Method for reducing defect sources of deep trench structure
By forming a stacked structure on a semiconductor silicon substrate and using dry etching to remove sharp corners, the problem of cracking of oxide sharp corners at the top of deep trenches is solved, particles and silicon wafer scratch sources are reduced, and process quality is improved.
Patent Information
- Application Number
- CN202410852777.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
AI Technical Summary
In the semiconductor field, the sharp corners of SiO2 oxide remaining at the top of deep trenches are prone to brittle cracking during subsequent processes, becoming sources of particle defects or silicon wafer scratches, affecting process quality.
By forming a stacked structure on a silicon substrate, including a pad oxide layer, a nitride layer and a silicon oxide hard mask layer, the thermal oxidation method is used to form the thermal oxide layer, and the sharp corner structure is removed through dry etching to form a flat deep trench bottom to reduce oxide residue.
It effectively avoids the sharp-angular thermal oxide layer from cracking in the subsequent process, reduces the sources of particle defects and silicon wafer scratches, and improves the stability and quality of the process.
Smart Images

Figure CN118748145A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for reducing defect sources of a deep trench structure. Background Art
[0002] In the semiconductor field, great emphasis is placed on defect control in the process, such as particles. Reducing / eliminating the source of potential particles helps improve yield. In the BCD deep trench process, the sharp corners of oxide SiO2 remaining on the top of the deep trench are particularly prone to brittle fracture and breakage in subsequent processes (such as chemical grinding), becoming a source of particle defects or silicon wafer scratches.
[0003] In order to solve the above problems, it is necessary to propose a new method to reduce the defect sources of deep trench structures. Summary of the invention
[0004] In view of the shortcomings of the prior art described above, an object of the present invention is to provide a method for reducing the defect sources of deep trench structures, so as to solve the problem that the sharp corners of oxide SiO2 remaining on the top of the deep trench in the prior art are particularly prone to brittle fracture and breakage in subsequent processes (such as chemical grinding), becoming a source of particle defects or a source of silicon wafer scratches.
[0005] To achieve the above objectives and other related objectives, the present invention provides a method for reducing defect sources in a deep trench structure, comprising:
[0006] Step 1: providing a silicon substrate, forming a stacked structure on the substrate, wherein the stacked structure is composed of a pad oxide layer, a nitride layer, a first polysilicon layer, and a silicon oxide hard mask layer stacked in sequence from bottom to top; forming a deep trench on the stacked structure and the silicon substrate thereunder, and forming a thermal oxide layer on the surface of the deep trench and the exposed surface of the first polysilicon layer by a thermal oxidation method;
[0007] Step 2: The thermal oxide layer and the silicon oxide hard mask layer are processed by a first dry etching process using C5F8, Ar and O2 as etching gases, and the thermal oxide layer at the bottom of the deep trench and above the first polysilicon layer is removed. The surface of the first polysilicon layer will remain due to insufficient oxide etching at the trench opening, forming a sharp angle structure with a preset height at the side wall, wherein:
[0008] The first dry engraving comprises:
[0009] Main etching step: the etching selectivity ratio of oxide to silicon is 15-17:1;
[0010] Etching step of the endpoint monitoring method: the etching selectivity of oxide to silicon is 19-21:1;
[0011] Step 3: using a second dry etching process using C5F8, Ar and O2 as etching gases to remove the pointed structure and the thermal oxide layer at the bottom of the deep trench, wherein the etching selectivity ratio of the thermal oxide layer to silicon in the second dry etching process is 24-26:1;
[0012] Step 4: forming a second gate polysilicon layer filling the deep trench, grinding the second gate polysilicon layer onto the nitride layer, and then removing the pad oxide layer and the nitride layer.
[0013] Preferably, a silicon epitaxial layer is also formed on the silicon substrate in step one.
[0014] Preferably, in the etching step of the endpoint monitoring method in step 2, the power of the radio frequency source is 1150-1250W.
[0015] Preferably, in step 2, the height of the pointed thermal oxide layer is reduced to 90-110 nm.
[0016] Preferably, in step three, the etching selectivity is adjusted to 24-26:1 by reducing the ratio of C5F8 to O2.
[0017] Preferably, in the second dry etching in step three, the power of the RF source is 1150-1250W.
[0018] Preferably, the grinding method in step 4 is chemical mechanical planarization grinding.
[0019] Preferably, in step four, the pad oxide layer and the nitride layer are removed by wet etching.
[0020] As described above, the method of reducing the defect sources of deep trench structures of the present invention has the following beneficial effects:
[0021] The present invention can prevent the sharp-angled thermal oxide layer from breaking and breaking off in subsequent processes (such as chemical grinding), thereby reducing particle defect sources and silicon wafer scratch sources. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Shown is a schematic diagram of the process flow of the present invention;
[0023] Figure 2 Shown is a schematic diagram of a stacked structure formed according to the present invention;
[0024] Figure 3 It is a schematic diagram of forming a deep trench according to the present invention;
[0025] Figure 4 Shown is a schematic diagram of a sharp angle structure formed according to the present invention;
[0026] Figure 5 Shown is a schematic diagram of a structure for removing sharp corners according to the present invention;
[0027] Figure 6 It is a schematic diagram of forming a second gate polysilicon layer according to the present invention. DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0029] See also Figure 1 The present invention provides a method for reducing defect sources of deep trench structures, comprising:
[0030] Step 1: Provide a silicon substrate 101, and form a stacked structure on the silicon substrate 101. The stacked structure is composed of a pad oxide layer 103, a nitride layer 104, a first polysilicon layer 105, and a silicon oxide hard mask layer 106 stacked in sequence from bottom to top, forming a Figure 2 The structure shown in FIG. 1 is a structure in which a deep trench is formed on the stacked structure and the silicon substrate 101 thereunder, and a thermal oxide layer 107 is formed on the surface of the deep trench and the exposed surface (side wall) of the first polysilicon layer 105 by a thermal oxidation method. The silicon oxide hard mask layer 106 can be formed by a method such as chemical vapor deposition. During the thermal oxidation process, the thickness of the silicon oxide hard mask layer 106 does not increase much, and the exposed silicon will be oxidized into the thermal oxide layer 107.
