340MPa grade aluminum-silicon coating plated automobile steel and preparation method thereof
By designing the chemical composition and process of 340MPa grade aluminum-silicon coated automobile steel, combined with hot-dip aluminum-silicon heat treatment, the timeliness and cost problems of existing automobile outer panel steel have been solved, and the high strength and excellent mechanics of the steel plate have been achieved. performance and high surface quality.
Patent Information
- Application Number
- CN202410854210.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing steel for automobile exterior panels has natural aging problems in improving dent resistance and corrosion resistance. As zinc resources decrease, the cost of hot-dip galvanizing increases. It is necessary to develop a new type of steel that matches the heat treatment system of high-strength exterior panels. High quality coated steel for exterior panels.
340MPa grade aluminum-silicon coated automotive steel is used. Through reasonable design of chemical composition and production process, including smelting, hot rolling, pickling, cold rolling, and continuous annealing aluminum-silicon coating processes, ferrite and Ti(N,C ) precipitated phase and Cu-rich phase structure, combined with hot-dip aluminum-silicon heat treatment method, to achieve excellent mechanical properties and high surface quality of the steel plate.
The yield strength of the steel plate is 220~260MPa, the tensile strength is more than 340MPa, the elongation after fracture is more than 36%, the plastic strain ratio and strain hardening index are improved, and it has both excellent mechanical properties and high surface quality, reducing production costs and energy loss.
Smart Images

Figure CN118745552A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of automobile steel manufacturing, and in particular relates to a 340MPa grade aluminum-silicon coated automobile steel and a preparation method thereof. Background Art
[0002] The automobile industry is an important part of modern industry and has an important impact on my country's economic development. At the same time, automobiles are the main application of steel materials, of which the use of steel materials accounts for more than 60%. At present, the annual sales of automobiles exceed 26 million, and with the vigorous development of China's new energy vehicles, the automobile industry will continue to have an important impact on my country's steel industry. Among the steel used in automobiles, the steel used for automobile body outer panels is one of the most used steel materials. It is mainly used to manufacture parts such as the front, rear, left and right door outer panels, engine hood outer panels, and trunk lid outer panels of automobiles. The steel used for automobile outer panels should have excellent formability, corrosion resistance, dent resistance, and good weldability. Therefore, automobile outer panels generally use coated steel plates, and in order to improve dent resistance, the current automobile outer panels are mostly baked hardened (BH) steel plates and high-strength interstitial-free (IF) steels. BH steel uses interstitial solid solution atoms C to obtain partial strength improvement after baking paint (about 30MPa), but it also makes it have natural aging, which has an adverse effect on application. High-strength IF steel is made by adding microalloying elements to ultra-low carbon steel to ensure high strength and good formability through solid solution, precipitation or fine grain strengthening. In order to meet the requirements of corrosion resistance of automobile outer panels, the surface coating of the outer panels is currently mainly hot-dip galvanizing and alloy galvanizing. However, with the reduction of zinc resources and the increasing price, it is very necessary to develop a new type of high-quality coated outer panel steel that matches the heat treatment system of high-strength outer panels. Summary of the invention
[0003] The present invention provides a 340MPa grade aluminum-silicon coated automobile steel and a preparation method thereof. Through the reasonable design of the production process and the aluminum-silicon plating solution, a 340MPa grade automobile outer panel steel with both excellent mechanical properties and high surface quality is achieved.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The chemical composition of the substrate of 340MPa grade aluminum-silicon coated automobile steel is calculated by weight percentage as follows: C 0.003%~0.006%, Mn 0.3%~0.5%, P 0.03%~0.05%, Si 0.01%~0.03%, Ti 0.02%~0.05%, Cu 0.2%~0.4%, N≤0.002%, S≤0.005%, and the balance is Fe and unavoidable impurities.
[0006] The steel plate has a yield strength of 220 to 260 MPa, a tensile strength of 340 MPa or more, an elongation after fracture of 36% or more, a plastic strain ratio r of 2.0 or more, and a strain hardening exponent n of 0.2 or more.
[0007] The steel plate structure consists of ferrite, Ti(N,C) precipitation phase and Cu-rich phase.
[0008] The reasons for the alloy design of the present invention are as follows:
[0009] C: C is an important additive element in the present invention. When the C content increases, too much carbide and cementite are easily generated in the steel, which seriously affects the elongation, r value and n value of the steel. At the same time, too high a solid solution C content in the finished steel will cause serious aging problems in the steel, causing a rapid decrease in plasticity, thereby affecting the stamping and use of the steel plate. At the same time, when the C content is too low, the steelmaking cost is increased, and it cannot be guaranteed that a certain amount of carbides are formed in the steel, thereby making the precipitation strengthening weaker and causing the strength of the steel plate to be too low. Therefore, in order to ensure the comprehensive mechanical properties of the steel plate, the present invention requires that the C content be 0.003% to 0.006%.
