The present invention introduces Zn and rare earth alloys Ce, Yb, and Er into the Al-Mn-Mg-Zn basic alloy, and adjusts their proportions at the same time, so that the aluminum rare earth alloy has a yield ratio higher than 0.85 while maintaining high plastic toughness, and can also maintain a higher specific strength compared with alloys with similar alloying degrees and alloying elements.

[0006] The second object of the present invention is to provide a high specific strength aluminum rare earth alloy with a high yield ratio. The method has simple process operation and steps and is suitable for industrial production.

[0007] In order to achieve the above technical objectives, the present invention provides a high specific strength aluminum rare earth alloy with a high yield ratio, which includes the following components in mass percentage: Mg 4-6%, Zn 2-4%, Zr 0.05-0.3%, Mn 0.05-0.3%, Ce0.01-0.2%, Yb 0.01-0.2%, Er 0.01-0.2%, Mg / Zn 1-3, and the balance is Al and unavoidable impurity elements.

[0008] The key to the technical solution of the present invention is to obtain the solid solution strengthening effect of Mg and Zn elements by adjusting the content and ratio of the main elements (Mg, Zn), and to obtain the T phase (Mg phase) during the aging treatment. 32 (Al, Zn) 49) structure; adding trace strengthening elements (Mn, Zr), while obtaining the solid solution strengthening effect of Mn and Zr elements, forming Al3Zr nano-precipitation phase and Al6Mn submicron-level dispersion phase during ingot homogenization annealing, bringing dispersion strengthening effect; and adding rare earth elements (Ce, Yb, Er) at the same time, giving play to the role of rare earth elements in grain refinement in aluminum alloy, while obtaining fine grain structure, Yb and Er elements induce Al3Zr to precipitate in large quantities, forming L12 structure core-shell structure dispersion particles with Yb and Er in the inner layer and Zr in the outer layer, further strengthening the alloy, improving the specific strength, and obtaining multi-scale strengthening phases in the alloy. Controlling Mg / Zn within 1 to 3 helps to obtain a suitable proportion of strengthening phase T phase and improve the strength of the alloy.

[0009] Further preferably, the following components are included by mass percentage: Mg 4-6%, Zn 2-4%, Zr0.15-0.2%, Mn 0.2-0.3%, Ce 0.1-0.15%, Yb 0.1-0.15%, Er 0.1-0.2%, Mg / Zn 1-1.5, and the balance is Al and unavoidable impurity elements. Within the further preferred range, the aluminum alloy of the present invention has the highest specific strength, yield strength ratio, tensile strength and yield strength.

[0010] Further preferably, the following components are included by mass percentage: Mg 4-6%, Zn 2-3%, Zr 0.1-0.2%, Mn 0.1-0.2%, Ce 0.01-0.2%, Yb 0.01-0.2%, Er 0.01-0.1%, Mg / Zn 1-1.7, and the balance is Al and unavoidable impurity elements. In the further preferred range, the aluminum alloy of the present invention has the highest elongation while maintaining a high yield strength ratio and specific strength.

[0011] The present invention also provides a method for preparing an aluminum rare earth alloy with high yield ratio and high specific strength. The method comprises the following steps: weighing raw materials according to the designed aluminum alloy component ratio; melting pure aluminum, pure magnesium, pure zinc, aluminum-manganese master alloy, aluminum-zirconium master alloy, aluminum-ytterbium master alloy and aluminum-erbium master alloy in a resistance furnace to obtain a melt; performing composite degassing and deslagging treatment on the melt and casting and forming the melt after standing the melt to obtain an ingot; and sequentially performing heat treatment, rolling deformation, solution treatment and aging treatment to obtain the ingot.

[0012] The present invention also requires a corresponding preparation method. The present invention firstly performs a heat treatment on the ingot to eliminate the ingot stress, reduce the dendrite segregation, and precipitate the Al6Mn submicron dispersed phase and the Al3Zr nanoprecipitated phase; then, by rolling, deformation strengthening is introduced into the alloy, and a fine deformation structure is obtained; the rolled alloy is subjected to a solid solution and quenching treatment to obtain a supersaturated solid solution of elements such as Mg and Zn, and finally, a T phase (Mg32 (Al, Zn) 49 ). In summary, the present invention obtains a multi-scale strengthening phase in the alloy through reasonable process conditions of melting process, soaking annealing process, deformation process, solution treatment and aging treatment.

[0013] As a preferred solution, the conditions of the soaking treatment are: the homogenization temperature is 450-490°C, and the holding time is 12-24 hours. At the soaking treatment temperature selected by the present invention, the ingot stress can be better eliminated, the dendrite segregation can be reduced, and the Al6Mn submicron dispersed phase and the Al3Zr nano-precipitated phase can be precipitated.

