Semiconductor device and method of manufacturing the same

By forming a crystalline high-k dielectric layer at a lower temperature and using dopant diffusion technology, the problem of defects in the interface layer and high-k dielectric layer in the high-temperature process of semiconductor devices is solved, achieving more efficient manufacturing. and lower costs.

CN118748172APending Publication Date: 2024-10-08TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410645463.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-23
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

During the miniaturization process of semiconductor devices, the high-temperature crystallization process causes defects in the interface layer and high-k dielectric layer, affecting the dopant profile distribution and stress in the channels and source/drain regions, increasing manufacturing difficulty and cost.

Method used

By forming a crystalline high-k dielectric layer at a lower temperature, utilizing the first metal element dopant in the first high-k dielectric layer and the second metal element diffusion in the second high-k dielectric layer , lower the crystallization temperature, and adjust the dopant distribution of the dielectric layer during the annealing process, reducing interface defects and dopant profile distribution changes.

Benefits of technology

It achieves the manufacturing of high-k dielectric layers at lower temperatures, reduces the thermal budget of the manufacturing process, reduces defects in the interface layer and high-k dielectric layer, and maintains the connection between the channel and the source/drain region. stress, improving the performance and reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748172A_ABST
    Figure CN118748172A_ABST
Patent Text Reader

Abstract

The present disclosure provides for forming a crystalline high-k dielectric layer within a semiconductor device at a reduced crystallization temperature. The method includes forming a channel structure on a substrate; forming an interface layer on the channel structure; forming a first high-k dielectric layer on the interface layer; forming a dipole (dipole) in the first high k value dielectric layer with a dopant; and forming a second high-k dielectric layer on the first high-k dielectric layer. The dopant includes a first metal element. The second high-k dielectric layer includes a second metal element different from the first metal element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to a semiconductor technology, and more particularly to a semiconductor device and a method for manufacturing the same. Background Art

[0002] As semiconductor technology advances, the demand for higher storage capacity, faster processing systems, higher performance and lower costs continues to increase. To meet these demands, the semiconductor industry continues to shrink the size of semiconductor devices, such as metal oxide semiconductor field effect transistors (MOSFETs), including planar semiconductor field effect transistors (MOSFETs) and fin field effect transistors (finFETs). This miniaturization increases the complexity of semiconductor manufacturing processes and also increases the difficulty of semiconductor device process control. Summary of the invention

[0003] In some embodiments, a method for manufacturing a semiconductor device is provided, comprising: forming a channel structure on a substrate; forming an interface layer on the channel structure; forming a first high-k dielectric layer on the interface layer; forming a dipole in the first high-k dielectric layer using a dopant, wherein the dopant includes a first metal element; and forming a second high-k dielectric layer on the first high-k dielectric layer, wherein the second high-k dielectric layer includes a second metal element different from the first metal element.

[0004] In some embodiments, a method for manufacturing a semiconductor device is provided, comprising: forming first and second channel structures on a substrate; forming an interface layer on the first and second channel structures; forming a first dielectric layer on the interface layer on the first and second channel structures; forming a dipole with a first dopant in the first dielectric layer on the first channel structure, wherein the first dopant includes a first metal element; forming a dipole with a second dopant in the first dielectric layer on the second channel structure, wherein the second dopant includes a second metal element different from the first metal element; and forming a second dielectric layer on the first dielectric layer, wherein the second dielectric layer includes a third metal element different from the first and second metal elements.

[0005] In some embodiments, a semiconductor device is provided, comprising: a channel structure located on a substrate; an interface layer located on the channel structure; a first high-k value dielectric layer located on the interface layer on the channel structure, wherein the first high-k value dielectric layer is doped with a first dopant including a first metal element and a second dopant including a second metal element different from the first metal element; and a second high-k value dielectric layer located on the first high-k value dielectric layer, wherein the second high-k value dielectric layer includes a second metal element. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Figure 1 Depicted is an isometric view of a semiconductor device having a crystalline high-k dielectric layer fabricated at a reduced crystallization temperature, according to some embodiments.

[0007] Figure 2 A schematic cross-sectional view of a semiconductor device having a crystalline high-k dielectric layer fabricated at a reduced crystallization temperature according to some embodiments is shown.

[0008] Figure 3 A flow chart is depicted of a method for fabricating a crystalline high-k gate dielectric layer in a semiconductor device at a reduced crystallization temperature, according to some embodiments.

[0009] Figure 4-Figure 12 Schematic cross-sectional views of a semiconductor device having a crystalline high-k gate dielectric layer fabricated at a reduced crystallization temperature at various stages of fabrication are shown in accordance with some embodiments.

[0010] The reference numerals are described as follows:

[0011] 100: Semiconductor devices

[0012] 102A, 102B, 102C: Transistor; n-type field effect transistor; p-type field effect transistor; nanostructure transistor; gate all-around field effect transistor (GAA FET)

[0013] 104: Base

[0014] 106: Shallow Trench Isolation (STI) Region

[0015] 108: Fin structure 108

[0016] 109: Sidewall spacer

[0017] 110: Source / Drain (S / D) Structure

[0018] 112: Gate structure

[0019] 114: Gate spacer

[0020] 116: Etch stop layer (ESL)

[0021] 118: Interlayer dielectric (ILD) layer

[0022] 124: Gate dielectric layer

[0023] 211: Interface layer

[0024] 211t, 213t, 215t: thickness

[0025] 213: First high-k dielectric layer

[0026] 213-1: Part One

[0027] 213-2: Part 2

[0028] 215: Second highest k value dielectric layer

[0029] 222, 222-1, 222-2, 222-3: Nanostructures

[0030] 300: Methods

[0031] 310, 320, 330, 340, 350: Step blocks

[0032] 717: Dipole source layer DETAILED DESCRIPTION

[0033] The following disclosure provides many different embodiments or examples to implement different characteristic components of the present invention. The following disclosure describes specific examples of each component and its arrangement in order to simplify the present disclosure. Of course, these are only examples and are not used to define the present invention. For example, if the following disclosure describes that a first characteristic component is formed on or above a second characteristic component, it means that it includes an embodiment in which the first characteristic component and the second characteristic component are in direct contact, and also includes an embodiment in which an additional characteristic component can be formed between the first characteristic component and the second characteristic component, so that the first characteristic component and the second characteristic component may not be in direct contact. In addition, the present disclosure will repeat numbers and / or text in each different example. Repetition is for the purpose of simplification and clarification, rather than listing and specifying the relationship between the various different embodiments and / or configurations discussed.

[0034] Spatially related terms such as "below", "beneath", "below", "above", "above", etc. are used here to easily express the relationship between an element or feature in the drawings shown in this specification and another element or feature. These spatially related terms not only cover the orientation shown in the drawings, but also cover different orientations of the device during use or operation. The device can have different orientations (rotated 90 degrees or other orientations) and the spatially related symbols used here are also interpreted accordingly.

