Quantitative evaluation method for absorption time of auxiliary agent in production process of packaging adhesive film for photovoltaic module
By quantitatively evaluating the additive absorption time and vulcanization speed index, the problem of the lack of effective evaluation methods in the existing technology is solved, the photovoltaic film production efficiency is improved, the film factory is helped to screen out efficient additives, and the processing efficiency is improved.
Patent Information
- Application Number
- CN202410816687.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-08
AI Technical Summary
There is a lack of effective quantitative evaluation method of additive absorption time in the existing technology, which affects the production efficiency of photovoltaic film and the control of POE particle production efficiency of different manufacturers.
Using the quantitative evaluation method of additive absorption time, the matrix resin and additives are fully mixed and then matured at a constant temperature, the additive absorption time is recorded, and the vulcanization speed index is calculated through the vulcanization process to determine the additive absorption time to screen out the additive absorption Faster base resin.
The relationship between the additive absorption time and the vulcanization speed index is established, which helps the film factory to quickly screen out the matrix resin with faster additive absorption speed, and improves the film processing efficiency.
Smart Images

Figure CN118746677A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic application field, and specifically to a quantitative evaluation method for auxiliary agent absorption time in the production process of packaging adhesive film. Background Art
[0002] Against the backdrop of global warming and the depletion of fossil energy, the development and utilization of renewable energy has received increasing attention from the international community, and vigorously developing renewable energy has become a consensus among countries around the world. The photovoltaic industry is of great significance to sustainable development. With the development of my country's economy, energy shortages and environmental damage are becoming increasingly serious, and the photovoltaic industry is booming. The photovoltaic industry not only helps to meet energy needs and reduce carbon emissions, but also provides sustainable clean energy. In addition, the renewability of photovoltaic power generation systems also enables them to operate stably in the long term. Therefore, the development of the photovoltaic industry is of positive significance to promoting sustainable development.
[0003] Photovoltaic film is one of the core materials of photovoltaic modules. Although the cost of film only accounts for about 7% of the module cost, it is a key factor in determining the quality and life of photovoltaic modules. At present, the demand for photovoltaic film is huge. Improving the production efficiency of photovoltaic film is an important direction for film factories to reduce costs and improve efficiency. At present, the key step affecting the production efficiency of photovoltaic film is the absorption time of additives. Taking POE as an example, there is no quantitative evaluation method for the absorption time of additives of POE products with the same melt index from different manufacturers. This seriously affects the film customers' grasp of the production efficiency of POE particles from different manufacturers. In view of this, it is necessary to provide a quantitative evaluation method for evaluating the absorption performance of POE additives, so as to provide an effective reference for the selection of formulation additives and resin particles in POE photovoltaic films. Summary of the invention
[0004] In view of the above problems in the prior art, the present invention provides a quantitative evaluation method for the absorption time of additives in the production process of encapsulation films for photovoltaic modules, thereby providing an effective reference for the structural selection of formulation additives and resin particles in POE photovoltaic films.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a quantitative evaluation method for the absorption time of an additive in a production process of an encapsulation film, comprising the following steps:
[0007] (1) fully mixing the matrix resin samples of several encapsulation films with the additives and subjecting them to constant temperature aging;
[0008] (2) At regular intervals, one of the matrix resin samples is taken out and the unabsorbed additive on the surface of the sample is removed for later use, and the additive absorption time of the sample is recorded;
[0009] (3) After the surface of the matrix resin sample is dry, the constant temperature aging step is terminated, and each of the matrix resin samples taken out is molded to obtain a sample;
[0010] (4) The sample is vulcanized at 145-150°C for 15-20 minutes, and the vulcanization rate index V is calculated according to the following formula: c ;
[0011] V c =100 / (t 90 -t sx )
[0012] Among them, t 90 The time taken to reach 90% vulcanization degree, t sx is the initial vulcanization time (scorch time);
[0013] (5) Compare the vulcanization speed indexes of the various samples, and the additive absorption time corresponding to the sample with the fastest vulcanization speed index is the additive absorption time of the base resin.