[0014] As a preferred solution, the rolling deformation is firstly hot-rolled and then annealed and cold-rolled; the conditions of hot-rolling are: the starting temperature is 400-450°C, the total deformation is 60-90%; the conditions of annealing are: the annealing temperature is 380-430°C, the annealing holding time is 0.5-5h; after annealing, the sheet is cold-rolled, and the total deformation of the cold-rolling is 50-90%. The rolling deformation process of the present invention can introduce deformation strengthening into the alloy and obtain fine deformation structure at the same time.

[0015] As a preferred solution, the solution treatment conditions are: temperature of 450-490°C, holding time of 0.5-5h, and water cooling to room temperature after solution treatment. Under the solution treatment conditions selected by the present invention, supersaturated solid solutions of elements such as Mg and Zn can be further obtained in the alloy.

[0016] As a preferred solution, the aging treatment is a double-stage aging treatment, the temperature of the first stage aging treatment is 70-100°C, the time is 24-72h, and the temperature of the second stage aging treatment is 120-160°C, the time is 12-50h. In the first stage aging process, a large amount of precipitated phase precursors are nucleated, and in the second stage aging process, the precursors evolve into T phase (Mg 32 (Al, Zn) 49 ).

[0017] As a preferred solution, argon gas is used in the degassing and deslagging treatment.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1) The present invention obtains the solid solution strengthening effect of Mg and Zn elements by adjusting the content and ratio of the main elements (Mg, Zn), and obtains the T phase (Mg 32 (Al, Zn) 49) structure; adding trace strengthening elements (Mn, Zr) to obtain the solid solution strengthening effect of Mn and Zr elements, while forming Al3Zr nano-precipitation phase and Al6Mn submicron dispersed phase during the homogenization annealing of the ingot, bringing about dispersion strengthening effect; adding rare earth elements (Ce, Yb, Er), giving play to the role of rare earth elements in refining grains in aluminum alloys, obtaining fine-grained structure, while Yb and Er elements induce Al3Zr to precipitate in large quantities, forming L12 structure core-shell structure dispersed particles with Yb and Er in the inner layer and Zr in the outer layer, further strengthening the alloy and improving specific strength.

[0020] 2) The present invention obtains a multi-scale strengthening phase through reasonable smelting preparation process, soaking annealing process, deformation process, solution treatment and aging treatment process conditions, and finally obtains an aging-strengthened aluminum rare earth alloy, which has excellent specific strength and yield strength ratio while maintaining high plastic toughness (elongation after fracture ≥10%). The yield strength ratio of the obtained aluminum rare earth alloy is higher than 0.85, and the specific strength can reach 232.8kN·m / kg. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a TEM image of the aluminum rare earth alloy prepared in Example 1 of the present invention.

[0022] Figure 2 TEM image of the aluminum rare earth alloy prepared in Example 4 of the present invention.

[0023] Figure 3 TEM image of the aluminum rare earth alloy prepared in Example 8 of the present invention. DETAILED DESCRIPTION

[0024] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0025] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0026] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.

[0027] Example 1

[0028] The components of the alloy and their weight percentages are Al-4Mg-2Zn-0.3Zr-0.05Mn-0.01Ce-0.01Yb-0.01Er, and the Mg / Zn ratio is 2.

[0029] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-cerium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 450°C for 24 hours. The uniformly heated ingot is hot-rolled into a plate at 400°C with a total deformation of 90%. The plate is annealed at 430°C for 0.5h, and then cold-rolled into a thin plate with a total deformation of 90%. The thin plate alloy is kept at 490°C for 0.5h, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 70°C for 72h and 160°C for 12h for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0030] Example 2

[0031] The components of the alloy and their weight percentages are Al-6Mg-4Zn-0.3Zr-0.05Mn-0.01Ce-0.01Yb-0.1Er, and the Mg / Zn ratio is 1.5.

[0032] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-ytterbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 490°C for 12 hours. The uniformly heated ingot is hot-rolled into a plate at 450°C with a total deformation of 60%. The plate is annealed at 380°C for 5 hours, and then cold-rolled into a thin plate with a total deformation of 50%. The thin plate alloy is kept at 450°C for 5 hours, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 24 hours and 120°C for 50 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0033] Example 3

[0034] The alloy composition and weight percentage are Al-5.5Mg-3.5Zn-0.05Zr-0.3Mn-0.02Ce-0.02Yb-0.01Er. The Mg / Zn ratio is 1.6.