[0035] It should be noted that the terms "one embodiment", "an embodiment", "an exemplary embodiment", "exemplary", etc. mentioned in the specification indicate that the embodiment described may include specific characteristic components, structures or characteristics, but each embodiment does not necessarily include specific characteristic components, structures or characteristics. Furthermore, the above terms do not necessarily refer to the same embodiment. In addition, when the description of a specific characteristic component, structure or characteristic is related to an embodiment, within the scope of knowledge of a person with ordinary knowledge in the technical field, the above-mentioned characteristic component, structure or characteristic can be implemented in connection with other embodiments, whether or not explicitly described.

[0036] It should be understood that the terms and terminology herein are for the purpose of description rather than limitation, and thus the terms and terminology of this specification should be interpreted by a person having ordinary knowledge in the technical field according to the teachings herein.

[0037] In some embodiments, the terms "approximately" and "substantially" may represent a numerical value of a given number that varies within 20% of the numerical value (e.g., ±1%, ±2%, ±3%, ±4%, ±5%, ±10%, ±20% of the numerical value). These numerical values ​​are merely examples and are not meant to be limiting. The terms "approximately" and "substantially" may refer to a percentage of a numerical value as interpreted by a person of ordinary skill in the art based on the teachings herein.

[0038] As the demand for lower power consumption, higher performance and smaller semiconductor devices continues to increase, the size of semiconductor devices continues to shrink. The continued shrinking of device size and the increase in the demand for device performance may require various process and material improvements, which may have various challenges. For example, the gate dielectric layer of a nanostructured transistor may include an interface layer and a high-k value dielectric layer. The high-k value dielectric layer may include a high-k value dielectric material to reduce the size of the gate dielectric layer and increase gate control. The term "high-k value" may refer to a high dielectric constant. In the field of semiconductor device structure and manufacturing process, a high-k value may refer to a dielectric constant greater than that of silicon oxide (e.g., greater than about 3.9). High-k value dielectric materials can be crystallized into a cubic phase or other crystalline phase at high temperatures (e.g., about 800°C to 1000°C) to increase the dielectric constant (i.e., k value) and reduce leakage current. However, the high temperature of the crystallization process will produce defects at the interface between the interfacial layer and the high-k dielectric layer, changing the dopant profile of the channel and source / drain (S / D) regions of the nanostructure transistor and reducing the stress between the channel and source / drain (S / D) regions. The source / drain (S / D) region can refer to the source region or the drain region, either alone or both depending on the context.

[0039] Various embodiments of the present disclosure provide example methods for forming a crystalline high-k dielectric layer at a reduced crystallization temperature in a semiconductor device (e.g., a nanostructure transistor) and / or other semiconductor devices in an integrated circuit (IC). In some embodiments, a channel structure may be formed on a substrate and an interface layer may be formed on the channel structure. A first high-k dielectric layer may be formed on the interface layer and doped with a first dopant. The first dopant may include a first metal element to form a dipole within the first high-k dielectric layer and / or at an interface between the interface layer and the first high-k dielectric layer. A second high-k dielectric layer may be formed on the first high-k dielectric layer, and the second high-k dielectric layer may include a second metal element different from the first metal element. In a subsequent annealing process, the second metal element may diffuse into the first high-k dielectric layer as a second dopant and may reduce the crystallization temperature of the first high-k dielectric layer. In some embodiments, the crystallization temperature may be reduced to about 500° C. to 700° C. Therefore, the first high-k dielectric layer may be crystallized at a lower temperature and the thermal budget of the manufacturing process may be reduced. In addition, defects at the interface between the interfacial layer and the first high-k dielectric layer can be reduced, changes in the dopant profile distribution in the channel and source / drain (S / D) regions of the semiconductor device can be minimized, and stress between the channel and source / drain (S / D) regions can be maintained.

[0040] Figure 1 Depicted is an isometric view of a semiconductor device 100 having a crystalline high-k dielectric layer fabricated at a reduced crystallization temperature, according to some embodiments. Figure 2Depicts a span according to some embodiments Figure 1 FIG. 1 is a partial cross-sectional view of the semiconductor device 100 along line AA shown in FIG. In some embodiments, the semiconductor device 100 may include transistors 102A-102C, such as Figure 1 As shown. In some embodiments, transistors 102A-102C may include nanostructured transistors. Nanostructured transistors may include fin field effect transistors (finFETs), gate-all-around field effect transistors (GAA FETs), nanosheet transistors, nanowire transistors, multi-bridge channel transistors, nano-ribbon transistors, and other transistors of similar structures. Nanostructured transistors may provide one channel in a stacked nanosheet / nanowire configuration.

[0041] In some embodiments, transistors 102A-102C may be n-type field effect transistors (NFETs). In some embodiments, transistors 102A-102C may be p-type nanostructure field effect transistors (PFETs). In some embodiments, any one of transistors 102A-102C may be an NFET or a PFET. Figure 1 Three transistors are shown, but semiconductor device 100 may have any number of transistors. In addition, semiconductor device 100 may be integrated into an integrated circuit using other structural components (e.g., conductive vias, conductive lines, dielectric layers, passivation layers, and interconnects), which are not shown for simplicity. Unless otherwise noted, descriptions of components with the same reference numerals as transistors 102A-102C apply to each other. Similar reference numerals generally indicate components that are identical, functionally similar, and / or structurally similar.

[0042] Please refer to Figure 1 and Figure 2 , a semiconductor device 100 having transistors 102A-102C may be formed on a substrate 104 and may be isolated by a shallow trench isolation (STI) region 106. Each of the transistors 102A-102C may include a fin structure 108, a sidewall spacer 109, a gate dielectric layer 124, a gate structure 112, a gate spacer 114, a source / drain (S / D) structure 110, an etch stop layer (ESL) 116, and an interlayer dielectric (ILD) layer 118. In some embodiments, as Figure 2As shown, nanostructure transistors 102A- 102C may have nanostructures 222 - 1 , 222 - 2 , and 222 - 3 (collectively referred to as “nanostructures 222 ”) on fin structure 108 .

[0043] Reference Figure 1 , the substrate 104 may include a semiconductor material, such as silicon. In some embodiments, the substrate 104 includes a crystalline silicon substrate (e.g., a wafer). In some embodiments, the substrate 104 includes (i) an elemental semiconductor, such as germanium; (ii) a compound semiconductor, including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; (iii) an alloy semiconductor, including silicon germanium carbide, silicon germanium, gallium arsenic phosphide, and / or aluminum arsenide; or (iv) a combination thereof. Furthermore, according to design requirements (e.g., a p-type substrate or an n-type substrate), the substrate 104 may be doped. In some embodiments, the substrate 104 may be doped with a p-type dopant (e.g., boron, indium, aluminum, or gallium) or an n-type dopant (e.g., phosphorus or arsenic).