[0010] Mn: Mn is one of the important elements in the present invention, and plays a role in solid solution strengthening to improve the strength of the steel plate. However, when excessive Mn is added, the plasticity of the steel plate is reduced and the formability is affected. Therefore, the present invention requires that the Mn content is 0.3% to 0.5%.
[0011] P: P is also a strengthening element, which improves the strength of the steel plate by solid solution strengthening. However, excessive P makes the strength of the steel plate too high, and the element is prone to grain boundary segregation, thereby reducing the plasticity of the steel plate and affecting its formability. Therefore, the present invention requires that the P element content is 0.03% to 0.05%.
[0012] Si: Si element can play a role in solid solution strengthening and ensure the strength of the steel plate, but too high Si element will easily reduce the plasticity and toughness of the steel plate. Therefore, the present invention requires that the Si content is 0.01% to 0.03%.
[0013] Ti: Ti is one of the important elements of the present invention. Ti mainly forms Ti(N,C) precipitates to fix the interstitial atoms N and C in the steel, thereby greatly improving the plasticity and formability of the steel plate. However, excessive Ti will cause the precipitation of FeTiP phase in the steel, which is not conducive to the formation of a favorable γ texture ( <111> / / ND), which seriously reduces the r value of the steel plate. At the same time, excessive addition of Ti elements also has the effect of solid solution strengthening, which will increase the strength of the steel plate and reduce the plasticity. Therefore, the present invention requires that the Ti content is 0.02% to 0.05%.
[0014] Cu: Cu is one of the important elements in the present invention. Cu does not react with elements such as C and N in steel. It and Fe are easy to exist in the form of Cu-rich phase in the aging stage of the steel plate, which plays a role in precipitation strengthening. The limited content of Cu makes the ferrite matrix in the steel distribute nano-scale Cu-rich phase, which can ensure the strength of the steel plate. Therefore, the present invention requires that the content of Cu is 0.2% to 0.4%.
[0015] N: N is an impurity element in steel. Its presence in the form of interstitial solid solution atoms will seriously affect the plasticity and toughness of the steel plate, while causing the aging of the steel plate and being unfavorable for improving the r value. Therefore, the present invention requires that the N element content is ≤ 0.002%.
[0016] S: S is an impurity element in steel, which easily reacts with Mn to form MnS, which deteriorates the performance of the steel plate, so its content is required to be as low as possible. Therefore, the present invention requires that the S element content is ≤ 0.005%.
[0017] A method for preparing 340MPa grade aluminum-silicon coated automobile steel, comprising smelting, hot rolling, pickling, cold rolling, continuous annealing aluminum-silicon coating, and skin-finishing processes;
[0018] Smelting: Smelting is performed in a converter and refining is performed in an RH refining furnace to obtain an alloy composition within the above range, and then casting into a casting billet.
[0019] The hot rolling process comprises the following method:
[0020] 1) The heating temperature is between 1250 and 1300°C, and the furnace time is ≥120 minutes. When the heating temperature is greater than 1250°C, the Ti element added to the steel can fix the N element and completely precipitate TiN. However, when the temperature exceeds 1300°C, the austenite grains will grow excessively, affecting the final strength of the steel plate. A heating time of ≥120 minutes can ensure uniform distribution of alloy elements.
[0021] 2) The starting rolling temperature is between 1100 and 1150°C, and the final rolling temperature is ≥890°C to ensure that the steel plate is rolled in the austenite single phase range to avoid the occurrence of mixed crystals.
[0022] 3) The coiling temperature is between 650 and 750°C to ensure the precipitation of Ti-containing carbides and eliminate interstitial C atoms in the steel, thereby ensuring the plasticity of the steel plate.
[0023] The thickness of hot rolled plate is between 3 and 4 mm.
[0024] Pickling: The iron scale oxide on the steel surface after hot rolling is removed by pickling to ensure the surface quality of the cold rolled sheet.
[0025] The cold rolling process: the cold rolling reduction rate is controlled at 75% to 85%. It is ensured that the cold rolling deformation energy storage provides sufficient driving force for the subsequent annealing recrystallization, so that the recrystallization is fully completed and the final microstructure is refined, and the steel plate has a strong γ texture, so that the steel plate has good plasticity and forming ability. Too high rolling reduction rate will increase the load of the cold rolling mill and cannot ensure the realization of the target thickness.
[0026] The continuous annealing aluminum silicon plating process comprises the following method:
[0027] 1) The annealing isothermal temperature is 830-870°C and the annealing time is 30-60s to ensure that the recrystallization behavior of the cold-rolled deformed structure occurs fully and a strong γ texture is formed to obtain good forming performance.
