Perovskite composite film material, preparation method and application thereof, and perovskite light-emitting diode device
By generating a lead oxysalt layer in situ on the surface of the perovskite film, the stability problem of perovskite light-emitting diode devices caused by ion migration is solved, achieving higher stability and improved lifespan.
Patent Information
- Application Number
- CN202410883836.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-08
AI Technical Summary
The life of perovskite light-emitting diode devices is short, mainly due to internal defects and interface halide accumulation caused by ion migration, which affects its stability and electrical performance. The existing methods are not ideal.
A lead oxide salt layer is generated in situ on the surface of the perovskite film. The lead oxide salt layer has strong mechanical properties and can passivate surface defects of the perovskite and inhibit ion migration, thus improving the stability of the device.
Through the protection of the lead oxide salt layer, the stability and life of the perovskite light-emitting diode device are significantly improved, the non-radiative recombination loss of carriers is reduced, the ion movement damage between the perovskite and the electrode is blocked, and the device performance is improved. overall performance.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic devices, and more specifically, to a perovskite composite thin film material, a preparation method and application thereof, and a perovskite light-emitting diode device. Background Art
[0002] With the continuous optimization of perovskite film components and the improvement of device structure, the external quantum efficiency (EQE) of perovskite light-emitting diode devices has exceeded 20%. However, the operating life of visible light devices is only a few hours to a few hundred hours. Compared with organic light-emitting diode devices, the life of perovskite light-emitting diode devices is much shorter and far below the requirements of display applications. To realize the display application of green and red light devices, the devices are required to have a working life of at least tens of thousands of hours.
[0003] The reasons for the degradation of perovskite light-emitting diode devices are relatively complex, among which ion migration is considered to be one of the main reasons restricting its stability. Ion migration can cause vacancy defects inside the perovskite, accumulation of interface halides, and deformation of the crystal structure, which in turn affects the performance and stability of the perovskite material. In addition, halogen ions migrating through the interface to the metal electrode may also corrode the electrode, thereby reducing its electrical properties. Since ion migration is the main cause of the degradation of perovskite light-emitting diode devices, inhibiting ion migration has become the main strategy to improve the stability of the device. At present, researchers mainly add various additives to perovskite to enable it to repair defects or fix mobile ions through chemical reactions to inhibit ion migration in the device. However, the effect of this method is not ideal. The reason is that the instability of the interface of each functional layer is a major factor limiting the life of the device. The ideal charge transfer interface should have morphological stability when the device is working, and protect the perovskite layer from damage to the perovskite by the migration of electrode metal ions.
[0004] Therefore, it is urgent to develop a method that can improve the morphological stability of the charge transfer interface and protect the perovskite layer from damage to the perovskite caused by the migration of electrode metal ions, so as to improve the stability of perovskite light-emitting diode devices. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a perovskite composite thin film material and a preparation method and application thereof, and a perovskite light-emitting diode device. The perovskite composite thin film material provided by the present invention generates a lead-oxygen salt layer in situ on the surface of the perovskite, and the lead-oxygen salt layer has excellent mechanical properties and water-oxygen stability, and can passivate the surface defects of the perovskite, inhibit ion migration in the device, thereby comprehensively improving the stability of the perovskite light-emitting diode device.
[0006] A first aspect of the present invention provides a perovskite composite thin film material.
[0007] Specifically, a perovskite composite thin film material includes a perovskite film and a lead oxide salt layer, wherein the lead oxide salt layer covers the surface of the perovskite film; the raw material for preparing the lead oxide salt layer includes an organic salt, and the organic salt is a salt formed by an inorganic acid and an organic base.
[0008] The present invention covers a layer of lead oxide salt on the surface of the perovskite film, which is similar to giving the perovskite film a protective "shell layer", and the lead oxide salt layer has strong mechanical properties. Further, the perovskite composite film material with a protective "shell layer" is used to prepare a perovskite light-emitting diode device, which can improve the interface stability of the perovskite film surface on the one hand, and passivate the defects on the surface of the perovskite film on the other hand, inhibit ion migration in the device, thereby improving the stability of the perovskite light-emitting diode device.
[0009] Preferably, the thickness of the perovskite film is 20-60 nm.
[0010] Preferably, the thickness of the lead oxide salt layer is 2-5 nm. The thickness of the lead oxide salt layer is much thinner than that of the perovskite film, but the lead oxide salt layer of this thin layer structure has strong mechanical properties and can act as a thin protective shell, which can well protect the perovskite film and improve its stability.