[0044] The shallow trench isolation (STI) region 106 can provide electrical isolation between the transistors 102A-102C on the substrate 104, as well as electrical isolation between adjacent transistors (not shown) and / or electrical isolation between adjacent active and passive components (not shown) integrated or deposited on the substrate 104. The shallow trench isolation (STI) region 106 can be made of a dielectric material. In some embodiments, the shallow trench isolation (STI) region 106 can include silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass (FSG), low-k dielectric material and / or other suitable insulating materials. In some embodiments, the shallow trench isolation (STI) region 106 can include a multi-layer structure.

[0045] Please refer to Figure 1 and Figure 2 , the nanostructure 222 and the fin structure 108 can be formed on the patterned portion of the substrate 104. The embodiments of the nanostructures and fin structures described herein can be patterned by any suitable method. For example, the nanostructures and fin structures can be patterned using one or more lithography processes, including double patterning or multiple patterning processes. Double patterning or multiple patterning processes can combine lithography and self-alignment processes to form, for example, patterns with smaller pitch than can be obtained using a single direct lithography process. For example, a sacrificial layer is formed on the substrate and patterned using a lithography process. Spacers can be formed next to the patterned sacrificial layer using a self-alignment process. The sacrificial layer is then removed, and the remaining spacers can be used to pattern the nanostructures and fin structures.

[0046] like Figure 1 and Figure 2As shown, the nanostructure 222 and the fin structure 108 may extend along the X-axis and pass through the transistors 102A-102C. In some embodiments, the nanostructure 222 and the fin structure 108 may be disposed on the substrate 104. The nanostructure 222 may include a group of nanostructures 222-1, 222-2 and 222-3, which may be in the form of nanosheets, nanowires or nanobelts. Each nanostructure 222 may serve as a channel structure and form a channel region below the gate structure 112 of the transistors 102A-102C. In some embodiments, the nanostructure 222 and the fin structure 108 may include a semiconductor material similar to or different from the substrate 104. In some embodiments, the nanostructure 222 and the fin structure 108 may include silicon. In some embodiments, the nanostructure 222 and the fin structure 108 may include silicon germanium. The semiconductor material of the nanostructure 222 and the fin structure 108 may be undoped or may be in-situ doped during its formation process. In some embodiments, as Figure 2 As shown, the nanostructure 222 below the gate structure 112 can form a channel region of the semiconductor device 100 and serve as a current-carrying channel structure of the semiconductor device 100. Figure 2 Three layers of nanostructures 222 are shown, but transistors 102A- 102C may have any number of nanostructures 222 .

[0047] In some embodiments, the nanostructure 222 may have a thickness along the Z axis in a range of about 5 nm to 8 nm. In some embodiments, the nanostructure 222 may have a width along the Y axis in a range of about 15 nm to 50 nm. In some embodiments, the spacing between adjacent nanostructures 222 along the Z axis is in a range of about 8 nm to 12 nm.

[0048] Please refer to Figure 2 The gate dielectric layer 124 may be a multi-layer structure and may be formed on the nanostructure 222, the fin structure 108, and the shallow trench isolation (STI) region 106. Figure 2 As shown, the gate dielectric layer 124 may include an interface layer 211, a first high-k dielectric layer 213, and a second high-k dielectric layer 215. In some embodiments, the gate dielectric layer 124 may include a first high-k dielectric layer 213 in direct contact with the nanostructure 222. In some embodiments, the interface layer 211 may include silicon oxide formed by a deposition process or an oxidation process. In some embodiments, the interface layer 211 may have a thickness 211t in a range of about 0.1 nm to 1.5 nm.

[0049] In some embodiments, the first high-k dielectric layer 213 may include hafnium oxide, zirconium oxide or other suitable high-k dielectric materials. In some embodiments, the first high-k dielectric layer 213 may be crystalline and may include a crystalline high-k dielectric material. Crystalline high-k dielectric materials may have a higher dielectric constant than amorphous high-k dielectric materials. In some embodiments, crystalline high-k dielectric materials may have a cubic crystalline phase or other crystalline phases. In some embodiments, the first high-k dielectric layer 213 doped with a second dopant may have a higher dielectric constant. In some embodiments, the first high-k dielectric layer 213 may have a thickness 213t, approximately in the range of 1nm to 5nm. If the thickness 213t is greater than about 5nm, the gate capacitance will be reduced and the device performance will also be reduced. If the thickness 213t is less than about 1nm, the first high-k dielectric layer 213 may be uneven and the leakage current may be increased.

[0050] In some embodiments, the first high-k dielectric layer 213 may be doped with a first dopant to form a dipole within the first high-k dielectric layer 213 and / or at an interface between the interface layer 211 and the first high-k dielectric layer 213. In some embodiments, the dipole may be formed by diffusing the first dopant from a dipole source layer formed on the first high-k dielectric layer 213. In some embodiments, the first dopant may include a first metal element having a high chemical affinity for silicon or germanium and may form a dopant dipole at an interface with silicon or germanium under thermal conditions (e.g., thermal annealing). The amount of the first dopant diffused to the interface and the amount of the dipole formed around the interface may adjust the threshold voltage (V t ). In some embodiments, the dopant dipole may be formed before the second high-k dielectric layer 215 is formed. In some embodiments, the dopant dipole may be formed after the second high-k dielectric layer 215 is formed.

[0051] In some embodiments, depending on the nature of the first dopant used, the dipole formed at the interface can attract electrons (or holes) in the channel below the gate dielectric layer 124, thereby reducing the V of the NFET (or PFET). t The dipole at the interface can also repel holes (or electrons) in the channel, thereby increasing the V of the PFET (or NFET). t The dipole between the interface layer 211 and the first high-k dielectric layer 213 may induce more V than the dipole within the first high-k dielectric layer 213. tThe offset is due to the smaller distance between the interface and the channel and also due to the fact that the dipole charge shielding of the low-k interface layer material of the interface layer 211 is less than the high-k material of the first high-k dielectric layer 213. In some embodiments, the dipole source layer for NFET Vt adjustment may include a metal element different from the metal element in the dipole source layer for PFET Vt adjustment. In some embodiments, the dipole source layer for NFET Vt adjustment may include lanthanum oxide (La2O3), lutetium oxide (Lu2O3), yttrium oxide (Y2O3), thulium oxide (Tm2O3), scandium oxide (Sc2O3), gadolinium oxide (Gd2O3), or other suitable rare earth metal oxides, alkaline earth metal oxides, and transition metal oxides. In some embodiments, the dipole source layer for PFET Vt adjustment may include zinc oxide (ZnO), germanium oxide (GeOx), aluminum oxide (AlOx), titanium oxide (TiOx), vanadium oxide (VOx), or other suitable rare earth metal oxides, alkaline earth metal oxides, and transition metal oxides. In some embodiments, after doping the first high-k dielectric layer 213 with the first dopant, the dipole source layer may be removed.

