Composite roof insulation board and preparation method thereof
Through the seamless design of the composite roof insulation board, which integrates waterproofing, insulation and decorative functions, it solves the water leakage problem caused by cavities and joints in traditional roofing systems, improves the durability and construction efficiency of the building, and simplifies the construction process.
Patent Information
- Application Number
- CN202410760663.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional roofing systems have cavities and joint problems caused by layered structures, which lead to water leakage, aging, high maintenance costs and cumbersome construction steps, affecting the durability and safety of the building.
Composite roof insulation boards are used, through a combination of modified graphite flame retardants, polymeric flexible waterproof materials, anti-crack waterproof mortar, insulation materials and decorative materials, and through a lamination process to form an overall structure with no joints, no edges, and no seams. , integrating waterproof, thermal insulation and decorative functions.
The seamless design is achieved, which significantly improves the waterproof performance and structural stability of the roof, simplifies the construction steps, reduces labor costs and construction risks, and extends the service life of the building.
Smart Images

Figure CN118745796A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a composite roof insulation board and a preparation method thereof. Background Art
[0002] In modern buildings, the design and construction of roof systems are crucial to the safety and durability of the entire building. Traditional roof systems usually adopt a layered structure, including independent waterproof layers, insulation layers and decorative layers. The main advantage of this multi-layer structure is that each layer can be specifically optimized for different functional requirements.
[0003] Traditional roofing systems use a layered structure, with cavities and joints between the layers. These cavities and joints are prone to gaps during construction and use, causing water to penetrate and accumulate, and eventually causing water leakage. Especially in rainy seasons or environments with high humidity, water leakage is more serious, affecting the service life and safety of buildings. In addition, traditional waterproof layers usually use SBS waterproof membranes or other flexible materials, but these materials are prone to aging and cracking in long-term use. Especially in areas with large temperature changes, cracks in the waterproof layer will cause waterproofing failure, increasing maintenance costs and difficulties. In addition, the construction steps of traditional roofing systems are numerous and need to be divided into In addition, the waterproof layer, thermal insulation layer and decorative layer are laid, especially the pasting process of the decorative layer (such as tiles), which takes a lot of time and manpower, has a long construction period and high labor costs. At the same time, the decorative layer needs to be pasted later, which is prone to inconsistent decorative effects. In addition, the decorative layer is easy to fall off or be damaged after long-term use, requiring frequent maintenance and repair, which increases maintenance costs. Finally, traditional thermal insulation layers usually use materials such as polystyrene (XPS). These materials are easily affected by the environment in the layered structure, and there are cavities and thermal bridges, resulting in poor thermal insulation effects. Especially in cold or hot areas, the thermal insulation performance of the roof directly affects the energy consumption and indoor comfort of the building. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a composite roof insulation board and a preparation method thereof, which solves the problem of cavities and seams existing at the connection between the layered structures of the equipment.
[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a composite roof insulation board and a preparation method thereof, comprising the following component materials: 1 to 5 parts of modified graphite flame retardant, 20 to 40 parts of polymer flexible waterproof material, 10 to 30 parts of anti-cracking waterproof mortar, 40 to 60 parts of insulation material, and 5 to 15 parts of decorative material.
[0006] Preferably, the graphite flame retardant includes graphite powder and flame retardant, and the addition ratio of the graphite powder and the flame retardant is 1:2; the flame retardant includes aluminum hydroxide and brominated flame retardant, and the addition ratio of the aluminum hydroxide and the brominated flame retardant is 3:1; the polymer flexible waterproof material includes polyurethane and flexible additives, and the addition ratio of the polyurethane and the flexible additive is 3:1; the flexible additive includes polyacrylate and plasticizer, and the addition ratio of the polyacrylate and the plasticizer is 2:1.
[0007] Preferably, the anti-cracking and waterproof mortar includes cement and polymer additives, and the addition ratio of the cement and polymer additives is 3:1; the polymer additive includes emulsion and cellulose, and the addition ratio of the emulsion and cellulose is 3:1.
[0008] Preferably, the thermal insulation material comprises polystyrene foam and a reinforcing agent, the polystyrene foam and the reinforcing agent are added in a ratio of 4:1, and the reinforcing agent comprises silicate and a foaming agent, the silicate and the foaming agent are added in a ratio of 2:1.
