Preparation method and application of washable cuprous oxide antibacterial agent

By modifying cuprous oxide particles with chemical reaction functions in the water system, the problem of the decline of antibacterial ability of antibacterial agents after washing is solved, and a green and environmentally friendly washing resistance effect is achieved. Textiles still maintain efficient antibacterial performance after multiple washings.

CN118745656APending Publication Date: 2024-10-08北京天盾新材科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410931312.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The antibacterial ability of existing antibacterial agents drops significantly after repeated washing, and the production process is complex and the use of organic solvents is not friendly to the environment, making it difficult to meet the needs of water resistance and environmental protection.

Method used

By modifying cuprous oxide particles with chemical reaction functions in a water system to form chemical bonds with fibers, a washable cuprous oxide antibacterial agent without organic solvents is prepared. The steps are simple, no by-products, and green and environmentally friendly.

Benefits of technology

It achieves a stable and efficient combination of cuprous oxide antibacterial agent on the fiber surface. The textile still maintains more than 98% antibacterial effect after 100 times of washing. It is effective against a variety of bacteria, complies with 5A level standards, and is non-toxic, harmless and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745656A_ABST
    Figure CN118745656A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a washable cuprous oxide antibacterial agent, and the preparation method comprises the following steps: S1, adjusting the pH value of a mixture I containing an olefin compound, sulfydryl siloxane and a solvent to be acidic, and marking as a component A; s2, stirring a mixture II containing a photoinitiator and a component A under ultraviolet irradiation to obtain a functional organic matter; s3, stirring a mixture III containing functional organic matters and cuprous oxide II to obtain the washable cuprous oxide antibacterial agent. The antibacterial fabric prepared by forming chemical bonds between the cuprous oxide antibacterial agent and the textile has excellent washing antibacterial performance, the antibacterial rate of staphylococcus aureus, escherichia coli and candida albicans can still reach 99% or above after 100 times of washing, the antibacterial effect meets the 5A level, and the long-acting antibacterial ability can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a preparation method and application of a water-washable cuprous oxide antibacterial agent, belonging to the technical field of fabric antibacterial. Background Art

[0002] In recent years, due to the widespread prevalence of infectious diseases such as the new coronavirus and influenza A, which have had a huge impact on human health and life, people's demand for antibacterial products has increased, especially for various types of textiles such as clothing that come into contact with the human body and are easily contaminated and breed bacteria and viruses. Antibacterial finishing is currently one of the main processes for producing fabrics with antibacterial and antibacterial functions. The antibacterial agents used are divided into organic antibacterial agents and inorganic antibacterial agents. Organic antibacterial agents have the advantages of simple process and little impact on fabrics. Inorganic antibacterial agents, such as inorganic substances containing metal ions such as Ag, Cu and Zn, have the advantages of rapid, efficient and broad-spectrum sterilization. However, there is a problem of weak binding force between antibacterial agents and fibers, which leads to the loss of antibacterial agents, which is manifested in the significant decrease in the antibacterial ability of fabrics after multiple washings. Therefore, with the improvement of antibacterial performance requirements, the development of antibacterial agents with water-resistant functions has received increasing attention.

[0003] At present, there are reports on washable antibacterial agents. Fabrics treated with them can maintain good antibacterial effects after multiple washings. However, most of them have problems such as complex production process, many by-products and environmental unfriendliness. Patent CN115559116 A discloses a single-component washable antibacterial agent and its preparation method and application. The single-component washable antibacterial agent is configured into aqueous solutions of different mass concentrations, and cotton is soaked, washed and dried to obtain antibacterial finished cotton fabric. Although it has a certain antibacterial effect, the use of volatile organic solvents such as tetrahydrofuran solvent and ether in the preparation process has certain harm to the environment and human body. Patent CN 115897231 A discloses a high-efficiency washable antibacterial and anti-ultraviolet fabric and its preparation method and application. Acetoacetic acidized fabric is subjected to multi-component reaction with aldehyde and amino-containing antibiotics in a solvent, and then filtered, washed and dried to obtain a high-efficiency washable antibacterial and anti-ultraviolet fabric. The synthesis steps are not only cumbersome and complicated, but also the synthesis process uses environmentally unfriendly organic solvents.