[0011] Preferably, the material of the perovskite film is a three-dimensional perovskite material ABX3, wherein A is a methylamine ion (MA + ), formamidinium ion (FA + ), cesium ion (Cs + ), B is Pb 2+ , X is Br - , Cl - ,I - One of them or its quasi-two-dimensional (A'2 An- 1B n X 3n+1 , where A' is a relatively large organic amine cation, such as PEA + 、Bu + ) and perovskite quantum dot materials.
[0012] Preferably, the inorganic acid is at least one of phosphoric acid, sulfuric acid, carbonic acid and silicic acid, and / or the organic base is an amino-containing organic compound.
[0013] Preferably, the amino-containing organic compound is at least one of phenylethylamine, butylamine and octylamine.
[0014] Preferably, the organic salt is at least one of an organic phosphate, an organic sulfate, an organic carbonate and an organic silicate.
[0015] More preferably, the organic salt is at least one of amino-containing organic matter-phosphate, amino-containing organic matter-sulfate, amino-containing organic matter-carbonate, and amino-containing organic matter-silicate.
[0016] A second aspect of the present invention provides a method for preparing a perovskite composite thin film material.
[0017] A method for preparing a perovskite composite thin film material comprises the following steps:
[0018] An organic salt solution is applied to the surface of the perovskite film to cause an ion reaction and in-situ growth to obtain a lead oxide salt layer, thereby obtaining the perovskite composite film material; the organic salt is a salt formed by an inorganic acid and an organic base.
[0019] The present invention directly applies a salt solution to the surface of the perovskite film, so that an in-situ ion reaction occurs between the organic salt and the surface of the perovskite film, and a uniform and dense lead oxygen salt layer is in-situ produced on the surface of the perovskite film. Moreover, due to the fact that such lead oxygen salts (such as phosphates, sulfates, carbonates or silicates) have a very large solubility product coefficient in water (which can reach more than 40), the formed lead oxygen salt layer is completely insoluble in water, so the influence of water molecules on the perovskite film can be effectively reduced, and the perovskite film can be used as a "shell layer" that plays a good protective role on the perovskite film.
[0020] Preferably, the temperature of the ion reaction is 20-30° C., and / or the time of the ion reaction is 5-15 s.
[0021] Preferably, after the ion reaction, spin coating is performed, the rotation speed of the spin coating is 4000-6000 rpm, and / or the spin coating time is 20-30 s.
[0022] Preferably, during the spin coating process, a solvent is added dropwise for cleaning.
[0023] Preferably, the solvent used for the washing is the same as the solvent in the salt solution.
[0024] Preferably, the concentration of the organic salt solution is 0.01-0.05 mmol / L.
[0025] Further preferably, the concentration of the organic salt solution is 0.02-0.04 mmol / L.
[0026] Preferably, the organic salt solution is diluted 10 times, 100 times or 1000 times with a solvent before use.
[0027] Further preferably, the organic salt solution is diluted 100 times with a solvent before use.
[0028] Preferably, the solvent in the organic salt solution is at least one of toluene, chlorobenzene and isopropanol.
[0029] Preferably, the method for preparing the perovskite film comprises the following steps:
[0030] Firstly, a perovskite precursor is prepared, and then the perovskite precursor is spin-coated on the surface of a substrate and annealed to obtain the perovskite film.
[0031] Preferably, the molar concentration of the solute in the perovskite precursor is 0.01-1 mol / L.
[0032] Preferably, the three-dimensional perovskite material and an organic solvent are mixed to prepare a perovskite precursor.
[0033] Further preferably, the three-dimensional perovskite material and the organic solvent are mixed, stirred at 50-70° C. for 1-3 h, and filtered to obtain a perovskite precursor.
[0034] Preferably, the organic solvent is at least one of dimethyl sulfoxide, N,N-dimethylformamide and butyrolactone.
[0035] Preferably, the perovskite precursor is dropped onto the substrate surface, first rotated at 900-1100 rpm for 7-12 s, then rotated at 2500-3500 rpm for 55 s for annealing; or directly rotated at 2500-3500 rpm for 50-70 s for annealing.
[0036] Preferably, the annealing temperature is 90-110° C., and / or the annealing time is 1-5 min.
[0037] Further preferably, the annealing temperature is 100-110° C., and / or the annealing time is 1-2 min.
[0038] A third aspect of the present invention provides an application of a perovskite composite thin film material.
[0039] The invention discloses an application of a perovskite composite thin film material in preparing a perovskite light-emitting diode device.
[0040] A fourth aspect of the present invention provides a perovskite light emitting diode device.
