Continuous casting round billet and preparation method and application thereof

By optimizing the elemental composition and preparation method of continuous cast round billets, the problem of insufficient impact energy and component segregation of wind power flange steel in low temperature environments has been solved, and wind power flange products with high impact energy and long life have been realized.

CN118745559APending Publication Date: 2024-10-08CHENGDE JIANLONG SPECIAL STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410624505.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing steel used for wind power flanges has insufficient impact power in low temperature environments, resulting in short service life and component segregation problems, making it difficult to meet the requirements for long-term use.

Method used

By optimizing the element composition and content ratio of the continuous cast round billet, increasing the contents of C, Mn, Cr and Mo, and combining the composite strengthening principle of V, Nb, Al and N elements, we can prepare a product with high impact energy and improved component segregation. Large-sized continuous casting round billets are used in the manufacture of wind power flanges.

Benefits of technology

It significantly increases the impact energy at -50°C to 180~200J, reduces the cross-sectional carbon segregation range, extends the service life of the wind power flange, simplifies the preparation process, and ensures the high quality and controllability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a continuous casting round billet as well as a preparation method and application thereof. The continuous casting round billet comprises the following components: 0.15 to 0.20 percent by weight of C, 1.40 to 1.70 percent by weight of Mn, 0.08 to 0.12 percent by weight of Cr, less than or equal to 0.10 percent by weight of Mo, less than or equal to 0.50 percent by weight of Ni, 0.02 to 0.05 percent by weight of Nb, 0.04 to 0.20 percent by weight of V, 0.020 to 0.040 percent by weight of Al, 0.20 to 0.50 percent by weight of Si, less than or equal to 0.015 percent by weight of P, less than or equal to 0.005 percent by weight of S, less than or equal to 0.0025 percent by weight of O, 0.006 to 0.012 percent by weight of N, less than or equal to 0.00015 percent by weight of H and the balance of Fe. According to the continuous casting round billet, by optimizing the element composition and the content ratio, the high impact toughness up to 180-200 J is achieved at the temperature of-50 DEG C, meanwhile, the cross section segregation phenomenon is effectively improved, and the service life of the continuous casting round billet used for a wind power flange is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and relates to a continuous casting round billet and a preparation method and application thereof, and in particular to a continuous casting round billet for a wind power flange and a preparation method thereof. Background Art

[0002] Wind turbine generator sets include towers, power equipment and blades that support the generator sets, and the power equipment includes battery charge controllers, inverters, unloaders, grid-connected controllers, battery packs, etc. At present, wind power equipment is mainly used in grasslands, mountains and seas, and the ambient temperature changes are very drastic. Since wind turbine flanges have the functions of fixing, supporting and sealing, they become important components for connecting the blades and towers of wind turbines. They are mainly divided into land-based wind turbine flanges and large wind turbine flanges for offshore use. When working, wind turbine flanges need to withstand large impact forces in various directions such as axial, lateral and longitudinal directions, which directly affects their service life. The design service life of steel for wind turbine flanges is generally 15 to 20 years, which requires the fatigue life of wind turbine flange products to reach 15 to 20 years. Impact energy is an important indicator for the inspection of wind turbine flange products. The value and stability of impact energy directly affect the service life of the final product. Therefore, it is of great significance to improve the low-temperature impact energy resistance of wind turbine flange products.

[0003] However, conventional steel for wind power flanges has small specifications and relatively small cross-sections of continuous casting round billets. The special restrictions of the composition and the segregation of the cross-sectional composition of the continuous casting round billets make the average impact energy at -50°C basically controlled above 50J after normal forging and heat treatment. The impact energy at individual points is as low as about 21J. The overall impact energy of the cross-section of the forging varies greatly, and the service life is short, which restricts the application prospects of wind power flange products. For this reason, people are committed to developing methods to improve the low-temperature impact performance of steel for wind power flanges.

[0004] CN114891947A discloses a method for improving the low-temperature impact performance of steel for wind power flanges, which mainly controls P≤0.110%, S≤0.030%, Si: 0.30-0.70% in the converter iron water, the converter iron water temperature is 1350-1450°C, the P content of the furnace molten steel is ≤0.012%, and the normalizing and tempering temperature time of the heat treatment process, to prepare steel for wind power flanges with a low-temperature impact energy of ≥70J at -50°C. However, the method still cannot meet the requirements for long-term use of wind power flanges in low-temperature environments, and there is still a lot of room for improvement.