[0004] The present application provides a water-washable cuprous oxide antibacterial agent which has simple steps, no by-products and is green and environmentally friendly. Summary of the invention

[0005] The purpose of the present application is to provide a method for preparing a water-resistant cuprous oxide antibacterial agent, in which the functional modification of the surface of cuprous oxide particles is achieved by chemical reaction in a water system. A chemical bond can be formed between the modified cuprous oxide and the fibers of the textile, firmly bonded to the surface of the fabric fibers, effectively improving the problems of reduced antibacterial properties due to washing, soaking, etc., and achieving a stable and efficient antibacterial effect. The preparation process does not use organic solvents, is green and environmentally friendly, has simple steps, and has no by-products. The prepared cuprous oxide antibacterial agent is a water-based antibacterial agent, which is non-toxic and harmless to the human body, and does not affect the fabric feel, color, breathability and other properties.

[0006] According to one aspect of the present application, a method for preparing a water-washable cuprous oxide antibacterial agent is provided, the preparation method comprising the following steps:

[0007] S1: adjusting the pH value of a mixture I containing an olefin compound, mercaptosiloxane and water to be acidic, which is recorded as component A;

[0008] S2: Under ultraviolet light, stirring mixture II containing a photoinitiator and component A with I to obtain a functional organic compound;

[0009] S3: Stir II the mixture III containing the functional organic matter and cuprous oxide to obtain the water-resistant cuprous oxide antibacterial agent.

[0010] Optionally, in step S1, the olefin compound is selected from at least one of sodium vinyl sulfonate, methyl methacrylate, β-hydroxyethyl methacrylate, and sodium methacrylic acid.

[0011] Optionally, the mercaptosiloxane is selected from at least one of 3-mercaptopropylmethyldiethoxysiloxane, 3-mercaptopropylmethyldimethoxysiloxane, 3-mercaptopropyltriethoxysiloxane and 3-mercaptopropyltrimethoxysiloxane.

[0012] Optionally, in step S2, the photoinitiator is selected from at least one of benzophenone derivatives, benzil derivatives, aqueous benzoin derivatives, aqueous acetophenone derivatives, and organic phosphine compounds.

[0013] Optionally, the molar ratio of the olefin compound, mercaptosiloxane and photoinitiator is 1:0.2-3:0.001-0.2.

[0014] Optionally, the molar volume ratio of the olefin compound to the water is 1:0.001-4 mol / L.

[0015] Optionally, in step S3, the volume ratio of the functional organic matter to the cuprous oxide is 1:1.3-8.

[0016] Optionally, in step S3, the volume ratio of the functional organic matter to the cuprous oxide is independently selected from any value of 1:1.3, 1:2, 1:3, 1:5, 1:6, 1:8 or a range between any two of the above values.

[0017] Optionally, the pH value is 1.5-5.

[0018] Optionally, the pH value is independently selected from any value of 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or a range between any two of the above values.

[0019] Optionally, the wavelength of the ultraviolet light is 250-400 nm.

[0020] Optionally, the wavelength of the ultraviolet light is independently selected from any value of 250nm, 280nm, 300nm, 350nm, 400nm or a range between any two of the above.

[0021] Optionally, the light source of the ultraviolet light is selected from at least one of an LED lamp, a mercury lamp, and a xenon lamp.

[0022] Optionally, the stirring temperature is 0 to 40° C., and the stirring time is 10 to 120 min.

[0023] Optionally, the stirring temperature I is independently selected from any value of 0°C, 5°C, 10°C, 20°C, 30°C, 40°C or a range between any two of the above values.

[0024] Optionally, the stirring time I is independently selected from any value among 10min, 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min or a range value between any two of the above.

[0025] Optionally, the stirring time II is 2 to 20 hours.

[0026] Optionally, the stirring time II is independently selected from any value among 2h, 4h, 5h, 8h, 10h, 12h, 14h, 16h, 20h or a range between any two of the above.

[0027] According to another aspect of the present application, a water-washable cuprous oxide antibacterial agent prepared by the above-described preparation method is provided.