[0041] A perovskite light-emitting diode device comprises the perovskite composite thin film material.
[0042] Preferably, the perovskite light-emitting diode device comprises a conductive substrate, a hole transport layer, a hole modification layer, an active light-emitting layer, an electron transport layer, an electrode modification layer and an electrode in sequence; or comprises a conductive substrate, an electron transport layer, a hole modification layer, an active light-emitting layer, a hole transport layer, an electrode modification layer and an electrode in sequence; the material of the active light-emitting layer is the perovskite composite thin film material.
[0043] Preferably, the conductive substrate is made of a tin-doped indium dioxide transparent conductive substrate (ITO) and / or a fluorine-doped tin dioxide transparent conductive substrate (FTO).
[0044] Preferably, the material of the hole transport layer is at least one of poly[(N,N'-(4-n-butylphenyl)-N,N'-diphenyl-1,4-phenylenediamine)-alt-(9,9-di-n-octylfluorenyl-2,7-diyl)] (TFB), poly(9-vinylcarbazole) (PVK), 4-butyl-N,N-diphenylaniline homopolymer (TPD), 4-[1-[4-[di(4-methylphenyl)amino]phenyl]cyclohexyl]-N-(3-methylphenyl)-N-(4-methylphenyl)aniline (TPAC), N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB), and nickel oxide (NiOX).
[0045] Preferably, the hole transport layer has a thickness of 10-100 nm.
[0046] Further preferably, the hole transport layer has a thickness of 30-40 nm.
[0047] Preferably, the hole modification layer is made of at least one of lithium fluoride, aluminum oxide and molybdenum oxide.
[0048] Preferably, the hole modification layer has a thickness of 1-6 nm.
[0049] More preferably, the hole modification layer has a thickness of 3-5 nm.
[0050] Preferably, the material of the electron transport layer is at least one of 1,3,5-tris(1-phenyl-1H-benzimidazol-2-yl)benzene (TPBi), [6.6]-phenyl-C61-butyric acid methyl ester (PCBM), 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD), 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP), 4,7-diphenyl-1,10-phenanthroline (Bphen), titanium oxide (TiO2), and zinc oxide (ZnO).
[0051] Preferably, the thickness of the electron transport layer is 5-80 nm.
[0052] Further preferably, the thickness of the electron transport layer is 30-40 nm.
[0053] Preferably, the material of the electrode modification layer is lithium fluoride.
[0054] Preferably, the thickness of the electrode modification layer is 1-6 nm.
[0055] Further preferably, the thickness of the electrode modification layer is 2-3 nm.
[0056] Preferably, the electrode is made of at least one of aluminum, silver, gold and copper.
[0057] Preferably, the thickness of the electrode is 30-300 nm.
[0058] Further preferably, the thickness of the electrode is 80-100 nm.
[0059] A fifth aspect of the present invention provides a method for preparing a perovskite light-emitting diode device.
[0060] A method for preparing a perovskite light-emitting diode device comprises the following steps:
[0061] (1) forming a hole transport layer on the surface of a conductive substrate;
[0062] (2) forming a hole modification layer on the surface of the hole transport layer;
[0063] (3) forming an active light-emitting layer on the surface of the hole modification layer;
[0064] (4) sequentially forming an electron transport layer, an electrode modification layer and an electrode on the surface of the active light-emitting layer to obtain the perovskite light-emitting diode device;
[0065] or,
[0066] (1) forming an electron transport layer on the surface of a conductive substrate;
[0067] (2) forming a hole modification layer on the surface of the electron transport layer;
[0068] (3) forming an active light-emitting layer on the surface of the hole modification layer;
[0069] (4) forming a hole transport layer, an electrode modification layer and an electrode in sequence on the surface of the active light-emitting layer to obtain the perovskite light-emitting diode device.
[0070] Preferably, in step (1), the conductive substrate is first pretreated with oxygen plasma.
[0071] Preferably, in step (3), a perovskite film is first prepared on the surface of the modified layer by spin coating, and then an ion reaction occurs on the surface of the perovskite film to prepare the perovskite composite film material.
[0072] A sixth aspect of the present invention provides an application of a perovskite light emitting diode device.
[0073] A perovskite light-emitting diode device is used in the preparation of display screens, lighting equipment, and solar cells.
