Antioxidant conductive copper paste and preparation method thereof

By coating the surface of copper powder with thermoplastic resin to form an antioxidant layer, and combining it with silver iodide powder, an antioxidant conductive copper paste is prepared, which solves the problems of easy oxidation and insufficient conductivity of copper, achieving efficient conductivity and cost reduction.

CN118748098APending Publication Date: 2024-10-08SHANGHAI SILVER PASTE SCI & TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410780058.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Copper is easily oxidized in the air, resulting in reduced electrical conductivity. In the existing technology, silver-coated copper or chemical modification treatments are costly and have unstable effects, making it difficult to effectively improve the oxidation resistance and electrical conductivity of copper paste.

Method used

The copper powder is surface-coated with the first thermoplastic resin to form an antioxidant layer, and the antioxidant copper powder is combined with a thermosetting resin, auxiliary conductive agent, curing agent, etc. to prepare an antioxidant conductive copper paste, which is enhanced with silver iodide powder. Conductivity.

Benefits of technology

It significantly improves the oxidation resistance and conductivity of copper paste, reduces production costs, replaces silver powder, and forms excellent conductivity and oxidation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748098A_ABST
    Figure CN118748098A_ABST
Patent Text Reader

Abstract

The invention discloses antioxidant conductive copper paste and a preparation method thereof. The preparation method comprises the following steps: step 1, copper powder treatment: cleaning copper powder with an acid solution, and drying for later use; step 2, preparation of antioxidant copper powder: heating and dissolving first thermoplastic resin in a first organic solvent to form coating liquid, adding the dried copper powder into the coating liquid, and evaporating to remove the first organic solvent to obtain the antioxidant copper powder; and step 3, mixing the prepared antioxidant copper powder with thermosetting resin, second thermoplastic resin, an auxiliary conductive agent, a curing agent, a coupling agent and a second organic solvent, and grinding to obtain the antioxidant copper paste. The conductive copper paste solves the problem that the conductivity of the copper paste is poorer than that of the silver paste, and the oxidation resistance and conductivity of the conductive copper paste are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar cells, and in particular to an anti-oxidation conductive copper paste and a preparation method thereof. Background Art

[0002] At present, the mainstream market mainly uses silver powder as a conductive filler to prepare conductive paste. Silver paste has excellent conductivity and oxidation resistance. However, silver is expensive, which greatly hinders the widespread application and development of silver paste. Copper's conductivity is second only to silver and its price is relatively low. It has certain applications in electronic packaging and electronic components, such as copper as the terminal electrode of multi-layer ceramic capacitors, or circuit boards made of copper paste and ceramic substrates. However, copper is easily oxidized in the air and easily forms an oxide film layer on the surface. The oxide film layer has a high resistivity and reduced conductivity, which greatly reduces its practicality. The easy oxidation property of copper has become a bottleneck in the development of copper paste.

[0003] To address the issue of copper's easy oxidation, a common method in the prior art is to coat or chemically plate the copper powder with an anti-oxidation metal shell, such as silver-coated copper powder. However, the use of silver increases the cost of the conductive paste. Another method involves chemically modifying the copper powder surface. This chemical modification is easily damaged during subsequent operations of the conductive copper paste, thereby reducing its oxidation resistance, and the technology needs to be improved. To address the problem that copper paste has inferior electrical properties to silver paste, a common method in the prior art is to add other conductive fillers, such as graphene, carbon nanotubes, and carbon black, to the copper paste. However, due to their large specific surface area and difficulty in dispersion, the improvement in conductivity is not significant. Summary of the Invention

[0004] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide an antioxidant conductive copper paste and a preparation method thereof, which solves the problem that the conductivity of copper paste is not as good as that of silver paste and improves the antioxidant and conductivity of the conductive copper paste.