[0009] Preferably, the decorative material includes ceramic particles and a binder, the ceramic particles and the binder are added in a ratio of 1:1, the binder includes a cement-based binder and rubber powder, the cement-based binder and the rubber powder are added in a ratio of 2:1, the cement-based binder includes Portland cement and fine aggregate, the Portland cement and the fine aggregate are added in a ratio of 3:1.
[0010] A method for preparing a composite roof insulation board comprises the following steps:
[0011] S1. Prepare materials: prepare graphite flame retardant, polymer flexible waterproof material, anti-cracking waterproof mortar, thermal insulation material and decorative material;
[0012] S2, stacking and pressing: first, the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine, and then the polymer flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed by a hydraulic press, and the thermal insulation layer and the decorative material layer are also matched layer by layer;
[0013] S3, template curing: place the pressed board template and materials at room temperature for curing for 24 hours;
[0014] S4, beautification cutting: the solidified plate is polished by a grinder and cut by a laser cutting machine according to the required size;
[0015] S5. Quality inspection: Use inspection instruments to conduct quality inspection on the cut boards, including waterproof performance test, crack resistance test and thermal insulation performance test.
[0016] Preferably, in the step S2, the operating pressure of the laminating machine is 5MPa-10MPa, and the operating temperature of the laminating agent is 50°C-70°C.
[0017] Preferably, in step S4, the rotation speed of the grinder is 966RPM-2900RPM, and the diameter of the grinding disc of the grinder is 150mm.
[0018] Preferably, in step S4, the laser wavelength of the laser cutting machine is 1015nm-1065nm, and the cutting accuracy of the laser cutting machine is ±0.1mm.
[0019] Preferably, in step S5, the inspection instrument group includes a water permeability tester, a universal material testing machine and a thermal conductivity tester.
[0020] The present invention provides a composite roof insulation board and a preparation method thereof. The composite roof insulation board has the following beneficial effects:
[0021] 1. The present invention integrates waterproofing, thermal insulation and decorative functions into one board to achieve an overall structure without joints, edges or seams. This design completely eliminates the cavity and water leakage problems in traditional roof structures, significantly improves the overall performance of the roof, and ensures long-term stability and reliability.
[0022] 2. The present invention adopts modified polymer flexible waterproof material and anti-cracking waterproof mortar. The present invention enables the board to have excellent waterproof performance and good anti-cracking performance. This feature effectively prevents the traditional waterproof layer from failing due to cracks, extends the service life of the roof, and enhances the durability and safety of the building.
[0023] 3. The present invention greatly simplifies the construction steps through the integrated panel design. There is no need for layered construction, which eliminates the tedious decoration steps such as pasting tiles in traditional roof construction. The construction process is more convenient and the decorative effect is more beautiful and unified. In addition, this design greatly shortens the construction period, reduces labor costs and construction risks, and improves overall construction efficiency.
[0024] 4. The present invention ensures the close combination between the thermal insulation layer and the decorative layer through the layer-by-layer kneading and pressing process, avoiding the generation of any gaps. This seamless design effectively prevents the accumulation, penetration and diffusion of water, completely solves the water seepage problem in traditional roof construction, and further improves the waterproof performance and structural stability of the roof. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a flow chart of the preparation steps of the present invention. DETAILED DESCRIPTION
[0026] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1: Preparation of standard waterproof composite roof insulation board
[0028] step:
[0029] S1. Material preparation: 3 parts of graphite flame retardant, 30 parts of polymer flexible waterproof material, 20 parts of anti-cracking waterproof mortar, 45 parts of thermal insulation material, and 10 parts of decorative material;
[0030] S2. Stacking and pressing: Spread the graphite flame retardant evenly in the bottom mold, and press it into shape by a pressing machine at a pressure of 7MPa and a temperature of 60°C; lay the polymerized flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer in sequence, and press them layer by layer by a hydraulic press, and rub the thermal insulation layer and the decorative material layer layer by layer;
[0031] S3, template curing: curing at room temperature for 24 hours;
[0032] S4, beautification cutting: use a grinder for grinding, the speed is 2000RPM, the grinding disc diameter is 150mm, and the laser cutting machine is used for cutting, the laser wavelength is 1030nm, and the cutting accuracy is ±0.1mm;
[0033] S5. Quality inspection: Use water permeability tester, universal material testing machine and thermal conductivity tester to test the waterproof, crack resistance and thermal insulation performance respectively, and conduct inspection according to relevant standards.
[0034] Summarize:
[0035] This embodiment uses standardized material ratios and a laminating process to prepare a composite roof insulation board with good waterproof, crack resistance and thermal insulation properties.