[0005] CN114921720A discloses a steel ingot for flange of offshore high-power wind turbine and a production method thereof. The chemical composition of the steel ingot for flange includes C: 0.13-0.18%, Si: 0.15-0.35%, Mn: 1.30-1.50%, P≤0.015%, S≤0.005%, V: 0.02-0.06%, Al: 0.020-0.050%, Nb: 0.020-0.050%, H≤0.0002%, O≤0.0020% and N: 60-110ppm, As+Pb+Sb+Bi+Sn≤0.025%; however, the steel ingot for flange still has segregation phenomenon, and the maximum impact energy at low temperature of -50°C can only reach 72J, and the service life does not meet the standard.

[0006] Therefore, people are in urgent need of developing a large-size continuous casting round billet with strong low-temperature impact resistance and toughness and a preparation method thereof, which can significantly improve the cross-sectional component segregation phenomenon and increase the service life of wind turbine flanges, and has important research significance for the field of wind power generation. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a continuous casting round billet and a preparation method and application thereof, wherein the element composition and content ratio of the continuous casting round billet are optimized, and by adjusting the components, the impact energy thereof is as high as 180 to 200 J at -50°C, the extreme value of cross-sectional carbon segregation is ≤0.060%, and the cross-sectional component segregation phenomenon is improved; and the preparation process thereof is simple and controllable; and the continuous casting round billet has a long service life when used for wind power flanges.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In the first aspect, the present invention provides a continuous casting round billet, which comprises the following components: C: 0.15-0.20wt%, Mn: 1.40-1.70wt%, Cr: 0.08-0.12wt%, Mo≤0.10wt%, Ni≤0.50wt%, Nb: 0.02-0.05wt%, V: 0.04-0.20wt%, Al: 0.020-0.040wt%, Si: 0.20-0.50wt%, P≤0.015wt%, S≤0.005wt%, O≤0.0025wt%, N: 0.006-0.012wt%, H≤0.00015wt% and the balance Fe.

[0010] The content of each element can be selected as follows: C: 0.15-0.20wt%, for example, 0.15wt%, 0.16wt%, 0.17wt%, 0.18wt%, 0.19wt% or 0.20wt%; Mn: 1.40-1.70wt%, for example, 1.40wt%, 1.45wt%, 1.50wt%, 1.55wt%, 1.60wt%, 1.65wt% or 1.70wt%; Cr: 0.08-0.12wt%, for example, 0.08wt%, 0.085wt%, 0.09wt%, 0.095wt%, 0.10wt%, 0.105wt%, 0.11wt%, 0.115 wt% or 0.12wt%; Mo≤0.10wt%, for example, it can be 0.10wt%, 0.09wt%, 0.08wt%, 0.07wt%, 0.06wt% or 0.05wt%; Ni≤0.50wt%, for example, it can be 0.50wt%, 0.45wt%, 040wt%, 0.35wt%, 0.30wt%, 0.20wt% or 0.10wt%; Nb: 0.02-0.05wt%, for example, it can be 0.02wt%, 0.025wt%, 003wt%, 0.035wt%, 0.04wt%, 0.045wt% or 0.05wt%; V: 0.04-0.20wt%, for example, it can be 0.04 wt%, 0.06wt%, 0.08wt%, 0.10wt%, 0.12wt%, 0.14wt%, 0.16wt%, 0.18wt% or 0.20wt%; Al: 0.020-0.040wt%, for example, 0.020wt%, 0.025wt%, 0.030wt%, 0.035wt% or 0.040wt%; Si: 0.20-0.50wt%, for example, 0.20wt%, 0.25wt%, 0.30wt%, 0.35wt%, 0.40wt%, 0.45wt% or 0.50wt%; P≤0.015wt%, for example, 0.015wt%, 0.012wt%, 0.0 10wt%, 0.008wt% or 0.006wt%; S≤0.005wt%, for example, it can be 0.005wt%, 0.004wt%, 0.003wt%, 0.002wt% or 0.001wt%; O≤0.0025wt%, for example, it can be 0.0025wt%, 0.0022wt%, 0.0020wt% or 0.0018wt%; N: 0.006~0.012wt%, for example, it can be 0.006wt%, 0.008wt%, 0.010wt% or 0.012wt%; H≤0.00015wt%, for example, it can be 0.00015wt%, 0.00013wt% or 0.00010wt%.

[0011] The present invention optimizes the element composition and content ratio of the continuous casting round billet, improves the content ratio of C, Mn, Cr and Mo elements, combines the composite strengthening principle of four elements of V, Nb, Al and N, and adds specific contents of V, Nb, Al and N elements; the composite strengthening of the elements jointly strengthens the impact toughness of the obtained continuous casting round billet, and improves the segregation phenomenon of the element composition of the cross section; the continuous casting round billet obtained after optimizing the content ratio of each element has an impact energy of up to 180 to 200 J, and the extreme value of carbon segregation in the cross section is ≤0.060%, and the service life of the wind power flange is increased.