[0005] The purpose of the present invention is achieved through the following technical solutions:

[0006] The present invention provides a method for preparing an oxidation-resistant conductive copper paste, comprising the following steps:

[0007] Step 1: Copper powder treatment: The copper powder is cleaned with acid solution and dried for later use;

[0008] Step 2, preparing antioxidant copper powder: heating and dissolving a first thermoplastic resin in a first organic solvent to form a coating liquid, mixing the dried copper powder with the coating liquid, and evaporating and removing the first organic solvent to obtain antioxidant copper powder;

[0009] Step 3: Mix the antioxidant copper powder prepared above with a thermosetting resin, a second thermoplastic resin, an auxiliary conductive agent, a curing agent, a coupling agent, and a second organic solvent to obtain an antioxidant copper slurry.

[0010] Furthermore, in step 1, the particle size of the copper powder is 0.5-5 μm.

[0011] Furthermore, in step 2, the first thermoplastic resin forms an anti-oxidation layer on the surface of the copper powder, the thickness of the anti-oxidation layer is 4-7 nm, and the particle size of the anti-oxidation copper powder is 1-2 μm.

[0012] Furthermore, in step 2, in the coating liquid, the mass percentage of the first thermoplastic resin is 8 to 15%; and the mass ratio of the copper powder to the coating liquid is 1:4 to 6.

[0013] Furthermore, in step 2, the first thermoplastic resin is one or more of polycarbonate resin, cellulose acetate butyrate, ethyl cellulose, acrylic resin, polyester resin, and polyurethane resin.

[0014] Furthermore, in step 2, the second organic solvent is one or more of ethanol, diethylene glycol butyl ether acetate, dibasic acid ester, ethylene glycol diacetate, terpineol, dimethyl adipate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate.

[0015] Furthermore, in step 2, the first organic solvent is ethanol, and the first thermoplastic resin is one or more of cellulose acetate butyrate and ethyl cellulose.

[0016] Furthermore, in step 3, the contents of the components in the conductive copper paste are, by mass percentage, 85-90% of antioxidant copper powder, 3-5% of thermosetting resin, 0.1-0.5% of the second thermoplastic resin, 1-3% of the auxiliary conductive agent, 0.1-0.5% of the curing agent, 0.1-0.5% of the coupling agent, and 4-8% of the second organic solvent.

[0017] Furthermore, in step 3, the auxiliary conductive agent is one or more of silver iodide powder or silver powder.

[0018] The present invention also provides an anti-oxidation conductive copper paste, which is prepared by the above-mentioned preparation method.

[0019] The beneficial effects of the present invention are as follows: the surface of the copper powder is coated by the first thermoplastic resin to form an anti-oxidation layer on the surface of the copper powder, so that the anti-oxidation copper powder has excellent anti-oxidation properties, solving the problem that the original copper powder is easily oxidized; the conductive copper paste synthesized by the anti-oxidation copper powder has excellent conductivity, and the anti-oxidation copper powder replaces the original silver powder, greatly reducing the production cost.

[0020] Attached photos

[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 This is a 3D electron microscope image of the conductive copper paste after printing according to Example 1 of the present invention;

[0023] Figure 2 This is a 3D electron microscope image of the conductive copper paste after printing according to Example 2 of the present invention. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing an oxidation-resistant conductive copper paste, comprising the following steps:

[0025] Step 1: Copper powder treatment: The copper powder is cleaned with acid solution and dried for later use;

[0026] Step 2, preparing antioxidant copper powder: heating and dissolving a first thermoplastic resin in a first organic solvent to form a coating liquid, mixing the dried copper powder with the coating liquid, and evaporating and removing the first organic solvent to obtain antioxidant copper powder;

[0027] Step 3: Mix the antioxidant copper powder prepared above with a thermosetting resin, a second thermoplastic resin, an auxiliary conductive agent, a curing agent, a coupling agent, and a second organic solvent to obtain an antioxidant copper slurry.

[0028] In this embodiment, the copper powder is surface-coated with a first thermoplastic resin to form an anti-oxidation layer on the surface of the copper powder, so that the formed anti-oxidation copper powder has excellent anti-oxidation properties, solving the problem of easy oxidation of the original copper powder; the conductive copper paste synthesized by the anti-oxidation copper powder has excellent conductivity, and the anti-oxidation copper powder replaces the original silver powder, greatly reducing production costs.