[0028] According to another aspect of the present application, there is provided an application of the above-mentioned water-resistant cuprous oxide antibacterial agent in textile fabrics, the application comprising:

[0029] According to the water-bath ratio of 1:10 to 1:20, a mixture containing dyes, auxiliaries and water-resistant cuprous oxide antibacterial agents is stirred and dyed to obtain a textile fabric containing the water-resistant cuprous oxide antibacterial agent.

[0030] Optionally, the addition amount of the water-washable cuprous oxide antibacterial agent is 0.2% to 5%.

[0031] As an optional implementation method, the present application is implemented through the following technical solutions:

[0032] (1) Dissolve the olefin derivative compound in deionized water and stir thoroughly to dissolve.

[0033] (2) Stirring and mixing the mercaptosiloxane and the aqueous solution of the olefin derivative compound to be uniform, and adjusting the pH of the solution to be acidic.

[0034] (3) Dissolve the photoinitiator in water and add it into the above mixed solution and stir evenly.

[0035] (4) Under ultraviolet light irradiation, the reaction is stirred and maintained at a certain temperature to obtain functional organic matter.

[0036] (5) Add the functional organic matter into the cuprous oxide suspension and stir thoroughly to obtain the cuprous oxide antibacterial agent.

[0037] When the cuprous oxide antimicrobial agent is applied to the finishing of textile fabrics, the fabrics are placed in a dye vat according to the dyeing process requirements, and dyes, auxiliaries, etc. are first placed in a premixing tank according to a water bath ratio of 1:10-1:20, and then an appropriate amount of cuprous oxide antimicrobial agent (added at a ratio of 0.2%-5% (owf)) is weighed and added to the premixing tank, and the mixture is fully stirred and evenly mixed, and the dyeing material in the premixing tank is injected into the dye vat for subsequent dyeing process. When the dyeing temperature is above 90°C, the cuprous oxide antimicrobial agent can be quickly combined with the fabric fiber, and the fabric finished with the cuprous oxide antimicrobial agent is obtained after post-treatment. The application method is simple, the usage amount is small, and the cost is low. The obtained antibacterial cotton fabric has excellent water-resistant and antibacterial functions, and the antibacterial effect is better when the addition ratio is greater than 1.5% and above.

[0038] The beneficial effects of this application include:

[0039] 1) The cuprous oxide antibacterial agent provided in the present application does not require post-treatment and can be directly applied to textile fabrics, and the method and process are simple.

[0040] 2) The solvent of the cuprous oxide antibacterial agent prepared in the present application is a pure water system, does not contain any organic solvent, is green and environmentally friendly, and does not contain any toxic or harmful components to the human body.

[0041] 3) The cuprous oxide antibacterial agent provided in the present application uses cuprous oxide as an antibacterial component and achieves broad-spectrum and high-efficiency antibacterial effects through two antibacterial mechanisms: contact antibacterial and dissolution antibacterial.

[0042] 4) The antibacterial fabric prepared by forming a chemical bond between the cuprous oxide antibacterial agent and the textile provided in the present application has excellent water-washable antibacterial properties. After washing 100 times, the antibacterial rate against Staphylococcus aureus and Candida albicans can still reach more than 98%, and the antibacterial rate against Escherichia coli is more than 86%. The antibacterial effect meets the 5A level and can achieve long-term antibacterial ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a SEM electron microscope image of the cuprous oxide antibacterial agent prepared in Example 1 of the present application, with a scale of 200 nm.

[0044] Figure 2 This is a SEM electron microscope image of the cuprous oxide antibacterial agent prepared in Example 3 of the present application, with a scale of 200 nm.

[0045] Figure 3 This is a SEM electron microscope image of the cuprous oxide antibacterial agent prepared in Example 5 of the present application, with a scale of 200 nm.

[0046] Figure 4 Figures of cuprous oxide antibacterial agents prepared in Example 1 (left), Example 3 (middle) and Example 5 (right) of the present application.

[0047] Figure 5 This is a comparison chart of the antibacterial rates of fabrics treated with cuprous oxide antibacterial agent before and after washing 100 times in Application Examples 1 and 2 of this application.