[0012] Preferably, the C content in the continuous casting round billet is 0.17-0.18wt%, for example, it can be 0.17wt%, 0.172wt%, 0.174wt%, 0.176wt%, 0.178wt% or 0.18wt%.

[0013] Preferably, the Mn content in the continuous casting round billet is 1.53-1.57wt%, for example, 1.53wt%, 1.54wt%, 1.55wt%, 1.56wt% or 1.57wt%.

[0014] Preferably, the Cr content in the continuous casting round billet is 0.09-0.11wt%, for example, it can be 0.09wt%, 0.095wt%, 0.010wt%, 0.0105wt% or 0.11wt%.

[0015] Preferably, the Ni content in the continuously cast round billet is ≤0.30wt%, for example, it may be 0.30wt%, 0.20wt% or 0.10wt%.

[0016] Preferably, the Nb content in the continuous casting round billet is 0.023-0.027wt%, for example, 0.023-0.20wt% or 0.10wt%.

[0017] Preferably, the V content in the continuous casting round billet is 0.045-0.050wt%, for example, it may be 0.045wt%, 0.0455wt% or 0.050wt%.

[0018] Preferably, the Al content in the continuous casting round billet is 0.025-0.035wt%, for example, it can be 0.025wt%, 0.0255wt%, 0.030wt% or 0.035wt%.

[0019] Preferably, the Si content in the continuous casting round billet is 0.28-0.32wt%, for example, 0.28wt%, 0.29wt%, 0.30wt%, 0.31wt% or 0.32wt%.

[0020] Preferably, the P content in the continuous casting round billet is ≤0.010wt%, for example, it may be 0.010wt%, 0.009wt%, 0.008wt% or 0.007wt%.

[0021] Preferably, the S content in the continuous casting round billet is ≤0.003wt%, for example, it may be 0.003wt%, 0.002wt% or 0.001wt%.

[0022] Preferably, the O content in the continuously cast round billet is ≤0.0012wt%, for example, it may be 0.0012wt%, 0.0010wt% or 0.0008wt%.

[0023] Preferably, the N content in the continuous casting round billet is 0.007-0.009wt%, for example, it may be 0.007wt%, 0.008wt% or 0.009wt%.

[0024] Preferably, the H content in the continuously cast round billet is ≤0.00012wt%, for example, it may be 0.00012wt%, 0.00010wt% or 0.00008wt%.

[0025] Preferably, the CEV in the continuous casting round billet ranges from 0.44 to 0.48wt%, for example, it can be 0.44wt%, 0.45wt%, 0.46wt%, 0.47wt% or 0.48wt%, preferably 0.45 to 0.47wt%; wherein CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, and the chemical symbols in the formula actually represent the mass percentage of the corresponding chemical elements.

[0026] The present invention further preferably has a CEV range of 0.44-0.48wt%, and the continuous casting round billet has excellent welding performance and is not prone to cracking; if the CEV is greater than 0.48wt%, the continuous casting round billet is prone to cracking during welding, and the welding performance deteriorates.

[0027] Preferably, the sum of the contents of Nb and V in the continuous casting round billet is 0.06-0.25wt%, for example, it can be 0.06wt%, 0.08wt%, 0.10wt%, 0.13wt%, 0.15wt%, 0.18wt%, 0.20wt%, 0.23wt% or 0.25wt%, preferably 0.068-0.077%.

[0028] Preferably, the sum of the contents of N and Al in the continuous casting round billet is 0.026-0.052wt%, for example, it may be 0.026wt%, 0.030wt%, 0.035wt%, 0.040wt%, 0.045wt%, 0.050wt% or 0.052wt%, preferably 0.032-0.044wt%.

[0029] The present invention further optimizes the sum of the contents of Nb and V in the continuous casting round billet to be 0.06-0.25wt%, and the sum of the contents of N and Al to be 0.026-0.052wt%, so that the composite strengthening effect of the four elements Nb, V, N and Al is better, and the impact toughness of the continuous casting round billet is improved; if the sum of the contents of Nb and V or the sum of the contents of N and Al is outside the range of the present invention, the composite strengthening effect between the four elements Nb, V, N and Al is deteriorated, the impact toughness cannot be improved, and the performance of the continuous casting round billet product finally obtained is deteriorated.

[0030] Preferably, the diameter of the continuously cast round billet is 700-1200 mm, for example, 700 mm, 800 mm, 900 mm, 1000 mm or 1200 mm.

[0031] In a second aspect, the present invention provides a method for preparing the continuously cast round billet as described in the first aspect, the preparation method comprising: continuously casting and cooling molten steel in sequence to obtain the continuously cast round billet.