[0029] Furthermore, in step 1, the copper powder has a particle size of 0.5-5 μm and a shape of spheres, flakes, dendrites, etc. Preferably, the copper powder has a particle size of 1-2 μm and a spherical shape. The copper powder is acid-washed using ultrasonic dispersion to remove surface oxides and organic impurities, and then dried in a vacuum oven until ready for use. The acid solution is one or more of dilute sulfuric acid and dilute hydrochloric acid, with a mass concentration of 7% to 9%.

[0030] Furthermore, in step 2, the first thermoplastic resin forms an antioxidant layer on the surface of the copper powder. The thickness of the antioxidant layer is 4-7 nm, and the particle size of the antioxidant copper powder is 1-2 μm. In the coating liquid, the mass percentage of the first thermoplastic resin is 8-15%. The higher the mass percentage of the first thermoplastic resin, the thicker the antioxidant layer. By adjusting the mass percentage of the first thermoplastic resin to obtain an optimal antioxidant layer thickness, the antioxidant copper powder has excellent oxidation resistance and conductivity, and avoids the formation of excessively large particles that affect subsequent printing. The mass ratio of copper powder to coating liquid is 1:4-6.

[0031] Wherein, the first thermoplastic resin is one or more of polycarbonate resin, cellulose acetate butyrate, ethyl cellulose, acrylic resin, polyester resin, and polyurethane resin; the first organic solvent is one or more of ethanol, diethylene glycol butyl ether acetate, divalent acid ester, ethylene glycol diacetate, terpineol, dimethyl adipate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate, and the second organic solvent can be removed by using a rotary evaporator to obtain antioxidant copper powder. Preferably, the second organic solvent is ethanol, and the first thermoplastic resin is one or more of cellulose acetate butyrate and ethyl cellulose. In the process of obtaining antioxidant copper powder, the solvent is removed by evaporation, and ethanol is easy to remove, making the copper powder drying process simple and not easy to leave organic matter. Ethanol is the best solvent for dissolving the first thermoplastic resin, and cellulose acetate butyrate and ethyl cellulose have good solubility in ethanol. A rotary evaporator is used to remove the first organic solvent to obtain pure antioxidant copper powder.

[0032] Furthermore, in step 3, the contents of the components in the conductive copper paste are, by mass percentage, 85-90% antioxidant copper powder, 3-5% thermosetting resin, 0.1-0.5% second thermoplastic resin, 1-3% auxiliary conductive agent, 0.1-0.5% curing agent, 0.1-0.5% coupling agent, and 4-8% second organic solvent.

[0033] Specifically, a thermosetting resin, a thermoplastic resin, a curing agent, an auxiliary conductive agent, a coupling agent, and a second organic solvent in appropriate proportions are weighed and mixed to obtain an organic carrier. Then, antioxidant copper powder is weighed and added to the organic carrier. After manual stirring, the mixture is stirred with a homogenizer, and finally ground with a three-roll mill to prepare an antioxidant copper slurry.

[0034] The antioxidant copper powder serves as the primary conductive agent, while the auxiliary conductive agent has conductivity superior to or equivalent to that of copper powder. The auxiliary conductive agent is either silver iodide powder or one or more of silver powder. Silver iodide powder also forms elemental silver upon thermal decomposition, and the addition of the auxiliary conductive agent enhances the conductivity of the copper paste. Alternatively, the auxiliary conductive agent can be the antioxidant copper powder mentioned above. Preferably, the auxiliary conductive agent is silver iodide powder. Silver iodide has α, β, and γ phases. At room temperature, the β and γ phases are relatively stable, while above 146°C, the α phase gradually becomes dominant. It is a body-centered cubic crystal with high conductivity. Thermal decomposition of silver iodide into elemental silver enhances contact between the copper powders, creating a synergistic effect with the copper powder, further enhancing the conductivity of the conductive copper paste and resolving the issue of copper paste being less conductive than silver paste. Furthermore, during the curing process of printing the electrode with the conductive copper paste, the silver elemental silver decomposed from the silver iodide has a small particle size and can be evenly dispersed in the gaps between the antioxidant copper powder, improving the conductive properties of the electrode.