[0014] The vulcanization treatment mentioned in the quantitative evaluation method of the present invention is well known to those skilled in the art, and the specific process is explained in conjunction with GB / T16584-1996: Place the sample in a completely closed or almost completely closed mold cavity and keep it at the test temperature. The mold cavity has two parts, an upper and a lower part, one of which oscillates with a small linear reciprocating motion or a swing angle. The oscillation causes shear strain in the sample, and the reaction torque (force) of the sample on the mold cavity is measured. This torque (force) depends on the shear modulus of the sample. At the beginning of vulcanization, the shear modulus of the sample increases. When the recorded torque (force) rises to a stable value or a maximum value, a curve of the relationship between torque (force) and time is obtained, that is, the vulcanization curve (such as Figure 1 ). The shape of the curve is related to the test temperature and the characteristics of the specimen. Figure 1 The symbols used in can be combined with the vulcanization curve ( Figure 2 ) is understood. From the vulcanization curve Figure 1 and Figure 2 The following data can be read: F L is the minimum torque or force, in N·m or N; F max The flat, maximum, highest torque or force achieved within a specified time; t sx is the initial vulcanization time (scorch time), that is, from the start of the test to the curve from F L The time corresponding to the rise to x N·m(N), in min; t c (y) is the time required to reach a certain degree of vulcanization. Usually y has three common values 10, 50, and 90. For example, t 90The time required to reach 90% vulcanization degree (optimal vulcanization time).
[0015] In step (1) of the quantitative evaluation method of the present invention, the base resin sample is selected from ethylene-α-olefin copolymer, EVA resin, PVB resin; the auxiliary agent is selected from cross-linking agent, auxiliary cross-linking agent and coupling agent.
[0016] In some specific embodiments, the raw materials are mixed according to the following ratio: 100 parts by weight of base resin sample, 0.1-1.7 parts by weight of cross-linking agent, 0.3-1 parts by weight of auxiliary cross-linking agent and 0.1-0.7 parts by weight of silane coupling agent; in some preferred embodiments, the raw materials are mixed according to the following ratio: 100 parts by weight of base resin sample, 0.6-1.2 parts by weight of cross-linking agent, 0.3-0.7 parts by weight of auxiliary cross-linking agent and 0.1-0.5 parts by weight of silane coupling agent.
[0017] In some specific embodiments, the constant temperature aging is carried out at 40-55°C (eg, 45°C, 50°C, 52°C).
[0018] In some specific implementations, the matrix resin sample is taken out every 10 to 15 minutes, and the unabsorbed additives on the surface of the matrix resin sample are wiped with oil-absorbing cotton or oil-absorbing paper to remove the additives from the surface.
[0019] In some specific embodiments, the temperature of the compression molding in step (3) of the present invention is 85-95°C, for example, 90°C, 92°C; the time of the compression molding is 10-20 min, 15 min, 18 min.
[0020] In the quantitative evaluation method of the present invention, the crosslinking agent used can be selected from peroxide crosslinking agents; the auxiliary crosslinking agent is selected from one or more multifunctional acrylate substances; and the coupling agent is selected from silane coupling agents.
[0021] In some specific embodiments, the cross-linking agent is selected from one or more of tert-butyl peroxy isopropyl carbonate, 2,5-dimethyl-2,5-(bis-tert-butylperoxy)hexane, tert-butyl peroxy carbonate-2-ethylhexyl ester, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy 2-ethylhexyl carbonate, tert-amyl peroxy carbonate, or tert-butyl peroxy 3,3,5-trimethylhexanoate.
[0022] In some specific embodiments, the auxiliary cross-linking agent is selected from one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tris(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, ditrimethylolpropane tetraacrylate, ditrimethylolpropane tetramethacrylate, propoxylated pentaerythritol tetraacrylate, tricyclohexane dimethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A, dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate or polyethylene glycol dimethacrylate.