[0052] In some embodiments, the second high-k dielectric layer 215 may be disposed on the first high-k dielectric layer 213 and may include a high-k dielectric material different from the first high-k dielectric layer 213. In some embodiments, the second high-k dielectric layer 215 may be deposited on NFET and PFET devices. In some embodiments, the high-k dielectric material in the second high-k dielectric layer 215 may include Lu2O3, Y2O3, Tm2O3, erbium oxide (Er2O3), Gd2O3, or other suitable transition metal oxides. In some embodiments, the high-k dielectric material in the second high-k dielectric layer 215 may include a second metal element different from the first metal element. The second metal element may diffuse into the first high-k dielectric layer 213 in a subsequent annealing process to form a second dopant in the first high-k dielectric layer 213. In some embodiments, a metal element in the dielectric material may have a dopant solubility limit. In order to avoid reaching the dopant solubility limit of a metal element, the first and second metal elements may be different. In some embodiments, the peak of the second dopant profile distribution in the first high-k dielectric layer 213 may be located at the bottom, middle, or top of the first high-k dielectric layer 213. In some embodiments, the second metal element may include lutetium, yttrium, thulium, erbium, or gadolinium. In some embodiments, the second metal element may include lutetium or yttrium. In some embodiments, the second metal element may include lutetium or yttrium, and does not include thulium, erbium, or gadolinium.

[0053] In some embodiments, the concentration of the second metal element in the first high-k dielectric layer 213 may be in a range of about 5% to 25%. Through the second high-k dielectric layer 215 on the first high-k dielectric layer 213 and the second metal element in the first high-k dielectric layer 213, the crystallization temperature of the first high-k dielectric layer 213 may be reduced to a range of about 500° C. to 700° C. If the concentration of the second metal element in the first high-k dielectric layer 213 is less than about 5%, the crystallization temperature of the first high-k dielectric layer 213 may not be reduced. If the concentration of the second metal element in the first high-k dielectric layer 213 is greater than about 25%, defects in the first high-k dielectric layer 213 may increase due to the dopant concentration being higher than the dopant solubility limit. As the crystallization temperature of the first high-k dielectric layer 213 decreases, defects on the interface between the interface layer 211 and the first high-k dielectric layer 213 can be reduced, the change in the dopant profile distribution in the nanostructure 222 and the source / drain (S / D) structure 110 can be minimized, and the stress between the nanostructure 222 and the source / drain (S / D) structure 110 can be maintained.

[0054] In some embodiments, the second high-k dielectric layer 215 may have a lower dielectric constant than the first high-k dielectric layer 213. In some embodiments, the second high-k dielectric layer 215 may have a thickness 215t of about to In some embodiments, the ratio of thickness 213t to thickness 215t may be in the range of about 2 to 50. If thickness 215t is greater than about If the thickness 215t is less than about 2, the dielectric constant of the gate dielectric layer 124 will be reduced. Or when the above ratio is greater than about 50, the concentration of the second metal element in the first high-k dielectric layer 213 is less than about 5%, and the crystallization temperature of the first high-k dielectric layer 213 is not reduced.

[0055] The source / drain (S / D) structure 110 may be disposed on the substrate 104 and on two opposite sides of the gate structure 112. The source / drain (S / D) structure 110 may serve as a source / drain (S / D) region of the transistors 102A-102C. In some embodiments, the source / drain (S / D) structure 110 may have any geometric shape, such as a polygon, an ellipse, and a circle. In some embodiments, the source / drain (S / D) structure 110 may include an epitaxially grown semiconductor material, such as silicon (e.g., the same material as the substrate 104). In some embodiments, the epitaxially grown semiconductor material may include an epitaxially grown semiconductor material different from the material of the substrate 104, such as silicon germanium, and a strain is applied to the channel region below the gate structure 112. Since the lattice constant of such epitaxially grown semiconductor material is different from the material of the substrate 104, the channel region is strained to increase the carrier mobility in the channel region of the semiconductor device 100. The epitaxially grown semiconductor material may include: (i) semiconductor materials, such as germanium and silicon; (ii) compound semiconductor materials, such as gallium arsenide and aluminum arsenide; or (iii) semiconductor alloys, such as silicon germanium and gallium arsenide phosphide.

[0056] In some embodiments, the source / drain (S / D) structure 110 may include silicon and may be in-situ doped with n-type dopants (e.g., phosphorus and arsenic) during the epitaxial growth process. In some embodiments, the source / drain (S / D) structure 110 may include silicon, silicon germanium, germanium, or III-V materials (e.g., indium antimonide, gallium antimonide, or indium antimonide), and may be in-situ doped with p-type dopants (e.g., boron, indium, and gallium) during the epitaxial growth process. In some embodiments, the source / drain (S / D) structure 110 may include one or more epitaxial layers, wherein each epitaxial layer may have a different composition.

[0057] In some embodiments, Figure 1 and Figure 2 As shown, the gate structure 112 may be disposed on the gate dielectric layer 124. In some embodiments, the gate structure 112 may include one or more work function metal layers and a metal filler. The one or more work function metal layers may include a work function metal to adjust the threshold voltage (V t In some embodiments, the gate structures 112 for the NFET and PFET devices may have the same work function metal. In some embodiments, the gate structures 112 for the NFET and PFET devices may have different work function metals. In some embodiments, the work function metals for the NFET and PFET devices may be adjusted based on the second dopant in the first high-k dielectric layer 213. In some embodiments, as Figure 2As shown, each of the nanostructures 222 may be surrounded by a gate structure 112. These gate structures 112 may be referred to as "gate all-around (GAA) structures", and the transistors 102A-102C may also be referred to as "gate all-around field effect transistors (GAAFETs) 102A-102C". The one or more work function metal layers may surround the nanostructures 222 and may include work function metal to adjust the V t In some embodiments, transistors 102A-102C may include any number of work function metal layers for V t Adjustment (e.g., ultra-low V t , Low V t And standard V t ).

[0058] In some embodiments, the n-type field effect transistors (NFETs) 102A-102C may include an n-type work function metal layer. The n-type work function metal layer may include aluminum, titanium aluminum, titanium aluminum carbon, tantalum aluminum, tantalum aluminum carbon, tantalum silicon carbide, hafnium carbide, silicon, titanium nitride, titanium silicon nitride, or other suitable work function metals. In some embodiments, the p-type field effect transistors (PFETs) 102A-102C may include a p-type work function metal layer. The p-type work function metal layer may include titanium nitride, titanium silicon nitride, tantalum nitride, tungsten carbon nitride, tungsten, molybdenum, or other suitable work function metals. In some embodiments, the work function metal layer may include a single metal layer or a metal layer stack. The metal layer stack may include work function metals having work function values ​​that are equal to or different from each other. In some embodiments, the metal filler may include titanium, tantalum, aluminum, cobalt, tungsten, nickel, ruthenium, or other suitable conductive materials.