[0074] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0075] The perovskite composite film material provided by the present invention includes a perovskite film and a lead-oxygen salt layer, the lead-oxygen salt layer covers the surface of the perovskite film, and the raw materials for preparing the lead-oxygen salt layer include organic salts, which are salts formed by inorganic acids and organic bases. This lead-oxygen salt layer has strong mechanical properties, similar to giving the perovskite film a protective "shell" with excellent mechanical properties. The perovskite composite film material provided by the present invention is further applied to the preparation of perovskite light-emitting diode devices. Since the lead-oxygen salt layer is completely insoluble in water, the influence of water molecules on the perovskite film can be effectively reduced; and the lead-oxygen salt layer is relatively thin, which effectively passivates the surface defects of the perovskite and reduces the non-radiative recombination loss of carriers in the device; in addition, the lead-oxygen salt layer has strong mechanical properties, can inhibit ion migration, and can effectively block the damage caused by ion movement between the perovskite and the electrode, thereby improving the stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1 This is a schematic diagram of the structure of a perovskite light-emitting diode device obtained in Application Example 1 of the present invention;
[0077] FIG2 is a reaction equation of an amino-containing organic compound-phosphate prepared in Example 1 of the present invention and a schematic diagram of the molecular structure of a lead-oxygen salt layer formed;
[0078] Figure 3 This is a scanning electron microscope (SEM) comparison diagram of the perovskite film of Comparative Example 1 and the perovskite composite thin film material prepared in Example 1 of the present invention;
[0079] Figure 4 The XPS spectra of P 2p and O1s on the surface of the perovskite composite thin film material prepared in Example 1 of the present invention;
[0080] Figure 5 This is a comparison diagram of electroluminescence spectra of the perovskite light-emitting diode devices of Application Example 1 of the present invention and Comparative Application Example 1;
[0081] Figure 6 This is a performance comparison diagram of the perovskite light-emitting diode device of Application Example 1 of the present invention and Comparative Application Example 1;
[0082] Figure 7 TEM comparison of the perovskite film before and after the reaction with PEAP in Example 1 of the present invention. DETAILED DESCRIPTION
[0083] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0084] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0085] Example 1
[0086] A perovskite composite film material comprises a perovskite film and a lead-oxygen salt layer, wherein the lead-oxygen salt layer covers the surface of the perovskite film, and the raw materials for preparing the lead-oxygen salt layer comprise phenylethylamine-phosphate (organic salt).
[0087] The method for preparing the above-mentioned perovskite composite thin film material comprises the following steps:
[0088] (1) Preparation of perovskite precursor solution: 0.2 mmol PbBr2, 0.2 mmol CsBr, and 0.08 mmol PEABr were added to a solution containing crown ether (3.5 mg mL -1 ) in DMSO (1 mL), and stirred at 60° C. for 2 h to obtain a perovskite precursor solution; filtering the prepared perovskite precursor solution with a 0.45 μm organic filter head for later use;
[0089] (2) Preparation of organic phosphate (phenylethylamine phosphate): 100 μL phosphoric acid and 650 μL phenylethylamine (PEA) were diluted to 3 times with a mixed solvent (toluene:isopropanol volume ratio = 5:1), and then the diluted phenylethylamine was slowly added to the phosphoric acid dilution solution. The process was kept stirring. The reaction equation is shown in FIG. 2(a) to obtain phenylethylamine phosphate (Phenylethylamine phosphate, referred to as PEAP); the resulting solution was diluted to 100 times with a mixed solvent;
[0090] (3) Preparation of perovskite film: A two-step spin coating annealing method was used to drop 100 μL of perovskite precursor solution onto the substrate, first spinning at 1000 rpm for 10 s; then spinning at 3000 rpm for 55 s, and then heating and annealing at 100°C for 1 min to obtain a perovskite film;
[0091] (4) Preparation of perovskite composite thin film material (growth of lead oxide salt layer): 100 μL of diluted organic phosphate solution was dropped on the perovskite film, and after standing for 5 seconds for ion reaction, a lead oxide salt layer was generated in situ. The film was spin-coated at a speed of 5000 rpm for 50 seconds, and during the spin-coating process, i.e., 25 seconds after the start of spin-coating, a mixed solvent of toluene / isopropanol (5:1) was added for cleaning to obtain a perovskite composite thin film material.
[0092] The molecular structure of the lead-oxygen salt layer obtained by the ion reaction of organic phosphate on the surface of the perovskite film is shown in Figure 2(b). The lead-oxygen salt layer plays a protective role on the surface of the perovskite film and can effectively reduce the influence of water molecules on the perovskite film. 2- Represents the octahedral structure composed of lead ions and halogen ions.