[0023] In some specific embodiments, the coupling agent is selected from one or more of γ-chloropropylmethoxysilane, vinylethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, γ-glycidyloxypropyltrimethoxysilane, 3-(trimethoxysilyl)propyl-2-methyl-2-acrylate, anilinemethyltriethoxysilane or octyltrimethoxysilane.
[0024] The above technical solution has the following technical effects:
[0025] The quantitative evaluation method of the present invention establishes a connection between the auxiliary agent absorption time and the vulcanization speed index for the first time, and establishes a quantitative evaluation method for the auxiliary agent absorption of the matrix resin. By comparing the time taken to reach the fastest vulcanization speed index between different matrix resins, the shorter the time to reach the fastest vulcanization speed index, the faster the auxiliary agent absorption speed and the faster the corresponding film processing efficiency.
[0026] The quantitative evaluation method of the present invention can help adhesive film manufacturers to more quickly screen out adhesive film base resins with faster auxiliary agent absorption speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 : Vulcanization curve 1;
[0028] Figure 2 : Vulcanization curve 2. DETAILED DESCRIPTION
[0029] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0030] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0031] Source of raw materials:
[0032] Ethylene-octene copolymer A: 8660, manufacturer: Dow Chemical;
[0033] Ethylene-octene copolymer B: 8669, manufacturer: Dow Chemical;
[0034] Ethylene-butene copolymer C: LF575, manufacturer: LG;
[0035] Ethylene-butene copolymer D: LF675, manufacturer: LG;
[0036] Tert-butyl peroxy 3,3,5-trimethylhexanoate, Nourylon, purity 98%;
[0037] Triallyl isocyanurate, Acros, purity 98%;
[0038] Vinyltrimethoxysilane, Adamas, purity 98%;
[0039] tert-Butyl peroxycarbonate-2-ethylhexyl ester, Nourylon, purity 98%;
[0040] Tris(2-hydroxyethyl)isocyanurate triacrylate, sigima;
[0041] tert-Amyl peroxy-2-ethylhexyl carbonate, Nourylon, purity 98%;
[0042] Ethoxylated glycerol triacrylate, Shanghai Qiqiao Biotechnology Co., Ltd., purity 98%;
[0043] Vinyl triacetoxysilane, sigima;
[0044] Ethoxylated trimethylolpropane triacrylate, sigima;
[0045] γ-Glycidyloxypropyltrimethoxysilane, sigima.
[0046] The following examples of the present invention adopt the following detection method:
[0047] Vulcanization rate index: measured in accordance with GB / T16584-1996.
[0048] Example 1
[0049] (1) 200 g of a plurality of base resin samples of ethylene-octene copolymer A were fully mixed with 1.8 g of tert-butyl peroxidized 3,3,5-trimethylhexanoate, 1.4 g of triallyl isocyanurate and 0.2 g of vinyltrimethoxysilane, and then aged in an oven at a constant temperature of 50° C.;
[0050] (2) Take out one of the matrix resin samples every 10 minutes and wipe the unabsorbed additives on the surface with oil-absorbing cotton or oil-absorbing paper, and record the additive absorption time of the sample and set it aside;
[0051] (3) After the surface of the matrix resin sample during constant temperature aging is dry (i.e., the additive is completely absorbed), the constant temperature aging is terminated, and the matrix resin taken out each time is compression molded at 90° C. for 10 minutes to obtain a sample;
[0052] (4) Each sample after molding was vulcanized at 145°C for 15 min and then c =100 / (T90-T sx ) to calculate the vulcanization rate index V c (Specific details are shown in Table 1 below);
[0053] Table 1
[0054] Sample number Absorption time (min) Tsx(min) T90(min) Vc( / min) 1 50 4.8 12.29 13.351 2 60 4.78 12.21 13.459 3 70 4.72 12.13 13.495 4 80 4.71 12.12 13.495 5 90 4.71 12.12 13.495 6 100 4.72 12.13 13.495
[0055] By comparing the vulcanization speed index Vc of each sample in the above table, it can be seen that the additive absorption time corresponding to sample No. 3 which reaches the fastest vulcanization speed index (13.495 / min) is 70 minutes, that is, the additive absorption time of the ethylene-octene copolymer A is 70 minutes.