[0059] Please refer to Figure 1 , the gate spacer 114 can be disposed on the sidewall of the gate structure 112, and the sidewall spacer 109 can be disposed on the sidewall of the fin structure 108. The gate spacer 114 and the sidewall spacer 109 may include an insulating material, such as silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon oxycarbon, silicon oxycarbon nitride, low-k value materials, and combinations thereof. The gate spacer 114 and the sidewall spacer 109 may include a single layer or a stack of insulating layers. The gate spacer 114 and the sidewall spacer 109 may have a low-k value material having a dielectric constant less than about 3.9 (e.g., about 3.5, about 3.0, or about 2.8).

[0060] An etch stop layer (ESL) 116 may be disposed on the shallow trench isolation (STI) region 106, the source / drain (S / D) structure 110, and the sidewalls of the gate spacer 114 and the sidewall spacer 109. The etch stop layer (ESL) 116 may be used to protect the shallow trench isolation (STI) region 106, the source / drain (S / D) structure 110, and the gate structure 112 during the formation of a source / drain (S / D) contact structure on the source / drain (S / D) structure 110. In some embodiments, the etch stop layer (ESL) 116 may include silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbide nitride, boron nitride, silicon boron nitride, silicon carbide nitride, or a combination thereof.

[0061] An interlayer dielectric (ILD) layer 118 may be disposed on an etch stop layer (ESL) 116 over the source / drain (S / D) structure 110 and the shallow trench isolation (STI) region 106. The interlayer dielectric (ILD) layer 118 may include a dielectric material that is deposited using a deposition method suitable for a flowable dielectric material. For example, flowable silicon oxide may be deposited using flowable chemical vapor deposition (FCVD). In some embodiments, the dielectric material may include silicon oxide.

[0062] Figure 3 A flow chart is depicted of a method 300 for fabricating a crystalline high-k gate dielectric layer in a semiconductor device 100 at a reduced crystallization temperature in accordance with some embodiments. The method 300 may not be limited to nanostructured transistor devices, but may also be applicable to other devices that would benefit from a crystalline high-k dielectric layer fabricated at a reduced crystallization temperature. Additional fabrication operations may be performed between various operational steps of the method 300, and may be omitted solely for clarity and ease of illustration. Additional processes may be provided before, during, and / or after the method 300; one or more of these additional fabrication operations are briefly described herein. Furthermore, not all operational steps need to be performed as provided by the present disclosure. Additionally, some operational steps may be performed simultaneously or in different steps than the method 300. Figure 3 In some embodiments, in addition to the currently described operation steps, one or more other operation steps may be performed, or may replace the currently described operation steps.

[0063] For illustrative purposes, reference will be made to Figure 4-Figure 12 The exemplary manufacturing process for manufacturing the semiconductor device 100 is described in detail. Figure 3 The steps shown. Figure 4-Figure 12 A partial cross-sectional view of a semiconductor device 100 having a crystalline high-k gate dielectric layer fabricated at a reduced crystallization temperature at different fabrication stages is shown in accordance with some embodiments. Figure 4-Figure 12 Same as Figure 1 and Figure 2 The parts with part numbers in the middle are described as above.

[0064] Please refer to Figure 3 The method 300 begins at operation 310 by forming a channel structure on a substrate. Figure 1 , Figure 2 and Figure 4 As shown, nanostructures 222 - 1 , 222 - 2 , and 222 - 3 may be formed on the substrate 104 and may serve as channel structures in the semiconductor device 100 . Figure 4 Depicted are diagrams according to some embodiments. Figure 1 Schematic diagram of a partial cross-section of the semiconductor device 100 along line AA shown. In some embodiments, the nanostructure 222 can be epitaxially grown on the substrate 104 and stacked with other nanostructures (not shown) in an alternating configuration. The nanostructure 222 and the additional nanostructures can be patterned by the double or multiple patterning process described above. The additional nanostructure may include a semiconductor material different from the nanostructure 222. For example, the nanostructure 222 may include silicon, and the additional nanostructure may include silicon germanium. The semiconductor material of the nanostructure 222 may be undoped or may be in-situ doped during its formation process. The additional nanostructure may be removed in a subsequent process to form vertically stacked and separated nanostructures 222, such as Figure 4 In some embodiments, the nanostructure 222 may be in the form of a nanosheet, a nanowire, or a nanobelt. In some embodiments, the nanostructure 222 and the fin structure 108 may include a semiconductor material similar to or different from the substrate 104 .

[0065] Please refer to Figure 3 In operation step 320, an interface layer is formed on the channel structure. For example, Figure 5 As shown, the interface layer 211 can be formed on the nanostructure 222. In some embodiments, the interface layer 211 may include silicon oxide formed by a deposition process or an oxidation process. If the interface layer 211 is formed by a deposition process, the interface layer 211 can be formed on the nanostructure 222, the fin structure 108, and the shallow trench isolation (STI) region 106. If the interface layer 211 is formed by an oxidation process, the interface layer 211 can be formed on the nanostructure 222 and the fin structure 108. In some embodiments, the thickness of the interface layer 211 can be approximately in the range of 0.1nm to 1.5nm. In some embodiments, the interface layer 211 can be optional and can be omitted.

[0066] Please refer to Figure 3In operation step 330, a first high-k gate dielectric layer is formed on the interface layer. Figure 6 As shown, the first high-k dielectric layer 213 can be formed on the interface layer 211. In some embodiments, the first high-k dielectric layer 213 can be deposited on the interface layer 211 of the nanostructure 222, the fin structure 108, and the shallow trench isolation (STI) region 106. In some embodiments, the first high-k dielectric layer 213 can be conformally deposited at a temperature of about 200° C. to 400° C. by atomic layer deposition (ALD), chemical vapor deposition (CVD), or other suitable deposition methods. In some embodiments, the first high-k dielectric layer 213 can be amorphous after deposition. In some embodiments, the first high-k dielectric layer 213 can include hafnium oxide, zirconium oxide, or other suitable high-k dielectric materials. In some embodiments, the thickness 213t of the first high-k dielectric layer 213 can be approximately in the range of 1 nm to 5 nm. If the thickness 213t is greater than about 5 nm, the gate capacitance may decrease and the device performance may decrease. If the thickness 213t is less than about 1 nm, the first high-k dielectric layer 213 may be non-uniform and leakage current may increase.

[0067] Please refer to Figure 3 In operation 340, the first high-k gate dielectric layer is doped with a dopant including a first metal element to form a dipole. For example, Figure 7 As shown, a dipole source layer 717 may be formed on the first high-k dielectric layer 213 to dope the first high-k dielectric layer 213. In some embodiments, the dipole source layer 717 may be deposited on the first high-k dielectric layer 213 by ALD, CVD or other suitable deposition methods to a thickness of about 1000 nm. to In some embodiments, for NFET devices, the dipole source layer 717 may include La2O3, Lu2O3, Y2O3, Tm2O3, Sc2O3, Gd2O3, or other suitable rare earth metal oxides, alkaline earth metal oxides, and transition metal oxides. In some embodiments, for PFET devices, the dipole source layer 717 may include ZnO, GeOx, AlOx, TiOx, VOx, or other suitable rare earth metal oxides, alkaline earth metal oxides, and transition metal oxides. In some embodiments, the dipole source layer 717 for NFET and PFET devices may include different dopants with different metal elements.