[0035] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-erbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 450°C for 24 hours. The uniformly heated ingot is hot-rolled into a plate at 430°C with a total deformation of 80%. The plate is annealed at 400°C for 2 hours, and then cold-rolled into a thin plate with a total deformation of 70%. The thin plate alloy is kept at 470°C for 2 hours, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 48 hours and 140°C for 20 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0036] Example 4

[0037] The components of the alloy and their weight percentages are Al-5Mg-3Zn-0.2Zr-0.2Mn-0.2Ce-0.05Yb-0.01Er, and the Mg / Zn ratio is 1.7.

[0038] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-cerium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. The uniformly heated ingot is hot-rolled into a plate at 430°C with a total deformation of 80%. The plate is annealed at 400°C for 2 hours, and then cold-rolled into a thin plate with a total deformation of 70%. The thin plate alloy is kept at 470°C for 2 hours, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 48 hours and 140°C for 20 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0039] Example 5

[0040] The components of the alloy and their weight percentages are Al-5Mg-3Zn-0.1Zr-0.1Mn-0.01Ce-0.2Yb-0.1Er, and the Mg / Zn ratio is 1.7.

[0041] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-ytterbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. The uniformly heated ingot is hot-rolled into a plate at 430°C with a total deformation of 80%. The plate is annealed at 400°C for 2 hours, and then cold-rolled into a thin plate with a total deformation of 70%. The thin plate alloy is kept at 470°C for 2 hours, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 48 hours and 140°C for 20 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0042] Example 6

[0043] The alloy's components and their weight percentages are Al-5Mg-3Zn-0.1Zr-0.15Mn-0.01Ce-0.1Yb-0.2Er, and the Mg / Zn ratio is 1.7.

[0044] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, and aluminum-erbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. The uniformly heated ingot is hot-rolled into a plate at 430°C with a total deformation of 80%. The plate is annealed at 400°C for 2 hours, and then cold-rolled into a thin plate with a total deformation of 70%. The thin plate alloy is kept at 470°C for 2 hours, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 48 hours and 140°C for 20 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0045] Example 7

[0046] The components of the alloy and their weight percentages are Al-4Mg-4Zn-0.2Zr-0.2Mn-0.1Ce-0.1Yb-0.1Er, and the Mg / Zn ratio is 1.

[0047] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum zirconium master alloy, aluminum manganese master alloy, aluminum cerium master alloy, aluminum ytterbium master alloy, and aluminum erbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 470℃ for 16h. The uniform heat ingot is hot rolled into a plate at 400℃ with a total deformation of 90%, and the plate is annealed at 430℃ for 0.5h, and then cold rolled into a thin plate with a total deformation of 90%. The thin plate alloy is kept at 490℃ for 0.5h, and after the solid solution treatment, it is water-cooled to room temperature, and then kept at 70℃ for 72h and 160℃ for 12h for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0048] Example 8

[0049] The alloy components and their weight percentages are Al-6Mg-4Zn-0.15Zr-0.2Mn-0.15Ce-0.15Yb-0.1Er, and the Mg / Zn ratio is 1.5.

[0050] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, aluminum-manganese master alloy, aluminum-cerium master alloy, aluminum-ytterbium master alloy, and aluminum-erbium master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and statically cast to form. The casting mold is a water-cooled iron mold. The ingot is subjected to a uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. The uniformly heated ingot is hot-rolled into a plate at 450°C with a total deformation of 60%, and the plate is annealed at 380°C for 5 hours, and then cold-rolled into a thin plate with a total deformation of 50%. The thin plate alloy is kept at 450°C for 5 hours. After the solution treatment, it is water-cooled to room temperature, and then kept at 100°C for 24 hours and 120°C for 50 hours for aging treatment to obtain a finished aluminum rare earth alloy. Its properties are shown in Table 1.

[0051] Comparative Example 1

[0052] The composition and weight percentage of the alloy are Al-6Mg-4Zn-0.15Zr-0.2Mn, and the Mg / Zn ratio is 1.5.

[0053] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, and aluminum-manganese master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is an iron mold preheated at 200°C. The ingot is subjected to uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. Then hot rolling and cold rolling are performed into thin plates. After the alloy is solution treated, it is water-cooled to room temperature, and then kept at 140°C for 32 hours for aging treatment to obtain a finished alloy. Its properties are shown in Table 1.

[0054] Comparative Example 2

[0055] The typical Al-Li series 1420 aluminum-lithium alloy is used, and its composition is Al-2.2Li-5.0Mg-0.1Zr. The raw materials are added in the form of pure aluminum, industrial pure magnesium, Al-10Mn and Al-4Zr alloy. The alloy is melted and cast in a vacuum melting furnace, and then hot rolled into a 5mm plate. After the alloy is solution treated, it is water quenched at room temperature and aged at 145℃ for 48h to obtain the finished alloy. The properties of the material are shown in Table 1.