[0056] Example 2
[0057] (1) 200 g of a base resin sample of ethylene-octene copolymer B was fully mixed with 2.4 g of tert-butyl peroxycarbonate-2-ethylhexyl ester, 0.8 g of tris(2-hydroxyethyl)isocyanurate triacrylate and 0.2 g of vinyltrimethoxysilane, and then aged in an oven at a constant temperature of 50° C.;
[0058] (2) Take out one of the matrix resin samples every 10 minutes and wipe the unabsorbed additives on the surface with oil-absorbing cotton or oil-absorbing paper, and record the additive absorption time of the sample and set it aside;
[0059] (3) After the surface of the matrix resin sample during constant temperature aging is dry (i.e., the additive is completely absorbed), the constant temperature aging is terminated, and the matrix resin taken out each time is compression molded at 90° C. for 10 minutes to obtain a sample;
[0060] (4) Each sample after molding was vulcanized at 145°C for 15 min and then c =100 / (T90-T sx ) to calculate the vulcanization rate index V c (Specific details are shown in Table 2 below);
[0061] Table 2
[0062] Sample number Absorption time (min) Tsx(min) T90(min) Vc( / min) 1 50 6.51 12.57 16.502 2 60 6.51 12.55 16.556 3 70 6.51 12.51 16.667 4 80 6.46 12.44 16.722 5 90 6.46 12.41 16.807 6 100 6.47 12.42 16.807 7 110 6.46 12.41 16.807 8 120 6.46 12.41 16.807
[0063] Compare the vulcanization speed index V of each sample in the above table c It can be seen that the additive absorption time corresponding to the No. 5 sample which reaches the fastest vulcanization speed index (16.807 / min) is 90 minutes, that is, the additive absorption time of the ethylene-octene copolymer B is 90 minutes.
[0064] Example 3
[0065] (1) 200 g of a plurality of base resin samples of ethylene-octene copolymer C were fully mixed with 1.4 g of tert-amyl peroxy 2-ethylhexyl carbonate, 1 g of ethoxylated glycerol triacrylate and 0.2 g of vinyl triacetoxy silane, and then aged in an oven at a constant temperature of 50° C.;
[0066] (2) Take out one of the matrix resin samples every 10 minutes and wipe the unabsorbed additives on the surface with oil-absorbing cotton or oil-absorbing paper, and record the additive absorption time of the sample and set it aside;
[0067] (3) After the surface of the matrix resin sample during constant temperature aging is dry (i.e., the additive is completely absorbed), the constant temperature aging is terminated, and the matrix resin taken out each time is compression molded at 90° C. for 10 minutes to obtain a sample;
[0068] (4) Each sample after molding was vulcanized at 145°C for 15 min and then c =100 / (T90-T sx ) to calculate the vulcanization rate index V c (Specifications are shown in Table 3 below);
[0069] Table 3
[0070] Sample number Absorption time (min) Tsx(min) T90(min) Vc( / min) 1 50 5.3 12.69 13.532 2 60 5.29 12.65 13.587 3 70 5.29 12.62 13.642 4 80 5.28 12.58 13.699 5 90 5.27 12.54 13.755 6 100 5.28 12.55 13.755 7 110 5.28 12.55 13.755 8 120 5.28 12.55 13.755
[0071] Compare the vulcanization speed index V of each sample in the above table c It can be seen that the additive absorption time corresponding to sample No. 5, which reaches the fastest vulcanization speed index (13.755 / min), is 90 minutes, that is, the additive absorption time of ethylene-octene copolymer C is 90 minutes.