[0031] In some embodiments, a silicon epitaxial layer 102 is also formed on the silicon substrate 101 in step one.
[0032] Step 2: The thermal oxide layer 107 and the silicon oxide hard mask layer 106 are treated by a first dry etching process using C5F8, Ar and O2 as etching gases. The thermal oxide layer 107 at the bottom of the deep trench and above the first polysilicon layer 105 is removed. The surface of the first polysilicon layer 105 will remain due to insufficient etching of the oxide at the trench opening, forming a sharp corner structure 108 with a preset height at the sidewall, forming Figure 4 The structure shown, in which
[0033] The first dry engraving includes:
[0034] Main etching (by time) step: the etching selectivity of oxide to silicon is 15-17:1;
[0035] Etching step by endpoint monitoring (by epd): The oxide etch selectivity to silicon is 19-21:1;
[0036] In some embodiments, in the etching step of the endpoint monitoring method in step 2, the power of the RF source is 1150-1250W, for example, 1150W, 1200W, 1250W.
[0037] In some embodiments, in step 2, the height of the pointed thermal oxide layer 107 is reduced to 90-110 nm.
[0038] Step 3: Use a second dry etching process using C5F8, Ar and O2 as etching gases to remove the sharp corner structure 108, forming Figure 5 The structure shown, wherein the etching selectivity ratio of the thermal oxide layer 107 to silicon in the second dry etching is 24-26:1;
[0039] In some embodiments, in step three, the etching selectivity is adjusted to 24-26:1 by reducing the ratio of C5F8 to O2.
[0040] In some embodiments, in step three, during the second dry etching, the power of the RF source is 1150-1250W.
[0041] Step 4: forming a second gate polysilicon layer 109 filling the deep trench, grinding the second gate polysilicon layer 109 onto the nitride layer 104, and then removing the pad oxide layer 103 and the nitride layer 104 to form a Figure 6 The structure shown.
[0042] In some embodiments, the polishing method in step 4 is chemical mechanical planarization polishing.
[0043] In some embodiments, in step 4, the pad oxide layer 103 and the nitride layer 104 are removed by wet etching.
[0044] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0045] In summary, the present invention can prevent the sharp-angled thermal oxide layer from breaking apart in the subsequent process (such as chemical grinding), thereby reducing the sources of particle defects and scratches. Therefore, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.
[0046] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for reducing defect sources in deep trench structures, characterized in that: At least: Step 1, providing a silicon substrate, forming a stacked structure on the silicon substrate, wherein the stacked structure consists of a pad oxide layer, a nitride layer, a first polysilicon layer and a silicon oxide hard mask layer stacked in sequence from bottom to top; forming a deep trench on the stacked structure and the silicon substrate thereunder, and forming a thermal oxide layer on the surface of the deep trench and the exposed surface of the first polysilicon layer by a thermal oxidation method; Step 2: The thermal oxide layer and the silicon oxide hard mask layer are processed by a first dry etching process using C5F8, Ar and O2 as etching gases, and the thermal oxide layer at the bottom of the deep trench and above the first polysilicon layer is removed. The surface of the first polysilicon layer will remain due to insufficient oxide etching at the trench opening, forming a sharp angle structure with a preset height at the side wall, wherein: The first dry engraving comprises: Main etching step: the etching selectivity ratio of oxide to silicon is 15-17:1; Etching step of the endpoint monitoring method: the etching selectivity of oxide to silicon is 19-21:1; Step 3: removing the sharp corner structure by a second dry etching process using C5F8, Ar and O2 as etching gases, wherein the etching selectivity ratio of the thermal oxide layer to silicon in the second dry etching process is 24-26:1; Step 4: forming a second gate polysilicon layer filling the deep trench, grinding the second gate polysilicon layer onto the nitride layer, and then removing the pad oxide layer and the nitride layer.
2. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: A silicon epitaxial layer is also formed on the silicon substrate in step one.
3. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: In step 2, in the etching step of the endpoint monitoring method, the power of the radio frequency source is 1150-1250W.
4. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: In step 2, the height of the pointed thermal oxide layer is reduced to 90-110 nm.
5. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: In step 3, the etching selectivity is adjusted to 24-26:1 by reducing the ratio of C5F8 to O2.
6. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: In the second dry etching in step three, the power of the RF source is 1150-1250W.
7. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: The grinding method in step 4 is chemical mechanical planarization grinding.
8. The method for reducing defect sources in deep trench structures according to claim 1, characterized in that: In step 4, the pad oxide layer and the nitride layer are removed by wet etching.
Citation Information
Cited By
Method for adjusting thickness of oxide on side wall of deep groove
CN119943748A
Method for adjusting thickness of sidewall oxide of deep trench
WO2026148845A1