[0028] 2) The slow cooling rate is 2-10°C / s, the slow cooling temperature is 600-720°C, and the slow cooling isothermal time is 10-20s. The isothermal temperature and time ensure the formation of Cu-rich phase in the steel plate, which is dispersed in the matrix phase and promotes the strength of the steel plate.
[0029] 3) Aluminum-silicon plating: After the steel plate is isothermally cooled at the slow cooling temperature, the temperature of the aluminum-silicon plating solution is 600-720°C, and the slow cooling temperature difference between the aluminum-silicon plating solution and the steel plate is required to be ≤10°C, and the aluminum-silicon plating time is 3-10s. This limited aluminum-silicon plating temperature can ensure the fluidity of the aluminum-silicon plating solution, and at the same time, the temperature further promotes the formation of Cu-rich phase in the steel, thereby ensuring the strength of the steel plate. At the same time, the slow cooling temperature difference between the aluminum-silicon plating solution and the steel plate in this range prevents the aluminum-silicon plating solution temperature from fluctuating significantly, avoiding the generation of Fe-Al alloy particles caused by temperature fluctuations in the plating solution, which affects the coating quality of the steel plate.
[0030] 4) After aluminum silicon plating, the steel plate continues to cool down to room temperature at a rapid cooling rate of ≥20℃ / s. The high cooling rate can control the growth of branch crystals in the coating, thereby obtaining fine coating grains and improving the quality of the coating.
[0031] Finally, the steel plate enters the skin-pass mill for plate shape adjustment, and the skin-pass elongation is controlled at 0.5% to 1.0%, which can effectively eliminate the yield platform of the material and ensure the surface quality of the steel plate.
[0032] The composition of the aluminum-silicon plating liquid is calculated by mass percentage as follows: Si 8% to 12%, Fe ≤ 2%, and the rest is Al. This content of Si can effectively improve the fluidity of the plating solution, and Si can preferentially react with Fe on the surface of the steel plate to form Fe-Si phase, which can effectively prevent Fe-Al from generating brittle Fe-Al phase and improve the adhesion of the coating. The Fe in the plating solution comes from the steel plate. When it exceeds 2%, it is easy to react with Al within the aluminum-silicon plating temperature range. The reactants are suspended in the plating solution in the form of particles. When the particles adhere to the surface of the steel plate, it causes leakage plating, affecting the coating quality of the steel plate.
[0033] The final microstructure of the steel plate of the present invention is ferrite, Ti (N, C) precipitation phase and Cu-rich phase. The surface of the steel plate is an aluminum silicon coating. Through the above-mentioned novel heat treatment method combined with hot-dip aluminum silicon, the yield strength of the aluminum silicon-coated automobile steel can be obtained to be between 220 and 260 MPa, the tensile strength is above 340 MPa, the elongation after fracture is greater than 36%, the plastic strain ratio r is greater than 2.0, and the strain hardening index n is greater than 0.2, while achieving the characteristics of good mechanical properties and high surface quality without crystal flowers for automobile outer panels.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1) The chemical composition of the steel plate of the present invention is mainly C, Mn, P, Ti, and Cu as the main elements, and no expensive alloy elements are added, so the alloy cost of the steel plate is controlled. At the same time, a reasonable production process is adopted to control the precipitation of precipitates and obtain a strong γ texture, so that the steel plate has excellent strength, plasticity and formability.
[0036] 2) The present invention skillfully combines hot-dip aluminum silicon with heat treatment of steel plates, places the coating process in the slow cooling stage, and realizes the production of steel plate coating without affecting the mechanical properties of the steel plates, which helps to reduce energy loss in the production process.
[0037] 3) The present invention is based on a reasonable low-cost alloy composition design and adopts a new method combining an aluminum-silicon coating process with a heat treatment to achieve 340MPa grade automotive steel with excellent strength, plasticity, formability and high surface quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is the microstructure diagram of the steel plate. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with embodiments. The following embodiments are used to specifically illustrate the contents of the present invention. These embodiments are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.
[0040] Table 1 lists the chemical composition of the example steel, Table 2 lists the process parameters of hot rolling and cold rolling of the example steel, Table 3 lists the process parameters of continuous annealing of the example steel, and Table 4 gives the mechanical properties of the example steel.