[0072] Example 4
[0073] (1) 200 g of a plurality of base resin samples of ethylene-octene copolymer D were fully mixed with 1.6 g of tert-butyl peroxidized 3,3,5-trimethylhexanoate, 0.6 g of triallyl isocyanurate, 0.8 g of ethoxylated trimethylolpropane triacrylate, and 0.4 g of γ-glycidyloxypropyltrimethoxysilane, and then aged in an oven at a constant temperature of 50° C.;
[0074] (2) Take out one of the matrix resin samples every 10 minutes and wipe the unabsorbed additives on the surface with oil-absorbing cotton or oil-absorbing paper, and record the additive absorption time of the sample and set it aside;
[0075] (3) After the surface of the matrix resin sample during constant temperature aging is dry (i.e., the additive is completely absorbed), the constant temperature aging is terminated, and the matrix resin taken out each time is compression molded at 90° C. for 10 minutes to obtain a sample;
[0076] (4) Each sample after molding was vulcanized at 145°C for 15 min and then c =100 / (T90-T sx ) to calculate the vulcanization rate index V c (Specifications are shown in Table 4 below);
[0077] Table 4
[0078]
[0079]
[0080] By comparing the vulcanization speed index Vc of each sample in the above table, it can be seen that the additive absorption time corresponding to sample No. 7 which reaches the fastest vulcanization speed index (15.649 / min) is 110 minutes, that is, the additive absorption time of the ethylene-octene copolymer D is 110 minutes.
[0081] Comparative Example
[0082] (1) 200 g of a plurality of base resin samples of ethylene-octene copolymer B were fully mixed with 2.4 g of tert-butyl peroxycarbonate-2-ethylhexyl ester, 0.8 g of tris(2-hydroxyethyl)isocyanurate triacrylate and 0.2 g of vinyltrimethoxysilane, and then aged in an oven at a constant temperature of 50° C.;
[0083] (2) Take out one of the matrix resin samples every 10 minutes without wiping off the unabsorbed additive on the surface of the matrix resin sample, record the additive absorption time of the matrix resin, and keep it for later use;
[0084] (3) When the surface of the matrix resin sample in the constant temperature aging process is dry, the constant temperature aging process is stopped, and the matrix resin taken out each time is compression molded at 90° C. for 10 minutes to obtain a sample;
[0085] (4) Each sample after molding was vulcanized at 145°C for 15 min. c =100 / (T90-T sx ) to calculate the vulcanization rate index V c (Specifications are shown in Table 5 below);
[0086] Table 5
[0087] Sample number Absorption time (min) Tsx(min) T90(min) Vc( / min) 1 50 6.51 12.57 16.502 2 60 6.48 12.55 16.474 3 70 6.51 12.51 16.667 4 80 6.46 12.54 16.447 5 90 6.46 12.44 16.722 6 100 6.47 12.50 16.584 7 110 6.45 12.40 16.807 8 120 6.46 12.41 16.807
[0088] Compare the vulcanization speed index V of each sample in the above table c It can be seen that since the additives were not wiped off and remained on the particle surface, the vulcanization speed index fluctuated significantly during the aging process without obvious regularity. The vulcanization speed index of the examples gradually accelerated with the extension of time, while the comparative examples did not have such a correlation regularity. Compared with the above-mentioned Example 2, the fastest vulcanization speed index should have been reached in 90 minutes, but due to large fluctuations, it was not until 110 minutes that it reached equilibrium.