[0035] Furthermore, in the conductive copper paste, the thermosetting resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, hydantoin epoxy resin, and phenolic epoxy resin; the second thermoplastic resin is one or more of polycarbonate resin, cellulose acetate butyrate, ethyl cellulose, acrylic resin, polyester resin, and polyurethane resin; the curing agent generally includes a thermal cationic curing agent, for example, amine-blocked hexafluoroantimonate and / or boron trifluoride-monoethylamine complex; the coupling agent is one or more of glycidoxypropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, glycidyloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and methacryloxypropyltrimethoxysilane; the second solvent is one or more of butyl carbitol, butyl carbitol acetate, terpineol, alcohol ester dodecahydrate, tributyl citrate, and diethylene glycol butyl ether acetate.

[0036] The addition of a second thermoplastic resin to the conductive copper paste, which is the same type of resin as the first thermoplastic resin added to prepare the antioxidant copper powder, can improve the dispersion of the antioxidant copper powder in the organic vehicle. Preferably, the second thermoplastic resin can be cellulose acetate butyrate, which not only shrinks the paste, improving its electrical properties, but also improves its leveling properties, resulting in a smoother printed paste line.

[0037] The present invention also provides an anti-oxidation conductive copper paste, which is prepared by the above-mentioned preparation method.

[0038] The beneficial effects of the present invention are:

[0039] 1. Use thermoplastic resin solution to coat the surface of copper powder to obtain antioxidant copper powder. An antioxidant layer is formed on the outer layer of the copper powder, which makes the antioxidant copper powder have excellent antioxidant properties and solves the problem of easy oxidation of the original copper powder.

[0040] 2. Add silver iodide to the conductive copper paste. Silver iodide has α, β and γ phases. At room temperature, β and γ phases are relatively stable. Above 146°C, α phase will gradually become dominant. It is a body-centered cubic crystal with high conductivity. Silver iodide decomposes into silver when heated, which enhances the contact between copper powders and forms a synergistic effect with copper powder, further improving the conductivity of the conductive copper paste and solving the problem that copper paste is less conductive than silver paste.

[0041] 3. Adding a second thermoplastic resin to the conductive copper paste, which is the same type of resin as the first thermoplastic resin added to prepare the antioxidant copper powder, can improve the dispersion performance of the antioxidant copper powder in the organic carrier.

[0042] The present invention will be further explained below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0043] Example 1:

[0044] Step 1: Weigh spherical copper powder with an average particle size of 1.5 μm and pickle it by ultrasonic dispersion. The pickling solution is 8% by mass of dilute sulfuric acid to remove oxides and organic impurities on the surface of the copper powder. Then wash and filter it with deionized water. Finally, bake it in a vacuum oven at 50°C for 2 to 3 hours to obtain copper powder with a clean surface for use.

[0045] Step 2: First weigh cellulose acetate butyrate resin and heat it to dissolve it in ethanol to obtain a coating solution. The mass percentage of cellulose acetate butyrate resin is 10%. Add copper powder with a clean surface to the coating solution. The mass ratio of copper powder to coating solution is 1:5. Use a rotary evaporator to remove the ethanol and water to obtain antioxidant copper powder.

[0046] Step 3: Weigh bisphenol A epoxy resin, cellulose acetate butyrate resin, amine-blocked hexafluoroantimonate, glycidoxypropyltrimethoxysilane, silver iodide, and diethylene glycol butyl ether acetate in a ratio of 4:0.2:0.5:0.3:2:4 by mass and mix them. Weigh 89 parts by mass of the antioxidant copper powder obtained in step 2 and add it to the mixed organic carrier. After manual stirring, stir with a homogenizer and finally grind with a three-roll mill to prepare an antioxidant copper slurry.

[0047] Example 2

[0048] Compared with Example 1, step 1 remains unchanged;

[0049] In steps 2 and 3, cellulose acetate butyrate is replaced by ethyl cellulose, and the rest remain unchanged.