[0068] In some embodiments, after the deposition of the dipole source layer 717, a heat treatment may be performed to dope the first high-k dielectric layer 213 and the interface layer 211. For example, as shown in FIG. 7, the dipole source layer 717 may be treated by isothermal annealing, and the annealing temperature is about 500° C. to 800° C. The isothermal annealing may be performed in an inert gas (e.g., nitrogen and argon) environment, with a pressure in the range of about 10 mtorr to 5 torr, and a time in the range of about 3 seconds to 100 seconds. Following the heat treatment, the first metal element in the dipole source layer 717 may diffuse and form a dipole in the first high-k dielectric layer 213 and the interface layer 211.

[0069] Depending on the nature of the dopants used, the dipoles in the first high-k dielectric layer 213 and the interface layer 211 can attract electrons (or holes) in the channel under the gate dielectric layer 124, thereby reducing the V t (or reduce the V t The dipoles of the first high-k dielectric layer 213 and the interface layer 211 can also repel holes in the channel, thereby increasing the V t (or increase the V t In some embodiments, since the distance between the interface layer and the channel is small and since the low-k dielectric material of the interface layer 211 shields the dipole charge less than the high-k dielectric material of the first high-k dielectric layer 213, the dipole charge of the interface layer 211 can cause more V than the dipole charge in the high-k dielectric layer. t In some embodiments, the first metal element of the dopant for the NFET and PFET devices may be different, and the dipoles formed in the first high-k dielectric layer 213 and the interface layer 211 may be different.

[0070] In some embodiments, the dipole source layer 717 may be removed after doping the first high-k dielectric layer 213 and the interface layer 211. Figure 8 As shown, the dipole source layer 717 may be removed from the first high-k dielectric layer 213. After the doping process, a wet chemical etching process may remove the dipole source layer 717 at a temperature ranging from about 25° C. to 300° C. In some embodiments, the dipole source layer 717 may be first deposited on the NFET device to form an n-type dipole with one metal element, and then the dipole source layer 717 may be removed. Subsequently, the dipole source layer 717 may be deposited on the PFET device to form a p-type dipole with a different metal element, and then the dipole source layer 717 may be removed. During the process of forming the dipole in the PFET (or NFET) device, the NFET (or NFET) device may be covered with a mask layer.

[0071] Please refer to Figure 3In operation step 350, a second high-k dielectric layer is formed on the first high-k gate dielectric layer. The second high-k dielectric layer includes a second metal element different from the first metal element. For example, Fig. 9 As shown, a second high-k dielectric layer 215 may be formed on the first high-k dielectric layer 213. In some embodiments, the second high-k dielectric layer 215 may be deposited on NFET and PFET devices. In some embodiments, the second high-k dielectric layer 215 may include a high-k dielectric material different from the first high-k dielectric layer 213 and may have a lower dielectric constant than the first high-k dielectric layer 213. In some embodiments, the second high-k dielectric layer 215 may include a second metal element that is different from the first metal element doped in the first high-k dielectric layer 213. In some embodiments, the second high-k dielectric layer 215 may include Lu2O3, Y2O3, Tm2O3, Er2O3, Gd2O3, or other suitable transition metal oxides. In some embodiments, the second metal element in the second high-k dielectric layer 215 may diffuse into the first high-k dielectric layer 213 during the deposition process to form a second dopant. In some embodiments, the second metal element in the second high-k dielectric layer 215 may be different from the first metal element to avoid reaching the dopant solubility limit of one metal element.

[0072] In some embodiments, the second high-k dielectric layer 215 may have a thickness 215t of about to In some embodiments, the ratio of thickness 213t to thickness 215t may be in the range of about 2 to 50. If thickness 215t is greater than about If the thickness 215t is less than about 2, the dielectric constant of the gate dielectric layer 124 will be reduced. Or when the above ratio is greater than about 50, the concentration of the second metal element in the first high-k dielectric layer 213 will be less than about 5%, and the crystallization temperature of the first high-k dielectric layer 213 will not be reduced.

[0073] In some embodiments, a post deposition anneal (PDA) process may be performed after the deposition of the second high-k dielectric layer 215, for example, Fig.10As shown. In some embodiments, during the PDA process, the second metal element in the second high-k dielectric layer 215 can diffuse into the first high-k dielectric layer 213 to form a second dopant and reduce the crystallization temperature of the first high-k dielectric layer 213. In some embodiments, the PDA process can be performed at a temperature range of about 500° C. to 700° C. to crystallize the first high-k dielectric layer 213. Due to the second high-k dielectric layer 215 and the reduced annealing temperature, the regrowth of the interface layer 211 can be minimized during the PDA process. In this way, the gate capacitance and device performance can be improved. In some embodiments, the PDA process can be performed in a gas environment with a pressure in the range of about 10 mtorr to 5 torr and a duration in the range of about 1 second to 60 seconds. In some embodiments, the gas environment can include a mixture of oxygen, hydrogen and nitrogen. In some embodiments, the crystalline high-k dielectric material in the first high-k dielectric layer 213 can have a cubic crystalline phase or other crystalline phases. In some embodiments, doping the first high-k dielectric layer 213 with the second dopant may increase its dielectric constant.

[0074] In some embodiments, the concentration of the second metal element in the first high-k dielectric layer 213 may be in a range of about 5% to 25%. If the concentration of the second metal element in the first high-k dielectric layer 213 is less than about 5%, the crystallization temperature of the first high-k dielectric layer 213 will not decrease. If the concentration of the second metal element in the first high-k dielectric layer 213 is greater than about 25%, the defects of the first high-k dielectric layer 213 may increase due to the dopant concentration being higher than the dopant solubility limit. As the crystallization temperature of the first high-k dielectric layer 213 decreases, the defects at the interface between the interface layer 211 and the first high-k dielectric layer 213 may be reduced, the change in the dopant profile distribution in the nanostructure 222 and the source / drain (S / D) structure 110 may be minimized, and the stress between the nanostructure 222 and the source / drain (S / D) structure 110 may be maintained.

[0075] In some embodiments, the PDA process is optional and can be omitted. In some embodiments, the first high-k dielectric layer 213 can be crystallized during the deposition process of the second high-k dielectric layer 215. In some embodiments, after the PDA process, the second high-k dielectric layer 215 can diffuse into and mix with the first high-k dielectric layer 213, such as Fig.10 In some embodiments, after the PDA process, the second high-k dielectric layer 215 may be separated from the first high-k dielectric layer 213, as shown in FIG. Figure 2 and Fig. 9 shown.