[0036] Example 2: Preparation of reinforced crack-resistant composite roof insulation board
[0037] step:
[0038] S1. Material preparation: 2 parts of graphite flame retardant, 25 parts of polymer flexible waterproof material, 30 parts of anti-cracking waterproof mortar, 40 parts of thermal insulation material, and 10 parts of decorative material;
[0039] S2, stacking and pressing: the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine at a pressure of 6MPa and a temperature of 55°C, and the polymerized flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed layer by layer by a hydraulic press, and the thermal insulation layer and the decorative material layer are rubbed layer by layer;
[0040] S3, template curing: curing at room temperature for 24 hours;
[0041] S4, beautification cutting: use a grinder for grinding, the speed is 2500RPM, the grinding disc diameter is 150mm, and the laser cutting machine is used for cutting, the laser wavelength is 1040nm, and the cutting accuracy is ±0.1mm;
[0042] S5. Quality inspection: Use water permeability tester, universal material testing machine and thermal conductivity tester to test the waterproof, crack resistance and thermal insulation performance respectively, and conduct inspection according to relevant standards.
[0043] Summarize:
[0044] This embodiment significantly improves the anti-cracking performance of the board by increasing the proportion of the anti-cracking and waterproof mortar, while maintaining good waterproof and heat-insulating effects.
[0045] Example 3: Preparation of high thermal insulation composite roof insulation board
[0046] step:
[0047] S1. Material preparation: 4 parts of graphite flame retardant, 20 parts of polymer flexible waterproof material, 15 parts of anti-cracking waterproof mortar, 55 parts of thermal insulation material, and 6 parts of decorative material;
[0048] S2, stacking and pressing: the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine at a pressure of 8MPa and a temperature of 65°C, and the polymerized flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed layer by layer by a hydraulic press, and the thermal insulation layer and the decorative material layer are rubbed layer by layer;
[0049] S3, template curing: curing at room temperature for 24 hours;
[0050] S4, beautification cutting: use a grinder for grinding, the speed is 2200RPM, the grinding disc diameter is 150mm, and the laser cutting machine is used for cutting, the laser wavelength is 1050nm, and the cutting accuracy is ±0.1mm;
[0051] S5. Quality inspection: Use water permeability tester, universal material testing machine and thermal conductivity tester to test the waterproof, crack resistance and thermal insulation performance respectively, and conduct inspection according to relevant standards.
[0052] Summarize:
[0053] In this embodiment, by increasing the proportion of thermal insulation materials, the prepared board has excellent thermal insulation performance while maintaining good waterproof and crack resistance effects.
[0054] Example 4: Preparation of a composite roof insulation board with high decorative effect
[0055] step:
[0056] S1. Material preparation: 1 part of graphite flame retardant, 35 parts of polymer flexible waterproof material, 15 parts of anti-cracking waterproof mortar, 40 parts of thermal insulation material, 9 parts of decorative material;
[0057] S2, stacking and pressing: the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine at a pressure of 5MPa and a temperature of 50°C, and the polymerized flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed layer by layer by a hydraulic press, and the thermal insulation layer and the decorative material layer are rubbed layer by layer;
[0058] S3, template curing: curing at room temperature for 24 hours;
[0059] S4, beautification cutting: use a grinder for grinding, the speed is 2800RPM, the grinding disc diameter is 150mm, and the laser cutting machine is used for cutting, the laser wavelength is 1060nm, and the cutting accuracy is ±0.1mm;
[0060] S5. Quality inspection: Use water permeability tester, universal material testing machine and thermal conductivity tester to test the waterproof, crack resistance and thermal insulation performance respectively, and conduct inspection according to relevant standards.
[0061] Summarize:
[0062] In this embodiment, by increasing the proportion of decorative materials, the prepared board has excellent decorative effect, while ensuring good waterproof, crack resistance and heat preservation properties.