[0050] Example 3

[0051] Compared with Example 1, steps 1 and 2 are the same;

[0052] In step 3, the cellulose acetate butyrate resin is replaced with polyester resin, and the other conditions remain unchanged.

[0053] Example 4

[0054] Compared with Example 1, steps 1 and 2 are the same;

[0055] In step 3, silver iodide was replaced with silver powder with an average particle size of 1.5 μm, and the other parameters remained unchanged.

[0056] Example 5

[0057] Compared with Example 1, steps 1 and 2 are the same;

[0058] In step 3, silver iodide is removed, that is, silver iodide is replaced by antioxidant copper powder, and the total mass parts of the antioxidant copper powder become 91 parts, and the other parts remain unchanged.

[0059] Comparative Example 1

[0060] Compared with Example 1, steps 1 and 2 are the same;

[0061] In step 3, the cellulose acetate butyrate resin is removed, that is, the cellulose acetate butyrate resin is replaced by bisphenol A epoxy resin, and the mass parts of the bisphenol A epoxy resin are changed to 4.2 parts, and the other parts remain unchanged.

[0062] Comparative Example 2

[0063] Compared with Example 1, there is no step 1 or step 2;

[0064] In step 3, the antioxidant copper powder is replaced with copper powder, the average particle size of the copper powder is 1.5 μm, and the shape is spherical. Other factors remain unchanged.

[0065] Comparative Example 3

[0066] Compared with Example 1, there is no step 1 or step 2;

[0067] In step 3, the antioxidant copper powder is replaced with silver powder. The average particle size of the silver powder is 1.5 μm and the shape is spherical. Other parameters remain unchanged.

[0068] The conductive pastes of Examples 1 to 5 and Comparative Examples 1 to 3 were used as samples. Each sample was printed on the same substrate for relevant property tests. The curing conditions were 200° C. for 8 minutes. The test process was as follows:

[0069] 1. Resistivity test: Use a four-probe ohmmeter to test the resistance at both ends of the electrode.

[0070] 2. Viscosity test: The viscosity test is carried out using a Brookfield viscometer at a speed of 10 rpm to test the viscosity value after stirring for 4 minutes.

[0071] 3. Contact resistance: Print a specific pattern of low-temperature silver paste on the heterojunction cell and then dry and solidify it; use a laser slicer to cut out the cell of a specified size in the printed pattern area; use a contact resistance device to measure the contact resistance.

[0072] Table 1 Results of resistivity test, viscosity test and contact resistance test

[0073]

[0074]

[0075] Combined with Table 1, we can see through analysis that:

[0076] It can be concluded from Examples 1-3 and Comparative Example 1 that the electrical properties of Examples 1-3 are better than those of Comparative Example 1, that is, adding a thermoplastic resin of the same type as the antioxidant layer on the outside of the antioxidant copper powder to prepare the antioxidant conductive copper paste can not only improve the dispersion performance of the antioxidant copper powder in the organic carrier, but also such thermoplastic resin can play a shrinking role, thereby improving the electrical properties of the conductive copper paste;

[0077] From Examples 1, 4, 5 and Comparative Example 2, it can be concluded that the electrical conductivity of Examples 1 and 4 is better than that of Example 5, that is, when a small amount of auxiliary conductive agent, silver iodide powder or silver powder, is added to the copper paste, the electrical conductivity of the conductive copper paste is better than that of the conductive copper paste in which the auxiliary conductive agent is antioxidant copper, and the electrical conductivity of Example 1 is better than that of Example 4, and the electrical conductivity of Example 1 is similar to that of Comparative Example 2, that is, the conductive copper paste prepared by combining silver iodide powder with antioxidant copper powder can completely replace the conductive silver paste prepared by the original silver powder, greatly reducing the production cost; the silver iodide powder decomposes into silver element when heated, which plays a role in melting and connecting the antioxidant copper powder, filling the gaps between the antioxidant copper powders, and the silver iodide changes from the β phase to the α phase, which is a body-centered cubic crystal with higher electrical conductivity, thereby enhancing the contact between the antioxidant copper powders and forming a synergistic effect with the antioxidant copper powder, further improving the electrical conductivity of the conductive copper paste;

[0078] As can be seen from Examples 1 and 4, replacing the silver iodide powder in the slurry with silver powder increases both the bulk resistance and the contact resistance. The silver iodide powder decomposes into silver when heated, which can melt-connect the antioxidant copper powder and fill the gaps between the antioxidant copper powders. The silver powder is too large and cannot melt-connect, making the conductivity of Example 4 worse than that of Example 1.