[0093] Example 2
[0094] A perovskite composite film material comprises a perovskite film and a lead-oxygen salt layer, wherein the lead-oxygen salt layer covers the surface of the perovskite film, and the raw materials for preparing the lead-oxygen salt layer comprise organic sulfate.
[0095] The above method for preparing the perovskite composite thin film material is different from that of Example 1 in that step (2) and step (4) are different, as follows:
[0096] (1) Preparation of perovskite precursor solution: 0.2 mmol PbBr2, 0.2 mmol CsBr, and 0.08 mmol PEABr were added to a solution containing crown ether (3.5 mg mL -1 ) in DMSO (1 mL), and stirred at 60° C. for 2 h to obtain a perovskite precursor solution. The prepared perovskite precursor solution was filtered with a 0.45 μm organic filter for later use;
[0097] (2) Preparation of organic sulfate: sulfuric acid and octylamine (molar ratio of 1:3) were diluted with toluene respectively, and then the diluted octylamine was slowly added dropwise into the sulfuric acid while stirring. The resulting solution was diluted to 100 times with toluene;
[0098] (3) Preparation of perovskite film: A two-step spin coating annealing method was used to take 100 μL of perovskite precursor solution and drop it onto the substrate. The substrate was first spun at 1000 rpm for 10 s, then spun at 3000 rpm for 55 s, and then heated and annealed at 100 °C for 1 min to obtain a perovskite film.
[0099] (4) Preparation of perovskite composite thin film material: 100 μL of diluted organic sulfate solution was dropped on the perovskite film. After reacting for 5 seconds, the film was spin-coated at 5000 rpm for 50 seconds. During the spin-coating process, i.e., after 25 seconds, toluene was added for cleaning.
[0100] Example 3
[0101] A perovskite composite film material comprises a perovskite film and a lead-oxygen salt layer, wherein the lead-oxygen salt layer covers the surface of the perovskite film, and the raw materials for preparing the lead-oxygen salt layer include organic phosphate.
[0102] The above method for preparing the perovskite composite thin film material is different from that of Example 1 in that step (1) and step (3) are different, and are specifically as follows:
[0103] (1) Preparation of perovskite precursor solution: 1 mmol PbI2 and 1 mmol MAI were mixed in 2 mL DMSO to prepare MAPbI3 perovskite precursor solution;
[0104] (2) Preparation of organic phosphate: Phosphoric acid and phenethylamine were diluted with a mixed solvent (toluene: isopropanol = 5:1), and then the diluted phenethylamine was slowly added to the phosphoric acid while stirring. The resulting solution was diluted to 100 times with the mixed solvent;
[0105] (3) Preparation of perovskite film: Using a one-step spin coating annealing method, 100 μL of perovskite precursor solution was added to the substrate, rotated at 3000 rpm for 60 seconds, and then heated and annealed at 100 °C for 1 minute;
[0106] (4) Preparation of perovskite composite thin film material: 100 μL of the diluted organic phosphate solution was dropped on the perovskite film, allowed to react for 5 seconds, and then spin coated at 5000 rpm for 50 seconds. During the spin coating process, i.e., 25 seconds after the start of spin coating, a mixed solvent of toluene / isopropanol (5:1) was added for cleaning to obtain a perovskite composite thin film material.
[0107] Comparative Example 1
[0108] A perovskite thin film material, which differs from Example 1 in that it does not contain a lead oxide salt layer (there is no step related to growing a lead oxide salt layer).
[0109] Application Example 1
[0110] A perovskite light emitting diode device, having a structure as Figure 1 As shown, from bottom to top, it includes: an anode conductive substrate (or anode base, with a thickness of 150nm), a hole transport layer (with a thickness of 40nm), a hole modification layer (3nm), an active light-emitting layer (or an inorganic salt-perovskite core-shell layer, including a perovskite film and a lead oxygen salt layer, with a thickness of 40nm), an electron transport layer (with a thickness of 40nm), an electrode modification layer (with a thickness of 2nm) and a cathode (aluminum electrode, with a thickness of 100nm); wherein the active light-emitting layer is the perovskite composite thin film material prepared in Example 1.