[0032] The continuous casting round billet of the present invention can be obtained by directly continuous casting molten steel and then cooling it. The preparation process is simple and the continuous casting parameters are easy to control. A large-scale continuous casting round billet of 700-1200 mm resistant to low temperature can be prepared.

[0033] It is worth noting that the larger the size of the required continuous casting round billet, the larger the cross-sectional component segregation, which makes it difficult to control the surface and core quality of the continuous casting round billet. The present invention can reduce the cross-sectional component segregation phenomenon by controlling the parameters of the continuous casting process, and can successfully prepare large-sized continuous casting round billets of 700 to 1200 mm with a cross-sectional carbon content segregation extreme as low as less than 0.060%.

[0034] The method for preparing the molten steel comprises: selecting a steel ingot raw material according to the composition of the continuous casting round billet described in the first aspect, and sequentially subjecting the steel ingot raw material to KR desulfurization, converter smelting, ladle refining and vacuum refining to obtain the molten steel.

[0035] Preferably, the continuous casting is carried out in a continuous casting machine.

[0036] Preferably, the pulling speed during continuous casting is 0.08-0.32 m / min, for example, it can be 0.08 m / min, 0.10 m / min, 0.12 m / min, 0.15 m / min, 0.18 m / min, 0.20 m / min, 0.22 m / min, 0.24 m / min, 0.26 m / min, 0.28 m / min, 0.30 m / min or 0.32 m / min, preferably 0.18-0.32 m / min.

[0037] Preferably, the superheat during continuous casting is 15-35°C, for example, it can be 15°C, 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, 32°C or 35°C.

[0038] It is worth mentioning that superheat refers to the difference between the pouring temperature of molten steel during the process and the liquidus temperature.

[0039] The present invention further preferably sets the pulling speed during continuous casting to 0.08-0.32 m / min and the superheat to 15-35°C, which is beneficial to the uniform growth of the entire shell of the large-sized continuous casting round billet during the solidification process, the floating of inclusions, and the improvement of the surface and core quality of the continuous casting round billet; if the superheat during continuous casting is too low, it will lead to uneven growth of the shell during the relative solidification and crystallization process of the molten steel, which is not conducive to the floating of inclusions, and the low pulling speed will lead to surface stress cracks during the solidification process; if the superheat during continuous casting is too high, it will lead to poor surface fluidity of the continuous casting billet and uneven growth of the shell, and ultimately cause a large number of shrinkage holes and other quality defects in the continuous casting round billet during the solidification process; the high pulling speed will lead to uneven growth of the shell, which will easily increase the incidence of cracks in the casting billet, and in severe cases, steel leakage accidents will occur.

[0040] Preferably, the current of electromagnetic stirring of the crystallizer in the continuous casting machine is 280-380A, for example, it can be 280A, 300A, 320A, 340A, 360A or 380A.

[0041] Preferably, the frequency of the electromagnetic stirring of the crystallizer is 1.0-1.5 Hz, for example, 1.0 Hz, 1.1 Hz, 1.2 Hz, 1.3 Hz, 1.4 Hz or 1.5 Hz.

[0042] The present invention further preferably sets the current of the electromagnetic stirring of the crystallizer in the continuous casting machine to 280-380A and the frequency to 1.0-1.5Hz; this is beneficial to improving the uniformity of the liquid phase temperature, controlling the crystal size and morphology, promoting the self-assembly of the crystal, and adjusting the flow velocity and temperature distribution of the liquid phase inside the crystallizer, thereby optimizing the control of the crystal growth environment and improving the looseness and segregation of the center of the casting; if the current or frequency of the electromagnetic stirring of the crystallizer is not within the range described in the present invention, it will lead to severe looseness and segregation in the center of the casting, and the quality will be unqualified.

[0043] Preferably, the current for stirring the strand in the continuous casting machine is 55-75A, for example, 55A, 60A, 65A, 70A or 75A.

[0044] Preferably, the frequency of the strand stirring is 1.0 to 3.5 Hz, for example, 1.0 Hz, 1.5 Hz, 2.0 Hz, 2.5 Hz, 3.0 Hz or 3.5 Hz.

[0045] The present invention further preferably has a current of 55 to 75A and a frequency of 1.0 to 3.5 Hz for stirring the casting strand in the continuous casting machine; this is beneficial for breaking up the dendrite bridges in the liquid core and eliminating the central looseness and shrinkage cavities of the continuous casting round billet; the broken dendrite crystals serve as equiaxed crystal cores to expand the central equiaxed crystal area of ​​the continuous casting round billet, eliminate central segregation, promote the floating of inclusions in the liquid phase hole of the continuous casting round billet, and reduce the aggregation of inner arc inclusions; if the current or frequency of the casting strand stirring is not within the range described in the present invention, it will lead to central segregation of the continuous casting round billet, poor control of internal cracks and urgent inclusions, large quality fluctuations, and affect the use of downstream customers.