[0041] Table 1 Chemical composition of the example steel, wt%
[0042] No. C Mn P Si Ti Cu N S 1 0.0045 0.42 0.039 0.024 0.038 0.23 0.0017 0.0027 2 0.0037 0.37 0.042 0.019 0.040 0.39 0.0014 0.0043 3 0.0052 0.47 0.035 0.028 0.047 0.32 0.0012 0.0036 4 0.0057 0.39 0.048 0.017 0.045 0.28 0.0018 0.0046 5 0.0047 0.48 0.032 0.026 0.039 0.38 0.0015 0.0021 6 0.0036 0.50 0.037 0.015 0.041 0.23 0.0010 0.0027 7 0.0059 0.35 0.049 0.024 0.049 0.29 0.0016 0.0018 8 0.0042 0.43 0.047 0.027 0.048 0.36 0.0009 0.0032
[0043] Table 2 Hot rolling and cold rolling process of example steel
[0044]
[0045] Table 3 Example steel annealing and aluminum silicon plating process
[0046]
[0047] Table 4 Mechanical properties and surface quality of example steel
[0048] Example <![CDATA[R p0.2 / MPa]]> <![CDATA[R m / MPa]]> <![CDATA[A 50 / %]]> Plastic strain ratio r Strain hardening exponent n Surface quality 1 238 345 38 2.4 0.23 Crystalless Flower 2 245 350 37 2.3 0.25 Crystalless Flower 3 227 348 39 2.4 0.21 Crystalless Flower 4 232 358 38 2.2 0.22 Crystalless Flower 5 245 360 36 2.5 0.24 Crystalless Flower 6 253 364 37 2.1 0.23 Crystalless Flower 7 246 356 39 2.5 0.22 Crystalless Flower 8 235 348 40 2.2 0.21 Crystalless Flower
[0049] It can be seen from the above embodiments that through low-cost component design and the ingenious combination of heat treatment and aluminum-silicon plating processes, a hot-dip aluminum-silicon automobile outer panel is prepared, whose yield strength is above 220MPa, tensile strength is above 340MPa, and elongation is greater than 36%, achieving the performance of strong plasticity, formability and high surface quality of the automobile outer panel.
Claims
1. 340MPa grade aluminum-silicon coated automotive steel, It is characterized in that The chemical composition of the substrate is calculated by weight percentage as follows: C 0.003% to 0.006%, Mn 0.3% to 0.5%, P 0.03% to 0.05%, Si 0.01% to 0.03%, Ti 0.02% to 0.05%, Cu 0.2% to 0.4%, N≤0.002%, S≤0.005%, and the balance is Fe and unavoidable impurities.
2. The 340MPa grade aluminum-silicon coated automobile steel according to claim 1, It is characterized in that The steel plate has a yield strength of 220 to 260 MPa, a tensile strength of 340 MPa or more, an elongation after fracture of 36% or more, a plastic strain ratio r of 2.0 or more, and a strain hardening exponent n of 0.2 or more.
3. The 340MPa grade aluminum-silicon coated automobile steel according to claim 1, It is characterized in that The steel plate structure consists of ferrite, Ti(N,C) precipitation phase and Cu-rich phase.
4. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to any one of claims 1 to 3, It is characterized in that It includes smelting, hot rolling, pickling, cold rolling, continuous annealing aluminum silicon plating, and finishing processes; the continuous annealing aluminum silicon plating process includes the following methods: 1) The annealing isothermal temperature is 830-870°C and the annealing time is 30-60s; 2) The slow cooling rate is 2-10°C / s, the slow cooling temperature is 600-720°C, and the slow cooling isothermal time is 10-20s; 3) Aluminum-silicon plating: After the steel plate is isothermal at the slow cooling temperature, it enters the aluminum-silicon plating solution. The temperature difference between the aluminum-silicon plating solution and the steel plate slow cooling temperature is ≤10°C, and the aluminum-silicon plating time is 3 to 10 seconds; 4) After aluminum-silicon coating, the steel plate continues to cool down to room temperature at a rapid cooling rate ≥20℃ / s.
5. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to claim 4, It is characterized in that The hot rolling process comprises the following method: 1) The heating temperature is between 1250 and 1300°C, and the furnace time is ≥ 120 minutes; 2) The starting rolling temperature is between 1100 and 1150°C, and the final rolling temperature is ≥890°C; 3) The coiling temperature is between 650 and 750°C.
6. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to claim 5, It is characterized in that The thickness of hot rolled plate is between 3 and 4 mm.
7. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to claim 4, It is characterized in that The cold rolling process: the cold rolling reduction rate is controlled at 75% to 85%.
8. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to claim 4, It is characterized in that The finishing process: the finishing elongation is controlled at 0.5% to 1.0%.
9. The method for preparing the 340MPa grade aluminum-silicon coated automobile steel according to claim 4, It is characterized in that The aluminum-silicon plating liquid has the following components in percentage by mass: Si 8% to 12%, Fe≤2%, and the rest Al.
Citation Information
Patent Citations
Ultra-high strength steel plate, preparation method thereof, and ultra-high strength steel plate product
CN108707823A
340 MPa-grade boron-containing high-strength high-toughness hot galvanizing structural steel and production method thereof
CN110819905A
Low temperature resistant hot-dip galvanized steel plate with excellent welding performance and production method thereof
CN111304543A
340MPa-grade alloyed hot galvanized plate for new energy automobile and preparation method thereof
CN117165845A
Hot dip galvanized steel sheet with high tensile strength and its production