[0111] The method for preparing the above-mentioned perovskite light-emitting diode device comprises the following steps:
[0112] (1) The ITO transparent anode substrate was ultrasonically cleaned with acetone, ethanol, and deionized water for 20 minutes respectively, dried with nitrogen, and then treated with oxygen plasma for 15 minutes;
[0113] (2) Preparation of hole transport layer: Stir the purchased PEDOT:PSS solution at room temperature for 1 hour, filter it with a 0.22μm filter head and set aside to obtain a hole transport layer solution. In air, first use a one-step spin coating method to spin-coat the hole transport layer solution on the ITO substrate. Use a pipette to draw 100μL of PEDOT:PSS, then spin-coat at 4000rpm for 40s, and then anneal on a hot plate at 150℃ for 20min;
[0114] (3) Preparation of the modified layer: Place the sample in a vacuum evaporator and evacuate the sample. When the vacuum degree is less than 2×10 - 6 mbar, and then the evaporation started. 3nm LiF was evaporated at a speed of
[0115] (4) Preparation of active light-emitting layer (i.e., preparation of perovskite composite thin film material of Example 1): 100 μL of perovskite precursor was dripped onto the substrate, and first rotated at 1000 rpm for 10 s; then rotated at 3000 rpm for 55 s, and then heated and annealed at 100° C. for 1 min; then 100 μL of diluted organic phosphate solution was dripped onto the perovskite film, allowed to react for 5 s, and then spin-coated at 5000 rpm for 50 s. During the spin-coating process, i.e., 25 s after the start of spin-coating, a mixed solvent of toluene / isopropanol (5:1) was dripped for cleaning;
[0116] (5) Preparation of electron transport layer and electrode: The sample was transferred to a vacuum evaporator and the vacuum was less than 2×10 - 6 mbar, the 40nm electron transport layer TPBi was evaporated, and the evaporation rate was Then The electrode modification layer LiF of 2nm was evaporated at a speed of 100nm of metal electrode Al was evaporated at a speed of 100nm. The effective light emitting area of the device is 9mm 2 After the experiment, the device after evaporation was taken out and its performance was characterized in a nitrogen glove box.
[0117] Application Example 2
[0118] A perovskite light-emitting diode device, which differs from Application Example 1 in that the active light-emitting layer is replaced by the perovskite composite thin film material prepared in Example 2.
[0119] Application Example 3
[0120] A perovskite light-emitting diode device, which differs from Application Example 1 in that the active light-emitting layer is replaced by the perovskite composite thin film material prepared in Example 1.
[0121] The method for preparing the above-mentioned perovskite light-emitting diode device comprises the following steps:
[0122] (1) The ITO transparent anode substrate was ultrasonically cleaned with acetone, ethanol, and deionized water for 20 minutes in sequence, dried with nitrogen, and then treated with oxygen plasma for 15 minutes. The substrate was placed in a nitrogen glove box to prepare the device;
[0123] (2) Preparation of hole transport layer: TFB was dissolved in chlorobenzene at a concentration of 8 mg / mL; 100 μL of TFB chlorobenzene solution was spin-coated at 1500 rpm for 45 seconds, and then annealed on a heating stage at 120°C for 20 minutes;
[0124] (3) Preparation of the modified layer: Place the sample in a vacuum evaporator and evacuate the sample. When the vacuum degree is less than 2×10 - 6 mbar, and then the evaporation started. 3nm LiF was evaporated at a speed of
[0125] (4) Preparation of active light-emitting layer: The perovskite film was prepared by a two-step spin coating annealing method. 100 μL of the perovskite precursor solution was filtered through a 0.45 μm organic filter and dripped onto the substrate. The solution was first spun at 1000 rpm for 10 s, then spun at 3000 rpm for 55 s, and then heated and annealed at 100° C. for 1 min.
[0126] (5) Shell preparation: 100 μL of the diluted phosphate solution was dropped on the perovskite film. After reacting for 5 seconds, the film was spin-coated at 5000 rpm for 50 seconds. During the spin-coating process, i.e., after 25 seconds, a mixed solvent of toluene / isopropanol was added for cleaning.
[0127] (6) Preparation of electron transport layer and electrode: The sample was transferred to a vacuum evaporator and the vacuum was less than 2×10 - 6 mbar, the 40nm electron transport layer TPBi was evaporated, and the evaporation rate was Then The electrode modification layer LiF of 2nm was evaporated at a speed of 100nm of metal electrode Al was evaporated at a speed of 100nm. The effective light emitting area of the device is 9mm 2 After the experiment, the device after evaporation was taken out and its performance was characterized in a nitrogen glove box.
[0128] Application Example 4
[0129] A perovskite light-emitting diode device, which differs from Application Example 1 in that the active light-emitting layer is replaced by the perovskite composite thin film material prepared in Example 3.