[0046] Preferably, the current of the terminal electromagnetic stirring in the continuous casting machine is 320-420A, for example, it can be 320A, 340A, 360A, 380A, 400A or 420A.

[0047] Preferably, the frequency of the terminal electromagnetic stirring is 1.0 to 3.5 Hz, for example, 1.0 Hz, 1.5 Hz, 2.0 Hz, 2.5 Hz, 3.0 Hz or 3.5 Hz.

[0048] The present invention further prefers that the current of the terminal electromagnetic stirring in the continuous casting machine is 320-420A and the frequency is 1.0-3.5Hz; this is beneficial to more stable control of the carbon extreme difference in the cross section of large-size continuous casting round billets and the macrostructure of continuous casting round billets, and stable quality; if the current or frequency of the terminal electromagnetic stirring is not within the range described in the present invention, it will lead to central segregation of the continuous casting round billet, central looseness of the macrostructure, shrinkage holes and other quality that cannot be guaranteed.

[0049] Preferably, the cooling method includes slow cooling in a pit.

[0050] Preferably, the pit entry temperature for slow cooling is ≥500°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C.

[0051] Preferably, the time for slow cooling in the pit is ≥120h, for example, it can be 120h, 125h, 130h, 135h or 140h.

[0052] Preferably, the exit temperature of the slow cooling in the pit is ≤250°C, for example, it can be 200°C, 210°C, 220°C, 230°C, 240°C or 250°C.

[0053] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0054] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.08-0.32 m / min, the superheat is 15-35°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 280-380A, the frequency is 1.0-1.5Hz, the current of the casting strand stirring in the continuous casting machine is 55-75A, the frequency is 1.0-3.5Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 320-420A, the frequency is 1.0-3.5Hz; then, the steel is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is ≥500°C, the time is ≥120h, and the pit exit temperature is ≤250°C, so as to finally obtain the continuously cast round billet.

[0055] In a third aspect, the present invention provides an application of the continuously cast round billet described in the first aspect, wherein the continuously cast round billet is used to prepare a wind power flange.

[0056] The continuously cast round billet provided by the present invention can be used to prepare wind power flanges, and the prepared wind power flanges have strong impact toughness and long service life.

[0057] Preferably, the impact energy of the wind turbine flange at -50°C is 120-200J, for example, 120J, 130J, 140J, 150J, 160J, 170J, 180J, 190J or 200J.

[0058] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] (1) The continuous casting round billet provided by the present invention optimizes its element composition and content ratio to increase the contents of C, Mn, Cr and Mo. At the same time, by utilizing the composite strengthening principle of V, Nb, Al and N elements, specific contents of V, Nb, Al and N are added, and the elements are compounded to enhance the impact toughness of the obtained continuous casting round billet, and the impact energy at -50°C is increased to 180-200J; at the same time, the cross-sectional component segregation phenomenon of the continuous casting round billet is significantly improved, and the extreme difference value of the cross-sectional carbon content segregation of the large-size continuous casting round billet with a diameter of 700-1200mm is as low as 0.060%.

[0061] (2) The present invention provides a method for preparing a continuously cast round billet. The method controls the pulling speed, superheat, current and frequency of electromagnetic stirring of the crystallizer, current and frequency of casting strand stirring, and current and frequency of terminal electromagnetic stirring during continuous casting, so that the prepared continuously cast round billet has excellent impact toughness. The method has a simple process and easy-to-control conditions.

[0062] (3) Application of the continuous casting round billet provided by the present invention. The continuous casting round billet can be used to prepare wind power flanges and can be used in a low temperature environment of -50°C. It has strong impact toughness and a long service life. DETAILED DESCRIPTION

[0063] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0064] The specific implementation method of the present invention provides a continuous casting round billet and a preparation method and application thereof, wherein the continuous casting round billet comprises the following components:

[0065] C: 0.15~0.20wt%, Mn: 1.40~1.70wt%, Cr: 0.08~0.12wt%, Mo≤0.10wt%, Ni≤0.50wt%, Nb: 0.02~0.05wt%, V: 0.04~0.20wt%, A l: 0.020~0.040wt%, Si: 0.20~0.50wt%, P≤0.015wt%, S≤0.005wt%, O≤0.0025wt%, N: 0.006~0.012wt%, H≤0.00015wt% and balance Fe.