[0079] It can be concluded from Examples 1, 2 and Comparative Example 3 that the copper powder is surface-coated with cellulose acetate butyrate and ethyl cellulose to form an antioxidant layer on the outer layer of the copper powder, so that the antioxidant copper powder has excellent antioxidant properties, while the ordinary copper powder in Comparative Example 3 is easily oxidized, resulting in increased body resistance and contact resistance of Comparative Example 3 and poor conductivity.

[0080] Combine Figure 1 and Figure 2 It can be concluded that the printing effect of Example 1 is better than that of Example 2, and the printed slurry is smoother, which means that cellulose acetate butyrate can improve the leveling performance of the slurry, making the printed slurry line smoother.

[0081] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same and similar parts between the various embodiments can be referenced to each other.

[0082] The above description is merely a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with this profession can make some changes or modifications to the technical contents disclosed above without departing from the scope of the technical solution of the present invention, which are equivalent embodiments of equivalent changes. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing an anti-oxidation conductive copper paste, characterized in that: The following steps are involved: Step 1, copper powder treatment: the copper powder is cleaned with acid solution and dried for standby use; Step 2, preparation of antioxidant copper powder: heating and dissolving a first thermoplastic resin in a first organic solvent to form a coating liquid, mixing the dried copper powder and the coating liquid, and evaporating and removing the first organic solvent to obtain the antioxidant copper powder; Step 3: Mix the antioxidant copper powder prepared above with a thermosetting resin, a second thermoplastic resin, an auxiliary conductive agent, a curing agent, a coupling agent, and a second organic solvent to obtain an antioxidant copper slurry.

2. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 1, the particle size of the copper powder is 0.5-5 μm.

3. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 2, the first thermoplastic resin forms an anti-oxidation layer on the surface of the copper powder, the thickness of the anti-oxidation layer is 4-7 nm, and the particle size of the anti-oxidation copper powder is 1-2 μm.

4. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 2, in the coating liquid, the mass percentage of the first thermoplastic resin is 8-15%; the mass ratio of the copper powder to the coating liquid is 1:4-6.

5. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 2, the first thermoplastic resin is one or more of polycarbonate resin, cellulose acetate butyrate, ethyl cellulose, acrylic resin, polyester resin, and polyurethane resin.

6. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 2, the second organic solvent is one or more of ethanol, diethylene glycol butyl ether acetate, dibasic acid ester, ethylene glycol diacetate, terpineol, dimethyl adipate, ethylene glycol ethyl ether acetate, and propylene glycol methyl ether acetate.

7. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 2, the first organic solvent is ethanol, and the first thermoplastic resin is one or more of cellulose acetate butyrate and ethyl cellulose.

8. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 3, the contents of the components in the conductive copper paste are, by mass percentage, 85-90% antioxidant copper powder, 3-5% thermosetting resin, 0.1-0.5% second thermoplastic resin, 1-3% auxiliary conductive agent, 0.1-0.5% curing agent, 0.1-0.5% coupling agent, and 4-8% second organic solvent.

9. The method for preparing the anti-oxidation conductive copper paste according to claim 1, characterized in that: In step 3, the auxiliary conductive agent is one or more of silver iodide powder or silver powder.

10. An anti-oxidation conductive copper paste, characterized in that: The conductive copper paste is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Conductive slurry and preparation method of antioxidant copper powder in conductive slurry

    CN120032941A

  • Low-temperature curing copper-based conductive paste as well as preparation method and application thereof

    CN120280204A