[0130] Application Example 5
[0131] A perovskite light-emitting diode device comprises, from bottom to top, ITO (thickness of 150 nm), an electron transport layer (thickness of 40 nm), a modification layer (3 nm), an active light-emitting layer (thickness of 40 nm), a hole transport layer (thickness of 40 nm), an electrode modification layer (thickness of 2 nm) and an Au electrode (thickness of 100 nm); wherein the active light-emitting layer is the perovskite composite thin film material prepared in Example 1.
[0132] The method for preparing the above-mentioned perovskite light-emitting diode device comprises the following steps:
[0133] (1) The ITO transparent anode substrate was ultrasonically cleaned with acetone, ethanol, and deionized water for 20 minutes respectively, dried with nitrogen, and then treated with oxygen plasma for 15 minutes;
[0134] (2) Preparation of electron transport layer: 1.5mmol Zn(Ac)2·2H2O was added to 15mL dimethyl sulfoxide (DMSO) and stirred to dissolve at 30°C. Then 2.8mmol TMAH·5H2O was dissolved in 5mL ethanol. The two solutions were then mixed. The mixture was stirred for 24h and then entered the precipitation process. Nano-zinc oxide was precipitated with ethyl acetate, and the precipitate was washed again with ethanol and ethyl acetate. Finally, the ZnO nanoparticles were redispersed in 8mL ethanol to obtain ZnO nanoparticles. In air, 100uL of ZnO nanoparticle solution was taken and spin coated at 4000rpm for 30s;
[0135] (3) Preparation of the modified layer: Place the sample in a vacuum evaporator and evacuate the sample. When the vacuum degree is less than 2×10 - 6 mbar, and then the evaporation started. 3nm LiF was evaporated at a speed of
[0136] (4) Preparation of an active light-emitting layer (i.e., preparation of the perovskite composite thin film material of Example 1): A two-step spin coating annealing method was used, 100 μL of a perovskite precursor solution was filtered through a 0.45 μm organic filter head, and then dripped onto a substrate, first rotating at 1000 rpm for 10 s; then rotating at 3000 rpm for 55 s, and then heating and annealing at 100° C. for 1 min to obtain a perovskite film; 100 μL of a diluted organic phosphate solution was dripped onto the perovskite film, allowed to react for 5 s, and then spin coated at 5000 rpm for 50 s, and during the spin coating process, i.e., 25 s after the start of spin coating, a mixed solvent of toluene / isopropanol (5:1) was dripped for washing to obtain an active light-emitting layer;
[0137] (5) Preparation of hole transport layer: TFB was dissolved in chlorobenzene at a concentration of 8 mg / mL. 100 uL of TFB chlorobenzene solution was spin coated at 1500 rpm for 45 seconds, and then annealed on a heating stage at 120°C for 20 minutes;
[0138] (6) Preparation of electrode modification layer and Au electrode: Place the sample in a vacuum evaporator and evacuate the sample. When the vacuum degree is less than 2×10 -6 mbar and then 2nm LiF was evaporated at a speed of 100 nm of Au was evaporated at a speed of . After the experiment, the device after evaporation was taken out and the performance of the device was tested in a nitrogen glove box.
[0139] Comparative application example 1
[0140] A perovskite light-emitting diode device is different from Application Example 1 in that the perovskite composite thin film material of Example 1 is replaced by a perovskite film of Comparative Example 1 with the same thickness.
[0141] Product effect testing
[0142] The microscopic morphologies of the standard perovskite (Comparative Example 1) and the perovskite composite film materials prepared in Example 1 are as follows: Figure 3 (a) Figure 3 As shown in (b), it can be seen from the figure that after the lead oxide salt layer is generated by in-situ ion reaction in Example 1, the surface of the perovskite composite thin film material is smooth, uniform and dense.
[0143] In order to verify the existence of the lead-oxygen salt layer in the perovskite composite thin film material prepared in Example 1, the product was further characterized by XPS. The results are as follows: Figure 4 (a) Figure 4 As shown in (b), the P2P1 / 2, 2P5 / 2 and P=O, Pb=O peaks of O1s were detected on the surface of the perovskite, indicating that the phosphate and perovskite reacted to form lead phosphate. Figure 4 Binding Energy refers to binding energy, and Intensity refers to intensity.
[0144] Figure 5 (a) Figure 5 (b) are the electroluminescence spectra of the perovskite light-emitting diode devices of comparative application example 1 and application example 1. It can be seen from the figure that after the growth of the lead phosphate oxygen salt layer, the position of the device's luminescence peak remains unchanged and the spectrum does not move. Figure 5 Wavelenth is wavelength and Intensity is intensity.