[0048] Figure 6 This is a comparison chart of the antibacterial rates of the fabric treated with a common antibacterial agent before and after washing 100 times in Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0049] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0050] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0051] Field emission scanning electron microscopy was used to characterize the morphology of cuprous oxide antibacterial agent.

[0052] The antibacterial tests of fabrics were entrusted to Guangzhou Institute of Microbiology Group Co., Ltd.

[0053] Example 1

[0054] (1) Add 16 g of sodium vinyl sulfonate to 150 mL of deionized water and stir until dissolved.

[0055] (2) Weigh 24 g of 3-mercaptopropyl triethoxysiloxane and pour it into the above solution, stir evenly, and adjust the pH of the solution to 2.

[0056] (3) Weigh 1 g of the photoinitiator 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, add it to 50 mL of 90° C. distilled water, fully dissolve it, cool it to room temperature, then add it to the above mixed solution and stir evenly.

[0057] (4) Irradiate under 350 nm LED light for 30 min, maintain stirring at 20 °C for half an hour to obtain functional organic matter.

[0058] (5) Continue to weigh 50g of cuprous oxide, add it to a beaker of 650mL of distilled water, and stir to disperse it evenly. Add 200mL of functional organic matter to the cuprous oxide suspension, continue to stir, and react at room temperature for 20h to obtain a cuprous oxide antibacterial agent. Figure 1 It can be seen that the modified material is evenly covered on the surface of cuprous oxide, proving that the modification is successful.

[0059] Example 2

[0060] (1) Add 16 g of sodium methyl methacrylate sulfonate to 150 mL of deionized water and stir until dissolved.

[0061] (2) Weigh 24 g of 3-mercaptopropyl triethoxysiloxane, pour it into the above solution and stir evenly, and adjust the pH of the solution to 2.

[0062] (3) Weigh 1.5 g of the photoinitiator 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, add it to 50 mL of 90° C. distilled water, fully dissolve it, cool it to room temperature, then add it to the above mixed solution and stir evenly.

[0063] (4) Irradiate under 350 nm LED light for 50 min, maintain stirring at 20 °C for half an hour to obtain functional organic matter.

[0064] (5) Continue to weigh 50g of cuprous oxide, add it to a beaker of 650mL of distilled water, stir and disperse it evenly. Add 200mL of functional organic matter to the cuprous oxide suspension, continue to stir, and react at room temperature for 20h to obtain a cuprous oxide antibacterial agent.

[0065] Example 3

[0066] (1) Add 8 g of sodium methyl methacrylate sulfonate to 150 mL of deionized water and stir until dissolved.

[0067] (2) Weigh 24 g of 3-mercaptopropylmethyldiethoxysiloxane, pour it into the above solution and stir evenly, and adjust the pH of the solution to 5.

[0068] (3) Weigh 1 g of the photoinitiator 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone and add it to 50 mL of 90° C. distilled water to fully dissolve it. Then, cool it to room temperature and add it to the above mixed solution and stir evenly.

[0069] (4) Irradiate under 308 nm LED light for 70 min, maintain stirring at 20 °C for half an hour to obtain functional organic matter.

[0070] (5) Continue to weigh 50g of cuprous oxide, add it to a beaker of 650mL of distilled water, and stir to disperse it evenly. Add 200mL of functional organic matter to the cuprous oxide suspension, continue to stir, and react at room temperature for 20h to obtain a cuprous oxide antibacterial agent. Figure 2 It can be seen that the cuprous oxide surface modification covers more completely.

[0071] Example 4

[0072] (1) Add 16 g of sodium methyl methacrylate sulfonate to 150 mL of deionized water and stir until dissolved.

[0073] (2) Weigh 24 g of 3-mercaptopropylmethyldiethoxysiloxane, pour it into the above solution and stir evenly, and adjust the pH of the solution to 5.

[0074] (3) Weigh 1 g of photoinitiator 3,3',4,4'-benzophenone tetracarboxylic dianhydride and add it to 50 mL of 90° C. distilled water to fully dissolve it. Then, cool it to room temperature and add it to the above mixed solution and stir evenly.

[0075] (4) Irradiate under a 313 nm mercury lamp for 50 min, maintain the reaction at 20° C. with stirring for half an hour to obtain a functional organic compound.