[0066] 1. Implementation

[0067] Example 1

[0068] The present embodiment provides a continuous casting round billet and a preparation method thereof, wherein the continuous casting round billet comprises the following components: C: 0.18wt%, Mn: 1.55wt%, Cr: 0.10wt%, Mo: 0.08wt%, Ni: 0.3wt%, Nb: 0.024wt%, V: 0.048wt%, Al: 0.03wt%, Si: 0.35wt%, P: 0.010wt%, S: 0.003wt%, O: 0.0020wt%, N: 0.009wt%, H: 0.00010wt% and the balance Fe.

[0069] The preparation method comprises the following steps:

[0070] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.25m / min, the superheat is 25°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 330A, the frequency is 1.25Hz, the current of the casting strand stirring in the continuous casting machine is 65A, the frequency is 2.2Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 370A, the frequency is 2.2Hz; then it is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is 500°C, the time is 120h, and the pit exit temperature is 250°C, finally the continuously cast round billet is obtained.

[0071] The specification of the continuous casting round billet obtained in this embodiment is φ900mm.

[0072] Example 2

[0073] The present embodiment provides a continuous casting round billet and a preparation method thereof, wherein the continuous casting round billet comprises the following components: C: 0.19wt%, Mn: 1.60wt%, Cr: 0.09wt%, Mo: 0.09wt%, Ni: 0.40wt%, Nb: 0.04wt%, V: 0.15wt%, Al: 0.030wt%, Si: 0.40wt%, P: 0.014wt%, S: 0.003wt%, O: 0.0023wt%, N: 0.008wt%, H: 0.00012wt% and the balance Fe.

[0074] The preparation method comprises the following steps:

[0075] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.23m / min, the superheat is 28°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 350A, the frequency is 1.20Hz, the current of the casting strand stirring in the continuous casting machine is 70A, the frequency is 2.0Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 350A, the frequency is 2.0Hz; then it is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is 520°C, the time is 130h, and the pit exit temperature is 220°C, finally the continuously cast round billet is obtained.

[0076] The specification of the continuous casting round billet obtained in this embodiment is φ900mm.

[0077] Example 3

[0078] The present embodiment provides a continuous casting round billet and a preparation method thereof, wherein the continuous casting round billet comprises the following components: C: 0.15wt%, Mn: 1.4wt%, Cr: 0.08wt%, Mo: 0.06wt%, Ni: 0.3wt%, Nb: 0.02wt%, V: 0.04wt%, Al: 0.020wt%, Si: 0.20wt%, P: 0.008wt%, S: 0.003wt%, O: 0.0018wt%, N: 0.006wt%, H: 0.00008wt% and the balance Fe.

[0079] The preparation method comprises the following steps:

[0080] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.18 m / min, the superheat is 15°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 280A, the frequency is 1.0 Hz, the current of the casting strand stirring in the continuous casting machine is 55A, the frequency is 1.0 Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 320A, the frequency is 1.0 Hz; then it is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is 550°C, the time is 150h, and the pit exit temperature is 200°C, finally obtaining the continuously cast round billet.

[0081] The specification of the continuous casting round billet produced in this embodiment is φ700mm.

[0082] Example 4

[0083] The present embodiment provides a continuous casting round billet and a preparation method thereof, wherein the continuous casting round billet comprises the following components: C: 0.19wt%, Mn: 1.6wt%, Cr: 0.11wt%, Mo: 0.09wt%, Ni: 0.48wt%, Nb: 0.04wt%, V: 0.14wt%, Al: 0.032wt%, Si: 0.32wt%, P: 0.013wt%, S: 0.004wt%, O: 0.0022wt%, N: 0.010wt%, H: 0.00011wt% and the balance Fe.

[0084] The preparation method comprises the following steps:

[0085] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.28 m / min, the superheat is 30°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 320A, the frequency is 1.3Hz, the current of the casting strand stirring in the continuous casting machine is 70A, the frequency is 2.8Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 400A, and the frequency is 2.8Hz; then it is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is 530°C, the time is 130h, and the pit exit temperature is 180°C, finally the continuously cast round billet is obtained.

[0086] The specification of the continuous casting round billet produced in this embodiment is φ800mm.

[0087] Example 5

[0088] The present embodiment provides a continuous casting round billet and a preparation method thereof, wherein the continuous casting round billet comprises the following components: C: 0.20wt%, Mn: 1.70wt%, Cr: 0.12wt%, Mo: 0.10wt%, Ni: 0.50wt%, Nb: 0.05wt%, V: 0.20wt%, Al: 0.040wt%, Si: 0.50wt%, P: 0.015wt%, S: 0.005wt%, O: 0.0025wt%, N: 0.012wt%, H: 0.00015wt% and the balance Fe.