[0076] In some embodiments, as shown in FIG. 11 , a first portion 213-1 of the first high-k dielectric layer 213 may be deposited on the interface layer 211. A dipole source layer 717 may be deposited on the first portion 213-1 of the first high-k dielectric layer 213 so as to dope the first portion 213-1 with a first dopant and form a dipole in the first portion 213-1 (not shown). After removing the dipole source layer 717, a second high-k dielectric layer 215 may be deposited on the doped first portion 213-1 of the first high-k dielectric layer 213. The deposition of the second high-k dielectric layer 215 may be followed by the deposition of a second portion 213-2 of the first high-k dielectric layer 213. In some embodiments, the first portion 213-1 and the second portion 213-2 of the first high-k dielectric layer 213 may include the same high-k dielectric material. The first portion 213-1 and the second portion 213-2 of the first high-k dielectric layer 213 and the second high-k dielectric layer 215 can be processed by the above-mentioned PDA process. The PDA process can diffuse the second dopant in the second high-k dielectric layer 215 into the first high-k dielectric layer 213. The second dopant can be different from the first dopant. The second dopant can reduce the crystallization temperature of the high-k dielectric material in the first high-k dielectric layer 213. In some embodiments, the total thickness of the first portion 213-1 and the second portion 213-2 of the first high-k dielectric layer 213 can be approximately in the range of 1 nm to 5 nm.

[0077] In some embodiments, Fig.12 As shown, a second high-k dielectric layer 215 having a second dopant may be deposited on the interface layer 211. A first portion 213-1 of the first high-k dielectric layer 213 may be deposited on the second high-k dielectric layer 215, and the first dopant may be doped with a dipole source layer 717 to form a dipole in the first portion 213-1 of the first high-k dielectric layer 213. The first dopant may be different from the second dopant. A second portion 213-2 of the first high-k dielectric layer 213 may be deposited on the doped first portion 213-1. In some embodiments, the first and second portions of the first high-k dielectric layer 213 may include the same high-k dielectric material. In some embodiments, the total thickness of the first portion 213-1 and the second portion 213-2 of the first high-k dielectric layer 213 may be approximately in the range of 1 nm to 5 nm. The first high-k dielectric layer 213 and the second high-k dielectric layer 215 may be processed using the above-described PDA process. The PDA process can diffuse the second dopant in the second high-k dielectric layer 215 into the first high-k dielectric layer 213 and reduce the crystallization temperature of the first high-k dielectric layer 213 .

[0078] After doping the first high-k dielectric layer 213 with the second dopant, the source / drain (S / D) structure 110, the gate structure 112, and the etch stop layer (ESL) 116 and the interlayer dielectric (ILD) layer 118 may be formed, but for the sake of clarity, they are not described in detail. After these steps, the semiconductor device 100 having the crystalline first high-k dielectric layer 213 produced at a reduced crystallization temperature may be as shown in FIG. Figure 1 and Figure 2 drawn.

[0079] Various embodiments in the present disclosure provide exemplary methods for forming a crystalline first high-k dielectric layer 213 at a reduced crystallization temperature in a semiconductor device 100. In some embodiments, a nanostructure 222 may be formed on a substrate 104, and an interface layer 211 may be formed on the nanostructure 222. A first high-k dielectric layer 213 may be formed on the interface layer 211, and a first dopant may be doped to form a dipole. The first dopant may include a first metal element, and a dipole may be formed within the first high-k dielectric layer and / or at an interface between the interface layer 211 and the first high-k dielectric layer 213. A second high-k dielectric layer 215 may be formed on the first high-k dielectric layer 213, and the second high-k dielectric layer 215 may include a second metal element different from the first metal element. The second metal element may diffuse into the first high-k dielectric layer 213 as a second dopant during a subsequent annealing process, and may reduce the crystallization temperature of the first high-k dielectric layer 213. In some embodiments, the crystallization temperature can be reduced to about 500° C. to 700° C. Therefore, the first high-k dielectric layer 213 can be crystallized at a lower temperature and the thermal budget of the manufacturing process can be reduced. In addition, defects at the interface between the interface layer 211 and the first high-k dielectric layer 213 can be reduced, the change in the dopant profile distribution within the nanostructure 222 and the source / drain (S / D) structure 110 of the semiconductor device 100 can be minimized, and the stress between the nanostructure 222 and the source / drain (S / D) structure 110 can be maintained.

[0080] In some embodiments, a method for manufacturing a semiconductor device includes: forming a channel structure on a substrate; forming an interface layer on the channel structure; forming a first high-k dielectric layer on the interface layer; forming a dipole in the first high-k dielectric layer with a dopant; and forming a second high-k dielectric layer on the first high-k dielectric layer. The dopant includes a first metal element. The second high-k dielectric layer includes a second metal element different from the first metal element.

[0081] In some embodiments, the method further includes annealing the first high-k dielectric layer and the second high-k dielectric layer at a temperature of about 500° C. to 700° C. to diffuse the second metal element into the first high-k dielectric layer. In some embodiments, the method further includes forming a gate structure on the second high-k dielectric layer. In some embodiments, forming a channel structure includes forming a set of nanostructures on a substrate. In some embodiments, forming a second high-k dielectric layer includes depositing a high-k dielectric material on the first high-k dielectric layer. The high-k dielectric material includes lutetium oxide, yttrium oxide, thulium oxide, erbium oxide, or gadolinium oxide. In some embodiments, the dopant includes lutetium oxide, scandium oxide, yttrium oxide, thulium oxide, erbium oxide, gadolinium oxide, lanthanum oxide, zinc oxide, germanium oxide, aluminum oxide, titanium oxide, or vanadium oxide. In some embodiments, the method further includes forming a third high-k dielectric layer on the second high-k dielectric layer. The first high-k dielectric layer and the third high-k dielectric layer include the same high-k dielectric material. In some embodiments, forming a dipole in the first high-k dielectric layer includes: depositing a dipole source layer on the first high-k dielectric layer, wherein the dipole source layer includes the above-mentioned dopant; annealing the dipole source layer to diffuse the dopant into the first high-k dielectric layer; and removing the dipole source layer.

[0082] In some embodiments, a method for manufacturing a semiconductor device includes: forming first and second channel structures on a substrate; forming an interface layer on the first and second channel structures; forming a first dielectric layer on the interface layer on the first and second channel structures; forming a dipole with a first dopant in the first dielectric layer on the first channel structure; forming a dipole with a second dopant in the first dielectric layer on the second channel structure; and forming a second dielectric layer on the first dielectric layer. The first dopant includes a first metal element. The second dopant includes a second metal element different from the first metal element. The second dielectric layer includes a third metal element different from the first and second metal elements.