[0145] Figure 6 (a) is a comparison diagram of the current density-voltage-luminance curve (JVL) of the perovskite light-emitting diode device of application example 1 (corresponding to the core-shell structure in the figure) and comparative application example 1 (corresponding to the shell-free structure in the figure), Figure 6 (b) is a comparison diagram of the external quantum efficiency-current density curve (EQE-J) of the perovskite light-emitting diode device of Application Example 1 and Comparative Application Example 1. Figure 6 As can be seen in (a), after phosphate treatment, the leakage current of the device is lower, and the maximum brightness is about 4 times that of the comparison device (the brightness of the comparison application example 1 is about 10,000, and the brightness of the application example 1 is about 40,000). Figure 6 As can be seen in (b), after phosphate treatment, the roll-off of device efficiency is significantly reduced and the stability of the device is improved. Figure 6 Here Voltage is voltage and Current density is current density.
[0146] Figure 7 (a) Figure 7 (b) are TEM images of the perovskite before and after the reaction with PEAP in Example 1. By comparison, it can be seen that the surface edge of the perovskite film before the reaction is smooth and has a clear lattice; after the reaction, the surface morphology of the perovskite film is irregular and has an amorphous structure, indicating that a layer of lead oxide salt has been successfully grown in situ on the surface of the perovskite film.
[0147] The perovskite composite thin film material prepared in Example 2-3 has similar structure and performance to that of Example 1, and the perovskite light-emitting diode device prepared in Application Example 2-5 has similar performance to that of Application Example 1.
Claims
1. A perovskite composite thin film material, characterized in that: It includes a perovskite film and a lead oxide salt layer, wherein the lead oxide salt layer covers the surface of the perovskite film; the raw materials for preparing the lead oxide salt layer include organic salts, and the organic salts are salts formed by inorganic acids and organic bases.
2. The perovskite composite thin film material according to claim 1, characterized in that: The material of the perovskite film is a three-dimensional perovskite material ABX3, wherein A is one of methylamine ion, formamidine ion and cesium ion, and B is Pb 2+ , X is Br - , Cl - ,I - One of them or its quasi-two-dimensional and perovskite quantum dot materials.
3. The perovskite composite thin film material according to claim 1, characterized in that: The inorganic acid is at least one of phosphoric acid, sulfuric acid, carbonic acid and silicic acid, and / or the organic base is an amino-containing organic substance.
4. A method for preparing a perovskite composite thin film material, characterized in that: The steps include: An organic salt solution is applied to the surface of the perovskite film to cause an ion reaction and in-situ growth to obtain a lead oxide salt layer, thereby obtaining the perovskite composite film material; the organic salt is a salt formed by an inorganic acid and an organic base.
5. The method for preparing the perovskite composite thin film material according to claim 4, characterized in that: The temperature of the ion reaction is 20-30° C., and / or the time of the ion reaction is 5-15 s.
6. Use of the perovskite composite thin film material according to any one of claims 1 to 3 in the preparation of a perovskite light-emitting diode device.
7. A perovskite light-emitting diode device, characterized in that: The perovskite composite thin film material comprises the perovskite composite thin film material according to any one of claims 1 to 3.
8. The perovskite light-emitting diode device according to claim 7, characterized in that: The perovskite light-emitting diode device comprises a conductive substrate, a hole transport layer, a hole modification layer, an active light-emitting layer, an electron transport layer, an electrode modification layer and an electrode in sequence; or comprises a conductive substrate, an electron transport layer, a hole modification layer, an active light-emitting layer, a hole transport layer, an electrode modification layer and an electrode in sequence; the material of the active light-emitting layer is the perovskite composite thin film material.
9. The method for preparing a perovskite light-emitting diode device according to claim 8, characterized in that: The steps include: (1) forming a hole transport layer on the surface of a conductive substrate; (2) forming a hole modification layer on the surface of the hole transport layer; (3) forming an active light-emitting layer on the surface of the hole modification layer; (4) sequentially forming an electron transport layer, an electrode modification layer and an electrode on the surface of the active light-emitting layer to obtain the perovskite light-emitting diode device; or, (1) forming an electron transport layer on the surface of a conductive substrate; (2) forming a hole modification layer on the surface of the electron transport layer; (3) forming an active light-emitting layer on the surface of the hole modification layer; (4) forming a hole transport layer, an electrode modification layer and an electrode in sequence on the surface of the active light-emitting layer to obtain the perovskite light-emitting diode device.
10. Use of the perovskite light-emitting diode device according to claim 7 or 8 in the preparation of display screens, lighting equipment, and solar cells.