[0089] The preparation method comprises the following steps:

[0090] The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.32m / min, the superheat is 35°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 380A, the frequency is 1.5Hz, the current of the casting strand stirring in the continuous casting machine is 75A, the frequency is 3.5Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 420A, and the frequency is 3.5Hz; then it is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is 550°C, the time is 140h, and the pit exit temperature is 240°C, finally the continuously cast round billet is obtained.

[0091] The specification of the continuous casting round billet obtained in this embodiment is φ1200mm.

[0092] Example 6

[0093] This embodiment provides a continuous casting round billet and a preparation method thereof. The preparation method of the continuous casting round billet is the same as that of Embodiment 1 except that the drawing speed during the continuous casting is 0.15 m / min.

[0094] Example 7

[0095] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 260A, the rest is the same as that of Embodiment 1.

[0096] Example 8

[0097] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 400A, the rest is the same as that of Embodiment 1.

[0098] Example 9

[0099] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the frequency of the electromagnetic stirring of the crystallizer is 0.9 Hz, the rest is the same as that of Embodiment 1.

[0100] Example 10

[0101] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the frequency of the electromagnetic stirring of the crystallizer is 1.6 Hz, the rest is the same as that of Embodiment 1.

[0102] Embodiment 11

[0103] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current for stirring the casting strand is 50A, the rest is the same as that of Embodiment 1.

[0104] Example 12

[0105] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current for stirring the casting strand is 80A, the rest is the same as that of Embodiment 1.

[0106] Example 13

[0107] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current of the terminal electromagnetic stirring in the continuous casting machine is 300A, the rest is the same as that in Embodiment 1.

[0108] Embodiment 14

[0109] This embodiment provides a continuous casting round billet and a preparation method thereof. Except that the current of the terminal electromagnetic stirring in the continuous casting machine is 430A, the rest is the same as that in Embodiment 1.

[0110] Examples 15 to 19 and Comparative Examples 1 to 7 adjust the element composition and content ratio on the basis of Example 1, and the rest are the same as Example 1. The element composition and content ratio are shown in Table 1, the content of the unadjusted component is the same as that of Example 1, and the content of the adjusted component is adjusted correspondingly to the Fe content.

[0111] Table 1

[0112]

[0113]

[0114] 3. Test and its results

[0115] The impact energy (-50°C) of the continuous casting round billets provided in the above embodiments and comparative examples was tested with reference to EN 10025-3:2004 or GB / T1591-2008; and the extreme value of carbon segregation in the cross section of the continuous casting round billet was calculated by the difference between the maximum and minimum values ​​of the test results. The results are shown in Table 2.

[0116] Table 2

[0117]

[0118]

[0119] From Table 2, we can see that:

[0120] (1) It can be seen from Examples 1 to 5 that the present invention improves the impact toughness of the continuously cast round billet by regulating the element composition and content ratio of the continuously cast round billet, that is, increasing the content ratio of C, Mn, Cr and Mo, and adding specific contents of V, Nb, Al and N elements. The elements work together to improve the impact toughness of the continuously cast round billet. At -50°C, the impact energy is as high as 190J or more. The carbon content segregation extreme of the cross section of the continuously cast round billet is as low as 0.060% (700-1200mm) or less.

[0121] (2) It can be seen from Example 1 and Examples 6 to 14 that the present invention effectively improves the degree of cross-sectional component segregation of the continuously cast round billet by controlling the continuous casting conditions, including the pulling speed, superheat, and the current and frequency of the crystallizer electromagnetic stirring, the casting strand stirring and the end electromagnetic stirring within a specific range; when the continuous casting conditions are not within the preferred range of the present invention, the cross-sectional component segregation phenomenon of the obtained continuously cast round billet increases, and the impact energy at -50°C is also reduced compared to the impact energy when the continuous casting conditions are within the preferred range of the present invention.

[0122] (3) Based on Example 1 and Examples 15 to 19, it can be seen that the present invention further prefers the contents of C, Mn, Cr and Mo, the sum of the contents of Nb and V, and the sum of the contents of N and Al. The compounding of each element enhances the impact toughness of the obtained continuous casting round billet; and when any one of C, Mn, Cr and Mo or the sum of the contents of Nb and V and the sum of the contents of N and Al is outside the preferred range of the present invention, the impact performance of the continuous casting round billet is reduced, and the component segregation phenomenon in its cross section is also increased.

[0123] (4) Combining Example 1 with Comparative Examples 1 to 7, it can be seen that the impact energy of the continuously cast round billet described in Comparative Examples 1 to 7 at -50°C is greatly reduced to less than 160J; the extreme difference of the carbon content segregation in the cross section is increased to more than 0.059%. It can be seen that the present invention greatly improves the impact toughness of the continuously cast round billet by optimizing the element components and their content ratios.