[0056] Comparative Example 3

[0057] The typical 7085 aluminum-zinc-magnesium alloy of the Al-Zn-Mg-Cu system is used, and its composition is Al-7.5Zn-1.5Mg-1.6Cu-0.2Zr, and the Mg / Zn ratio is 0.2. The raw materials are added in the form of pure aluminum, industrial pure magnesium, pure zinc, Al-5Cu alloy and Al-4Zr alloy. The alloy is smelted in a resistance furnace and poured into an iron mold at a melt temperature of 720°C. The ingot is homogenized at 450°C for 24 hours, and then hot-rolled and cold-rolled into thin plates. After the alloy is solution treated, it is water quenched at room temperature and aged at 120°C for 24 hours to obtain the finished alloy. The properties of the material are shown in Table 1.

[0058] Comparative Example 4

[0059] The components of the alloy and their weight percentages are Al-3Mg-4Zn-0.15Zr-0.2Mn-0.1Yb-0.1Er-0.01Ce, and the Mg / Zn ratio is 0.8.

[0060] The preparation method is as follows: pure aluminum, pure magnesium, pure zinc, aluminum-zirconium master alloy, and aluminum-manganese master alloy are melted in a smelting furnace, degassed and deslaged by argon gas, and then statically cast and formed. The casting mold is an iron mold preheated at 200°C. The ingot is subjected to uniform heat treatment, and the uniform heat treatment process is: 470°C for 16 hours. Then hot rolling and cold rolling are performed into thin plates. After the alloy is solution treated, it is water-cooled to room temperature, and then kept at 140°C for 32 hours for aging treatment to obtain a finished alloy. Its properties are shown in Table 1.

[0061] The alloys prepared in Examples 1 to 8 and Comparative Examples 1 to 3 were tested for performance, and the results are shown in Table 1.

[0062] Table 1 Room temperature tensile properties of alloys prepared in Examples 1 to 8 and Comparative Examples 1 to 3

[0063]

[0064] By comparing the performance parameter values ​​of the embodiment and the comparative example, it can be seen that the aluminum alloy prepared by the present invention has significantly higher specific strength and yield strength ratio properties than the comparative example alloy when the alloying degree and alloying elements are similar.

Claims

1. A high specific strength aluminum rare earth alloy with high yield ratio, characterized in that: The invention comprises the following components in percentage by mass: Mg 4-6%, Zn 2-4%, Zr 0.05-0.3%, Mn 0.05-0.3%, Ce 0.01-0.2%, Yb 0.01-0.2%, Er 0.01-0.2%, Mg / Zn 1-3, and the balance is Al and unavoidable impurity elements.

2. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio as claimed in claim 1, characterized in that: Raw materials are weighed according to the designed aluminum alloy component ratio; pure aluminum, pure magnesium, pure zinc, aluminum-manganese master alloy, aluminum-zirconium master alloy, aluminum-ytterbium master alloy and aluminum-erbium master alloy are melted in a resistance furnace to obtain a melt; the melt is subjected to a composite degassing and deslagging treatment and then cast after being allowed to stand to obtain an ingot; the ingot is sequentially subjected to a heat treatment, rolling deformation, a solution treatment and an aging treatment to obtain the ingot.

3. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio according to claim 2, characterized in that: The conditions of the heat treatment are: the homogenization temperature is 450-490° C. and the heat preservation time is 12-24 hours.

4. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio according to claim 2 or 3, characterized in that: The rolling deformation is firstly processed by hot rolling and then annealing and cold rolling; The conditions of hot rolling treatment are: the starting rolling temperature is 400-450°C, the total deformation is 60-90%; Annealing conditions: annealing temperature is 380-430°C, annealing holding time is 0.5-5h; The total deformation amount of the cold rolling treatment is 50 to 90%.

5. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio according to claim 4, characterized in that: The conditions of the solution treatment are: a temperature of 450-490° C., a heat preservation time of 0.5-5 h, and after the solution treatment, water cooling to room temperature.

6. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio according to claim 5, characterized in that: The aging treatment is a double-stage aging treatment, wherein the temperature of the first stage aging treatment is 70-100° C., the time is 24-72 hours, and the temperature of the second stage aging treatment is 120-160° C., the time is 12-50 hours.

7. The method for preparing a high specific strength aluminum rare earth alloy with a high yield ratio according to claim 2, characterized in that: The degassing and deslagging treatment uses argon gas.

Citation Information

Cited By

  • High-strength and high-corrosion-resistance aluminum-magnesium alloy and preparation method thereof

    CN120967205A

  • Zinc-free magnesium-aluminum alloy and preparation method thereof

    CN122406046A

  • Zinc-free magnesium-aluminum alloy and method for producing the same

    CN122406046B