[0063] Example 5: Preparation of composite roof insulation board with balanced comprehensive performance
[0064] step:
[0065] S1. Material preparation: 2.5 parts of graphite flame retardant, 28 parts of polymer flexible waterproof material, 22 parts of anti-cracking waterproof mortar, 48 parts of thermal insulation material, 8 parts of decorative material;
[0066] S2, stacking and pressing: the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine at a pressure of 6.5MPa and a temperature of 57°C, and the polymerized flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed layer by layer by a hydraulic press, and the thermal insulation layer and the decorative material layer are rubbed layer by layer;
[0067] S3, template curing: curing at room temperature for 24 hours;
[0068] S4, beautification cutting: use a grinder for grinding, the speed is 2400RPM, the grinding disc diameter is 150mm, and the laser cutting machine is used for cutting, the laser wavelength is 1045nm, and the cutting accuracy is ±0.1mm;
[0069] S5. Quality inspection: Use water permeability tester, universal material testing machine and thermal conductivity tester to test the waterproof, crack resistance and thermal insulation performance respectively, and conduct inspection according to relevant standards.
[0070] Summarize:
[0071] This embodiment achieves a balance between various properties, so that the prepared board has comprehensive and excellent waterproof, crack resistance, thermal insulation and decorative properties.
[0072] Summary:
[0073] These five embodiments demonstrate the effects of different material proportions and processing techniques on the performance of composite roof insulation boards. By adjusting the proportions of the various components and optimizing the processing steps, different performance emphases can be achieved, such as composite roof insulation boards with high efficiency waterproofing, high strength crack resistance, high thermal insulation performance, high decorative effect, and balanced performance. These embodiments provide a variety of options for practical applications, and the most suitable solution can be selected according to specific needs.
[0074] Test experiment:
[0075] Test items:
[0076] 1. Waterproof performance test
[0077] Test standard: GB / T328.11-2007;
[0078] Testing instrument: water penetration tester;
[0079] Testing process:
[0080] S1. Fix the sample on the test frame;
[0081] S2, water flow that applies a certain pressure to the sample surface;
[0082] S3. Apply water flow continuously for 1 hour and observe the water seepage;
[0083] S4. Record the water seepage (unit: ml).
[0084] 2. Crack resistance test
[0085] Test standard: GB / T50082-2009;
[0086] Testing equipment: universal material testing machine;
[0087] Testing process:
[0088] S1. Fix the sample on the testing machine.
[0089] S2. Gradually increase the pressure until cracks appear on the sample.
[0090] S3. Record the pressure value when the sample ruptures (unit: MPa).
[0091] 3. Thermal insulation performance test
[0092] Test standard: GB / T10294-2008;
[0093] Testing instrument: thermal conductivity tester;
[0094] Testing process:
[0095] S1. Fix the sample in the tester;
[0096] S2, thermal conductivity of the test sample;
[0097] S3. Record the thermal conductivity value (unit: W / m·K).
[0098] 4.Decoration effect test
[0099] Test standard: custom standard;
[0100] Testing instruments: visual evaluation and colorimeter;
[0101] Testing process:
[0102] S1. Measure the color and surface finish of the samples by visual inspection and colorimeter; S1. Record the color consistency and finish scores (0-100 points).
[0103] Test Results
[0104] Example 1: Standard waterproof composite roof insulation board
[0105] Test items result Waterproof 0.5ml Crack resistance 6.8MPa Thermal insulation performance 0.035W / m·K Decorative Effect 85 points
[0106] Example 2: Reinforced crack-resistant composite roof insulation board
[0107] Test items result Waterproof 0.7ml Crack resistance 8.5MPa Thermal insulation performance 0.040W / m·K Decorative Effect 80 points
[0108] Example 3: High thermal insulation composite roof insulation board
[0109] Test items result Waterproof 0.6ml Crack resistance 6.5MPa Thermal insulation performance 0.030W / m·K Decorative Effect 78 points
[0110] Example 4: Highly decorative composite roof insulation board
[0111] Test items result Waterproof 0.8ml Crack resistance 6.0MPa Thermal insulation performance 0.045W / m·K Decorative Effect 95 points
[0112] Example 5: Composite roof insulation board with balanced comprehensive performance
[0113] Test items result Waterproof 0.6ml Crack resistance 7.0MPa Thermal insulation performance 0.035W / m·K Decorative Effect 82 points
[0114] Summary:
[0115] 1. Waterproof performance: The water-proof performance of all embodiments is between 0.5-0.8 ml, showing a good water-proof effect, especially the water-proof performance of embodiment 1 and embodiment 5 is the best.
[0116] 2. Crack resistance: Example 2 has the best crack resistance, reaching 8.5 MPa, which is significantly higher than other examples and is suitable for applications requiring high crack resistance.
[0117] 3. Thermal insulation performance: Example 3 has the best thermal insulation performance, with a thermal conductivity of 0.030 W / m·K, and is suitable for occasions with high thermal insulation requirements.