[0076] (5) Continue to weigh 50g of cuprous oxide, add it to a beaker of 650mL of distilled water, stir and disperse it evenly. Add 200mL of functional organic matter to the cuprous oxide suspension, continue to stir, and react at room temperature for 20h to obtain a cuprous oxide antibacterial agent.

[0077] Example 5

[0078] (1) Add 16 g of sodium methyl methacrylate sulfonate to 150 mL of deionized water and stir until dissolved.

[0079] (2) Weigh 24 g of 3-mercaptopropylmethyldiethoxysiloxane, pour it into the above solution and stir evenly, and adjust the pH of the solution to 5.

[0080] (3) Weigh 1 g of photoinitiator 3,3',4,4'-benzophenone tetracarboxylic dianhydride and add it to 50 mL of 90° C. distilled water to fully dissolve it. Then, cool it to room temperature and add it to the above mixed solution and stir evenly.

[0081] (4) Irradiate under a 313 nm mercury lamp for 70 min, maintain the reaction at 20° C. with stirring for half an hour to obtain a functional organic compound.

[0082] (5) Continue to weigh 50g of cuprous oxide, add it to a beaker of 300mL of distilled water and stir to disperse it evenly. Add 200mL of functional organic matter to the cuprous oxide suspension, continue stirring, and react at room temperature for 20h to obtain a cuprous oxide antibacterial agent. Figure 3 It can be seen that the cuprous oxide surface modification layer is more obvious. Figure 4 This is the dispersion of the cuprous oxide antibacterial agent after it has been stationary for one month. The more surface modifiers are coated, the more obvious the precipitation of the cuprous oxide antibacterial agent is.

[0083] Application Example 1

[0084] Cuprous oxide antimicrobial agent is used for finishing of textile fabrics. According to the dyeing process requirements, the fabrics are placed in the dye vat with a water bath ratio of 1:10. Dyes, auxiliaries, etc. are first placed in the premixing tank, and then 1.5% (owf) cuprous oxide antimicrobial agent is weighed and added to the premixing tank. The mixture is fully stirred and evenly mixed. The dyeing materials in the premixing tank are injected into the dye vat for subsequent dyeing process. The dyeing temperature is 90°C, the setting time is 50-120min, and the temperature is not higher than 140°C. According to the type of fabric, the fabric is finished, and the ironing and drying temperature does not exceed 200°C.

[0085] According to the method in GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial finished fabrics were washed 100 times and then tested for antibacterial properties. Figure 5 As shown, after washing 100 times, the antibacterial rate of the antibacterial fabric against Escherichia coli is 86%, the antibacterial rate against Staphylococcus aureus is 99%, and the antibacterial rate against Candida albicans is 98%, which are much higher than the 5A level specified Escherichia coli ≥80%, Staphylococcus aureus ≥90% and Candida albicans ≥70% standard values, and meet the 5A level washable antibacterial standards.

[0086] Application Example 2

[0087] Cuprous oxide antimicrobial agents are used in the finishing of textile fabrics. According to the dyeing process requirements, the fabrics are placed in the dye vat with a water bath ratio of 1:20. Dyes, auxiliaries, etc. are first placed in the premixing tank, and then 2% (owf) cuprous oxide antimicrobial agent is weighed and added to the premixing tank. The mixture is fully stirred and evenly mixed. The dyeing materials in the premixing tank are injected into the dye vat for subsequent dyeing process. The dyeing temperature is 130°C, the setting time is 10-20min, and the temperature is not higher than 140°C. According to the type of fabric, the fabric is finished, and the ironing and drying temperature does not exceed 200°C.

[0088] According to the method in GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the antibacterial finished fabrics were washed 100 times and then tested for antibacterial properties. Figure 5 As shown, after washing 100 times, the antibacterial rate of adding 2% antibacterial fabric against Escherichia coli is 99%, the antibacterial rate against Staphylococcus aureus is 99%, and the antibacterial rate against Candida albicans is 99%, which is better than the antibacterial effect of adding 1.5% antibacterial fabric, and is far higher than the 5A level specified Escherichia coli ≥80%, Staphylococcus aureus ≥90% and Candida albicans ≥70% standard values, meeting the 5A level water-resistant and antibacterial standards.