[0083] In some embodiments, the method further includes: annealing the first dielectric layer and the second dielectric layer at a temperature of about 500° C. to 700° C. to diffuse the third metal element into the first dielectric layer and the second dielectric layer. In some embodiments, the method further includes: forming a first gate structure on the second dielectric layer above the first channel structure, and forming a second gate structure different from the first gate structure on the second dielectric layer above the second channel structure. In some embodiments, forming the first and second channel structures includes forming first and second sets of nanostructures on a substrate. In some embodiments, forming the second dielectric layer includes depositing a high-k dielectric material on the first dielectric layer, wherein the high-k dielectric material includes lutetium oxide, yttrium oxide, thulium oxide, erbium oxide, or gadolinium oxide. In some embodiments, the method further includes: forming a third dielectric layer on the second dielectric layer, wherein the first dielectric layer and the third dielectric layer include the same high-k dielectric material. In some embodiments, forming a dipole in the first dielectric layer on the first and second channel structures includes: depositing a first dipole source layer including a first dopant on the first dielectric layer on the first channel structure, wherein the first dopant includes lutetium oxide, scandium oxide, yttrium oxide, thulium oxide, erbium oxide, gadolinium oxide, or lanthanum oxide; annealing the first dipole source layer to diffuse the first dopant into the first dielectric layer on the first channel structure; removing the first dipole source layer; depositing a second dipole source layer including a second dopant on the first dielectric layer on the second channel structure, wherein the second dopant includes zinc oxide, germanium oxide, aluminum oxide, titanium oxide, or vanadium oxide; annealing the second dipole source layer to diffuse the second dopant into the first dielectric layer on the second channel structure; and removing the second dipole source layer.

[0084] In some embodiments, a semiconductor structure includes: a channel structure on a substrate, an interface layer on the channel structure, a first high-k dielectric layer on the interface layer on the channel structure, and a second high-k dielectric layer on the first high-k dielectric layer. The first high-k dielectric layer is doped with a first dopant including a first metal element and a second dopant including a second metal element different from the first metal element. The second high-k dielectric layer includes a second metal element.

[0085] In some embodiments, the second metal element comprises lutetium or yttrium. In some embodiments, the semiconductor structure further comprises an additional channel structure, wherein the first high-k dielectric layer located on the additional channel structure is doped with a third dopant comprising a third metal element different from the first metal element and the second metal element. In some embodiments, the first high-k dielectric layer is crystalline and comprises the second metal element at a concentration of about 5% to 5%. In some embodiments, the ratio of the thickness of the first high-k dielectric layer to the thickness of the second high-k dielectric layer is in the range of about 2 to 50.

[0086] It should be understood that the claims are interpreted not by the above abstract, but by the above implementation. The abstract may describe one or more embodiments of the present disclosure contemplated by the inventor, but not all possible embodiments, and therefore, does not limit the attached claims in any way.

[0087] The above briefly describes the characteristic components of several embodiments of the present invention, so that those with ordinary knowledge in the relevant technical field can more easily understand the types of the present disclosure. Anyone with ordinary knowledge in the relevant technical field should understand that the present disclosure can be easily used as a basis for the change or design of other processes or structures to achieve the same purpose and / or obtain the same advantages as the embodiments described herein. Anyone with ordinary knowledge in the relevant technical field can also understand that structures equivalent to the above do not depart from the spirit and scope of protection of the present disclosure, and can be changed, replaced and modified without departing from the spirit and scope of the present disclosure.

Claims

1. A method for manufacturing a semiconductor device, include: forming a channel structure on a substrate; Forming an interface layer on the channel structure forming a first high-k dielectric layer on the interface layer; forming a dipole in the first high-k dielectric layer using a dopant, wherein the dopant includes a first metal element; A second high-k dielectric layer is formed on the first high-k dielectric layer, wherein the second high-k dielectric layer includes a second metal element different from the first metal element.

2. The method for manufacturing a semiconductor device according to claim 1, further comprising: include: The first high-k dielectric layer and the second high-k dielectric layer are annealed at a temperature of about 500° C. to 700° C. to diffuse the second metal element into the first high-k dielectric layer.

3. The method for manufacturing a semiconductor device according to claim 1, further comprising: include: A third high-k dielectric layer is formed on the second high-k dielectric layer, wherein the first high-k dielectric layer and the third high-k dielectric layer comprise the same high-k dielectric material.

4. The method for manufacturing a semiconductor device as claimed in claim 1, wherein the dipole is formed in the first high-k dielectric layer. include: Depositing a dipole source layer on the first high-k dielectric layer, wherein the dipole source layer includes the dopant; annealing the dipole source layer to diffuse the dopant into the first high-k dielectric layer; and The dipole source layer is removed.

5. A method for manufacturing a semiconductor device, include: forming a first channel structure and a second channel structure on a substrate; forming an interface layer on the first channel structure and the second channel structure; forming a first dielectric layer on the first channel structure and the interface layer on the second channel structure; forming a dipole with a first dopant in the first dielectric layer on the first channel structure, wherein the first dopant is a first metal element; forming a dipole with a second dopant in the first dielectric layer on the second channel structure, wherein the second dopant includes a second metal element different from the first metal element; and A second dielectric layer is formed on the first dielectric layer, wherein the second dielectric layer includes a third metal element different from the first metal element and the second metal element.

6. The method for manufacturing a semiconductor device as claimed in claim 5, wherein forming the second dielectric layer comprises depositing a high-k dielectric material on the first dielectric layer, wherein the high-k dielectric material comprises lutetium oxide, yttrium oxide, thulium oxide, erbium oxide or gadolinium oxide.

7. The method for manufacturing a semiconductor device according to claim 5, further comprising: include: A third dielectric layer is formed on the second dielectric layer, wherein the first dielectric layer and the third dielectric layer include the same high-k dielectric material.

8. The method for manufacturing a semiconductor device as claimed in claim 5, wherein a dipole is formed in the first dielectric layer on the first channel structure and the second channel structure. include: Depositing a first dipole source layer including the first dopant on the first dielectric layer on the first channel structure, wherein the first dopant includes lutetium oxide, scandium oxide, yttrium oxide, thulium oxide, erbium oxide, gadolinium oxide or lanthanum oxide; annealing the first dipole source layer to diffuse the first dopant into the first dielectric layer on the first channel structure; removing the first dipole source layer; Depositing a second dipole source layer including the second dopant on the first dielectric layer on the second channel structure, wherein the second dopant includes zinc oxide, germanium oxide, aluminum oxide, titanium oxide or vanadium oxide; annealing the second dipole source layer to diffuse the second dopant into the first dielectric layer on the second channel structure; as well as The second dipole source layer is removed.

9. A semiconductor device, include: a channel structure located on a substrate; an interface layer, located on the channel structure; a first high-k dielectric layer located on the interface layer on the channel structure, wherein the first high-k dielectric layer is doped with a first dopant including a first metal element and a second dopant including a second metal element different from the first metal element; and A second high-k dielectric layer is located on the first high-k dielectric layer, wherein the second high-k dielectric layer includes the second metal element.

10. The semiconductor device of claim 9, wherein the first high-k dielectric layer is crystalline and includes the second metal element at a concentration of about 5% to 5%.