[0118] 4. Decorative effect: Example 4 has the best decorative effect, with a score of 95 points, and is very suitable for applications requiring high decorative effects.
[0119] These five embodiments, through different material proportions and process optimization, show significant advantages in waterproofing, crack resistance, thermal insulation and decorative effects, providing a variety of options for different needs.
[0120] Comparative experiment:
[0121] Experiment 1: Comparative experiment on waterproof performance and thermal insulation performance
[0122] Existing technology: The existing technology adopts the traditional layered roof structure, including independent waterproof layer and thermal insulation layer, the materials of which are SBS waterproof membrane and XPS thermal insulation board respectively;
[0123] Technical solution of the present invention: The present invention adopts an integrated composite roof insulation board, and the materials include modified graphite flame retardant, polymer flexible waterproof material, anti-cracking waterproof mortar, insulation material and decorative material.
[0124] Experimental process:
[0125] S1. Sample preparation: prepare 5 samples of the prior art and 5 samples of the present invention;
[0126] S2. Waterproof performance test: According to GB / T328.11-2007 standard, use a water seepage tester to conduct a waterproof test and record the water seepage within 1 hour;
[0127] S3. Thermal insulation performance test: According to GB / T10294-2008 standard, use a thermal conductivity meter to test the thermal conductivity of the sample.
[0128] Test conditions: ambient temperature 25°C, humidity 50%.
[0129] Experimental data:
[0130] sample Waterproof water seepage (ml) Thermal conductivity (W / m·K) Prior art sample 1 5.2 0.040 Prior art sample 2 5.5 0.039 Prior art sample 3 5.3 0.041 Prior art sample 4 5.4 0.038 Prior art sample 5 5.1 0.042 Sample 1 of the present invention 0.5 0.035 Sample 2 of the present invention 0.6 0.034 Sample 3 of the present invention 0.4 0.035 Sample 4 of the present invention 0.6 0.034 Sample 5 of the present invention 0.5 0.033
[0131] Summarize:
[0132] The present invention is significantly better than the prior art in terms of waterproof performance, and the amount of water seepage is greatly reduced; at the same time, the thermal insulation performance is also improved, and the thermal conductivity coefficient is lower, indicating a better thermal insulation effect.
[0133] Experiment 2: Comparative experiment of crack resistance and fire resistance
[0134] Existing technology: The existing technology uses independent waterproof layer and protective layer, and the materials are SBS waterproof membrane and ordinary mortar;
[0135] Technical solution of the present invention: The present invention adopts an integrated composite roof insulation board, and the materials include modified graphite flame retardant, polymer flexible waterproof material and anti-cracking waterproof mortar.
[0136] Experimental process:
[0137] S1. Sample preparation: prepare 5 samples of the prior art and 5 samples of the present invention;
[0138] S2. Crack resistance test: According to GB / T50082-2009 standard, use a universal material testing machine to test the crack resistance of the sample;
[0139] S3. Fire resistance test: Place the sample in an environment with a flame temperature of 800°C and record its combustion conditions and integrity retention time.
[0140] Test conditions: ambient temperature 25°C, humidity 50%.
[0141] Experimental data:
[0142]
[0143]
[0144] Summarize:
[0145] The present invention is significantly superior to the prior art in terms of crack resistance and has higher crack resistance strength; the fire resistance is also greatly improved and the integrity retention time is significantly prolonged, indicating that the fire resistance effect is better.
[0146] Experiment 3: Comparative experiment on overall structural stability and construction efficiency
[0147] Existing technology: The existing technology uses independent waterproof layer, thermal insulation layer and protective layer, and the materials are SBS waterproof membrane, XPS thermal insulation board and ordinary mortar respectively;
[0148] Technical solution of the present invention: The present invention adopts an integrated composite roof insulation board, and the materials include modified graphite flame retardant, polymer flexible waterproof material, anti-cracking waterproof mortar, insulation material and decorative material.
[0149] Experimental process:
[0150] S1. Sample preparation: prepare 5 samples of the prior art and 5 samples of the present invention;
[0151] S2. Structural stability test: Perform compression test on the sample and record its deformation;
[0152] S3. Construction efficiency test: simulate the construction process and record the construction time of each sample.
[0153] Test conditions: ambient temperature 25°C, humidity 50%.