[0089] Comparative Example 1

[0090] Use common antimicrobial agents for finishing of textile fabrics. Put the fabrics into the dye vat according to the dyeing process requirements, with a water bath ratio of 1:10. First, put dyes, auxiliaries, etc. into the premixing tank, then weigh 1.5% (owf) cuprous oxide antimicrobial agent and add it to the premixing tank. Stir and mix well, inject the dye in the premixing tank into the dye vat for subsequent dyeing process. The dyeing temperature is 90°C, the setting time is 50-120min, and the temperature is not higher than 140°C. According to the type of fabric, the fabric is finished, and the ironing and drying temperature does not exceed 200°C.

[0091] According to the method in GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", the fabrics treated with common antibacterial agents were washed 100 times and then subjected to antibacterial testing. Figure 6 As shown, after washing 100 times, the antibacterial rate of the antibacterial fabric against Escherichia coli was 56%, the antibacterial rate against Staphylococcus aureus was 65%, and the antibacterial rate against Candida albicans was 60%.

[0092] Therefore, it can be seen that the fabric treated with the cuprous oxide antibacterial agent prepared by the preparation method of the present invention still exhibits excellent antibacterial performance after being washed 100 times, reaching the 5A antibacterial level. The fabric treated with the common antibacterial agent has no antibacterial effect after being washed 100 times.

[0093] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a water-resistant cuprous oxide antibacterial agent, It is characterized in that The preparation method comprises the following steps: S1: adjusting the pH value of a mixture I containing an olefin compound, mercaptosiloxane and water to be acidic, which is recorded as component A; S2: Under ultraviolet light, stirring mixture II containing a photoinitiator and component A with I to obtain a functional organic compound; S3: Stir II the mixture III containing the functional organic matter and cuprous oxide to obtain the water-resistant cuprous oxide antibacterial agent.

2. The preparation method according to claim 1, It is characterized in that In the step S1, the olefin compound is selected from at least one of sodium vinyl sulfonate, methyl methacrylate, β-hydroxyethyl methacrylate, and sodium methacrylic acid; Preferably, the mercaptosiloxane is selected from at least one of 3-mercaptopropylmethyldiethoxysiloxane, 3-mercaptopropylmethyldimethoxysiloxane, 3-mercaptopropyltriethoxysiloxane and 3-mercaptopropyltrimethoxysiloxane.

3. The preparation method according to claim 1, It is characterized in that In the step S2, the photoinitiator is selected from at least one of benzophenone derivatives, benzil derivatives, water-based benzoin derivatives, water-based acetophenone derivatives, and organic phosphine compounds.

4. The preparation method according to claim 1, It is characterized in that The molar ratio of the olefin compound, mercaptosiloxane and photoinitiator is 1:0.2-3:0.001-0.2; Preferably, the molar volume ratio of the olefin compound to the water is 1:0.001-4 mol / L.

5. The preparation method according to claim 1, It is characterized in that In the step S3, the volume ratio of the functional organic matter to the cuprous oxide is 1:1.3-8.

6. The preparation method according to claim 1, It is characterized in that The pH value is 1.5 to 5; Preferably, the wavelength of the ultraviolet light is 250-400 nm; Preferably, the light source of the ultraviolet light is selected from at least one of an LED lamp, a mercury lamp, and a xenon lamp.

7. The preparation method according to claim 1, It is characterized in that The stirring temperature is 0 to 40° C., and the stirring time is 10 to 120 min. Preferably, the stirring time II is 2 to 20 hours.

8. The water-washable cuprous oxide antibacterial agent prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the washable cuprous oxide antibacterial agent according to claim 8 in textile fabrics, It is characterized in that The applications include: According to the water-bath ratio of 1:10 to 1:20, a mixture containing dyes, auxiliaries and water-resistant cuprous oxide antibacterial agents is stirred and dyed to obtain a textile fabric containing the water-resistant cuprous oxide antibacterial agent.

10. The use according to claim 9, It is characterized in that The addition amount of the water-washable cuprous oxide antibacterial agent is 0.2% to 5%.