[0124] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A continuous casting round billet, characterized in that: The continuous casting round billet comprises the following components: C: 0.15-0.20wt%, Mn: 1.40-1.70wt%, Cr: 0.08-0.12wt%, Mo≤0.10wt%, Ni≤0.50wt%, Nb: 0.02-0.05wt%, V: 0.04-0.20wt%, Al: 0.020-0.040wt%, Si: 0.20-0.50wt%, P≤0.015wt%, S≤0.005wt%, O≤0.0025wt%, N: 0.006-0.012wt%, H≤0.00015wt% and the balance Fe.

2. The continuous casting round billet according to claim 1, characterized in that: The C content in the continuous casting round billet is 0.17-0.18wt%; Preferably, the Mn content in the continuous casting round billet is 1.53-1.57wt%; Preferably, the Cr content in the continuous casting round billet is 0.09-0.11wt%; Preferably, the Ni content in the continuous casting round billet is ≤0.30wt%; Preferably, the Nb content in the continuous casting round billet is 0.023-0.027wt%; Preferably, the V content in the continuous casting round billet is 0.045-0.050wt%; Preferably, the Al content in the continuous casting round billet is 0.025-0.035wt%; Preferably, the Si content in the continuous casting round billet is 0.28-0.32wt%; Preferably, the P content in the continuous casting round billet is ≤0.010wt%; Preferably, the S content in the continuous casting round billet is ≤0.003wt%; Preferably, the O content in the continuous casting round billet is ≤0.0012wt%; Preferably, the N content in the continuous casting round billet is 0.007-0.009wt%; Preferably, the H content in the continuously cast round billet is ≤0.00012wt%.

3. The continuous casting round billet according to claim 1 or 2, characterized in that: The CEV in the continuous casting round billet is in the range of 0.44-0.48 wt%, wherein CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, preferably 0.45-0.47 wt%.

4. The continuous casting round billet according to any one of claims 1 to 3, characterized in that: The sum of the contents of Nb and V in the continuous casting round billet is 0.06-0.25wt%, preferably 0.068-0.077wt%; Preferably, the sum of the contents of N and Al in the continuous casting round billet is 0.026-0.052wt%, preferably 0.032-0.044wt%; Preferably, the diameter of the continuously cast round billet is 700-1200 mm.

5. A method for preparing a continuous casting round billet according to any one of claims 1 to 4, characterized in that: The preparation method comprises: molten steel is continuously cast and cooled in sequence to obtain the continuously cast round billet.

6. The preparation method according to claim 5, characterized in that: The continuous casting is carried out in a continuous casting machine; Preferably, the pulling speed during continuous casting is 0.08 to 0.32 m / min, preferably 0.18 to 0.32 m / min; Preferably, the superheat degree during continuous casting is 15-35°C.

7. The preparation method according to claim 6, characterized in that: The current of electromagnetic stirring of the crystallizer in the continuous casting machine is 280-380A; Preferably, the frequency of the electromagnetic stirring of the crystallizer is 1.0 to 1.5 Hz; Preferably, the current for stirring the casting strand in the continuous casting machine is 55 to 75A; Preferably, the frequency of the strand stirring is 1.0 to 3.5 Hz; Preferably, the current of the terminal electromagnetic stirring in the continuous casting machine is 320-420A; Preferably, the frequency of the terminal electromagnetic stirring is 1.0 to 3.5 Hz.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The cooling method includes slow cooling in a pit; Preferably, the pit entry temperature for slow cooling is ≥500°C; Preferably, the slow cooling time in the pit is ≥120h; Preferably, the exit temperature of the slow cooling in the pit is ≤250°C.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The preparation method comprises the following steps: The molten steel is continuously cast in a continuous casting machine, the pulling speed during continuous casting is 0.08-0.32 m / min, the superheat is 15-35°C, the current of the electromagnetic stirring of the crystallizer in the continuous casting machine is 280-380A, the frequency is 1.0-1.5Hz, the current of the casting strand stirring in the continuous casting machine is 55-75A, the frequency is 1.0-3.5Hz, the current of the terminal electromagnetic stirring in the continuous casting machine is 320-420A, the frequency is 1.0-3.5Hz; then, the steel is cooled by slow cooling in a pit, the pit entry temperature of the slow cooling in the pit is ≥500°C, the time is ≥120h, and the pit exit temperature is ≤250°C, so as to finally obtain the continuously cast round billet.

10. An application of the continuous casting round billet according to any one of claims 1 to 4, characterized in that: The continuously cast round billet is used for preparing wind power flanges, preferably for wind power flanges at -50°C.