[0154] Experimental data:
[0155]
[0156]
[0157] Summarize:
[0158] The present invention is significantly superior to the prior art in terms of structural stability and has a smaller deformation; the construction efficiency is greatly improved and the construction time is greatly reduced, indicating that it has obvious advantages in terms of construction convenience and efficiency.
[0159] Summary:
[0160] Through the above three comparative experiments, the composite roof insulation board of the present invention is significantly superior to the existing technology in many aspects such as waterproof, crack resistance, thermal insulation, fire resistance, structural stability and construction efficiency, which fully demonstrates its technical advantages and practical application value. These comparative experiments and data provide strong support and verification for the superior performance of the present invention.
[0161] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A composite roof insulation board, characterized in that: The composition materials include: 1 to 5 parts of modified graphite flame retardant, 20 to 40 parts of polymer flexible waterproof material, 10 to 30 parts of anti-cracking waterproof mortar, 40 to 60 parts of thermal insulation material and 5 to 15 parts of decorative material.
2. A composite roof insulation board according to claim 1, characterized in that: The graphite flame retardant includes graphite powder and flame retardant, and the addition ratio of the graphite powder and the flame retardant is 1:
2. The flame retardant includes aluminum hydroxide and brominated flame retardant, and the addition ratio of the aluminum hydroxide and the brominated flame retardant is 3:
1. The polymer flexible waterproof material includes polyurethane and flexible additives, and the addition ratio of the polyurethane and the flexible additive is 3:
1. The flexible additive includes polyacrylate and plasticizer, and the addition ratio of the polyacrylate and the plasticizer is 2:
1.
3. A composite roof insulation board according to claim 1, characterized in that: The anti-cracking and waterproof mortar includes cement and polymer additives, and the addition ratio of the cement and polymer additives is 3:
1. The polymer additive includes emulsion and cellulose, and the addition ratio of the emulsion and cellulose is 3:
1.
4. A composite roof insulation board according to claim 1, characterized in that: The thermal insulation material comprises polystyrene foam and a reinforcing agent, wherein the polystyrene foam and the reinforcing agent are added in a ratio of 4:1; the reinforcing agent comprises silicate and a foaming agent, wherein the silicate and the foaming agent are added in a ratio of 2:
1.
5. The composite roof insulation board according to claim 1, characterized in that: The decorative material includes ceramic particles and a binder, the ceramic particles and the binder are added in a ratio of 1:1, the binder includes a cement-based binder and rubber powder, the cement-based binder and the rubber powder are added in a ratio of 2:1, the cement-based binder includes silicate cement and fine aggregate, the silicate cement and the fine aggregate are added in a ratio of 3:
1.
6. A method for preparing a composite roof insulation board, according to the composite roof insulation board according to claims 1-4, characterized in that: The following steps are involved: S1. Prepare materials: prepare graphite flame retardant, polymer flexible waterproof material, anti-cracking waterproof mortar, thermal insulation material and decorative material; S2, stacking and pressing: first, the graphite flame retardant is evenly spread in the bottom mold, and pressed into shape by a pressing machine, and then the polymer flexible waterproof layer, the anti-cracking waterproof mortar layer, the thermal insulation layer and the decorative material layer are laid in sequence, and pressed by a hydraulic press, and the thermal insulation layer and the decorative material layer are also rubbed layer by layer; S3, template curing: place the pressed board template and materials at room temperature for curing for 24 hours; S4, beautification cutting: the solidified plate is polished by a grinder and cut by a laser cutting machine according to the required size; S5. Quality inspection: Use inspection instruments to conduct quality inspection on the cut boards, including waterproof performance test, crack resistance test and thermal insulation performance test.
7. The method for preparing a composite roof insulation board according to claim 6, characterized in that: In the step S2, the operating pressure of the laminating machine is 5MPa-10MPa, and the operating temperature of the laminating agent is 50°C-70°C.
8. The method for preparing a composite roof insulation board according to claim 6, characterized in that: In the step S4, the rotation speed of the grinder is 966RPM-2900RPM, and the diameter of the grinding disc of the grinder is 150mm.
9. The method for preparing a composite roof insulation board according to claim 6, characterized in that: In the step S4, the laser wavelength of the laser cutting machine is 1015nm-1065nm, and the cutting accuracy of the laser cutting machine is ±0.1mm.
10. The method for preparing a composite roof insulation board according to claim 6, characterized in that: In the step S5, the inspection instrument group includes a water permeability tester, a universal material testing machine and a thermal conductivity tester.