Claims
1. A quantitative evaluation method for the absorption time of additives in the production process of encapsulation films for photovoltaic modules, characterized in that: The following steps are involved: (1) fully mixing the matrix resin samples of several encapsulation films with the additives and subjecting them to constant temperature aging; (2) taking out one of the matrix resin samples at regular intervals to remove the unabsorbed additive on the surface, and recording the additive absorption time of the sample for later use; (3) stopping the constant temperature aging process after the surface of the matrix resin sample in the constant temperature aging is dry, and molding each of the matrix resin samples taken out to obtain a sample; (4) The sample is vulcanized at 145-150°C for 15-20 minutes, and the vulcanization rate index V is calculated according to the following formula: c ; V c =100 / (t 90 -t sx ) Among them, t 90 The time taken to reach 90% vulcanization degree, t sx is the initial vulcanization time; (5) Compare the vulcanization speed index V of each sample c The additive absorption time corresponding to the sample that first reaches the fastest vulcanization speed index is the additive absorption time of the base resin sample.
2. The quantitative evaluation method according to claim 1, characterized in that: The matrix resin sample is selected from ethylene-α-olefin copolymer, EVA resin, and PVB resin; The auxiliary agent is selected from a cross-linking agent, a co-cross-linking agent and a coupling agent.
3. The quantitative evaluation method according to claim 2, characterized in that: In step (1), the raw materials are mixed according to the following ratio: 100 parts by weight of the base resin sample, 0.1 to 1.7 parts by weight of the cross-linking agent, 0.3 to 1 parts by weight of the auxiliary cross-linking agent and 0.1 to 0.7 parts by weight of the silane coupling agent; Preferably, 100 parts by weight of the base resin sample, 0.6 to 1.2 parts by weight of the cross-linking agent, 0.3 to 0.7 parts by weight of the auxiliary cross-linking agent and 0.1 to 0.5 parts by weight of the silane coupling agent.
4. The quantitative evaluation method according to any one of claims 1 to 3, characterized in that: In step (1), the constant temperature aging is carried out at 40-55°C.
5. The quantitative evaluation method according to any one of claims 1 to 4, characterized in that: In step (2), the matrix resin sample is taken out every 10 to 15 minutes, and the unabsorbed additives on the surface of the matrix resin sample are wiped with oil-absorbing cotton or oil-absorbing paper.
6. The quantitative evaluation method according to claim 5, characterized in that: In step (3), the temperature of the compression molding is 85 to 95° C., and the time of the compression molding is 10 to 20 minutes.
7. The quantitative evaluation method according to any one of claims 1 to 6, characterized in that: The cross-linking agent is selected from peroxide cross-linking agents; The auxiliary cross-linking agent is selected from one or more multifunctional acrylate substances; The coupling agent is selected from silane coupling agents.
8. The quantitative evaluation method according to any one of claims 1 to 7, characterized in that: The cross-linking agent is selected from the group consisting of tert-butyl isopropyl peroxycarbonate, 2,5-dimethyl-2,5-(bis-tert-butylperoxy)hexane, tert-butyl peroxycarbonate-2-ethylhexyl ester, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-amylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy-2-ethylhexyl carbonate, tert-amyl peroxycarbonate, or one or more tert-butyl peroxy-3,3,5-trimethylhexanoate.
9. The quantitative evaluation method according to any one of claims 1 to 8, characterized in that: The auxiliary cross-linking agent is selected from one or more of triallyl isocyanurate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylolpropane triacrylate, ethoxylated glycerol triacrylate, propoxylated glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, ditrimethylolpropane tetraacrylate, ditrimethylolpropane tetramethacrylate, propoxylated pentaerythritol tetraacrylate, tricyclohexane dimethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A, dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate or polyethylene glycol dimethacrylate.
10. The quantitative evaluation method according to any one of claims 1 to 9, characterized in that: The coupling agent is selected from one or more of γ-chloropropylmethoxysilane, vinyltrimethoxysilane, vinylethoxysilane, vinyltri(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, γ-glycidyloxypropyltrimethoxysilane, 3-(trimethoxysilyl)propyl-2-methyl-2-acrylate, anilinemethyltriethoxysilane or octyltrimethoxysilane.
Citation Information
Cited By
Polyolefin elastomer for photovoltaic packaging film, preparation method and application
CN121362278A
A polyolefin elastomer for photovoltaic encapsulation films, its preparation method and application
CN121362278B