Use of bismuth subcarbonate particles for filtering ultraviolet radiation

By using bismuth oxycarbonate particles of specific size and structure to filter UVB and UVA rays in cosmetics, the problem of skin whitening and roughness caused by existing mineral UV shielding agents is solved, and an efficient and comfortable sunscreen effect is achieved.

CN118748933APending Publication Date: 2024-10-08LOREAL SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280089649.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-12-19
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing mineral UV screeners can cause whitening, roughness and dryness when used on the skin, and cannot effectively filter UVB rays, limiting their application in sunscreen products.

Method used

Bismuth oxycarbonate particles (BiO)2-x(CO3) with specific size and structure are used, where -0.4

Benefits of technology

It achieves effective filtering of UVB and UVA rays, provides high transparency and good cosmetic properties, avoids skin whitening and roughness, and meets consumers' needs for efficient and comfortable sun protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004955140580000351
    Figure BDA0004955140580000351
  • Figure BDA0004955140580000371
    Figure BDA0004955140580000371
  • Figure BDA0004955140580000381
    Figure BDA0004955140580000381
Patent Text Reader

Abstract

The invention relates to the use of bismuth oxycarbonate particles of the empirical formula (BiO) 2-x (CO3), wherein-0.4 lt; xlt; 0.6, the maximum average size of the particles being less than 400 nm. The invention also relates to a composition comprising: i) bismuthyl carbonate particles as defined above, ii) at least one aqueous phase and / or at least one fatty phase, and iii) at least one compound selected from the group consisting of: a) a UV screening agent other than the bismuthyl carbonate particles i), b) a colorant, c) a cosmetic active agent for caring for keratinous materials, d) a surfactant, e) a thickener, and mixtures thereof. Finally, the present invention also relates to a method of filtering UV radiation comprising applying to a keratinous material at least a cosmetic composition comprising bismuth subcarbonate particles as defined above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sun protection, and more particularly to the use of specific bismuth oxycarbonate particles for filtering ultraviolet radiation.

[0002] Another subject of the present invention is a composition, in particular a cosmetic composition, comprising, inter alia, specific bismuth oxycarbonate particles.

[0003] Keratin material is exposed to sunlight every day.

[0004] It is well known that light radiation with a wavelength between 280 and 400 nm can cause a tan in the human epidermis. However, rays with a wavelength between 280 and 320 nm (called UVB rays) are detrimental to natural tanning. Such exposure may also lead to impairment of the biomechanical properties of the epidermis, which is reflected in the appearance of wrinkles, thus causing premature aging of the skin.

[0005] It is also known that UVA rays, with a wavelength between 320-400nm, penetrate the skin more deeply than UVB rays. UVA rays promote rapid and lasting pigmentation of the skin. Under normal circumstances, daily exposure to UVA radiation, even for a short period of time, causes damage to collagen fibers and elastin, which is reflected in changes in skin micro-lines, the appearance of wrinkles and uneven pigmentation (i.e. age spots, uneven skin tone, etc.).

[0006] Additionally, prolonged exposure to the sun can dry out your hair, making it brittle.

[0007] Therefore, protecting keratinous materials, especially human keratinous materials such as skin, is of vital importance. Prior art

[0008] In order to counteract these adverse effects, it is common practice to formulate organic and / or inorganic anti-UVA and / or anti-UVB screening agents in compositions intended to provide sun protection.

[0009] Many photoprotective cosmetic compositions for the skin have been proposed so far. They usually contain organic UV screening agents and / or inorganic UV screening agents, which act according to their own chemical properties and according to their own physical properties by absorbing, reflecting or scattering UV radiation. They usually contain a combination of oil-soluble organic UV screening agents and / or water-soluble organic UV screening agents combined with metal oxide pigments, such as titanium dioxide (TiO2) or zinc oxide (ZnO).

[0010] For conventional organic screening agents, they must have acceptable cosmetic properties, good solubility in conventional solvents (especially oils), and good light stability (used alone or in combination). They must also be colorless or have a color that is cosmetically acceptable to the consumer. These organic screening agents are often used in the form of mixtures, and such combinations of screening agents can limit the formulation range.

[0011] Furthermore, photoprotection with inorganic UV screeners is now a very important expectation of consumers, as they perceive mineral sunscreens as safer.

[0012] TiO2 and ZnO are the most commonly used mineral UV screeners.

[0013] However, one of the major disadvantages of such mineral sunscreens is that once applied to the skin, they produce a skin whitening effect which is cosmetically undesirable and not usually particularly preferred by the user.

[0014] This effect is more pronounced when the concentration of mineral screeners in the composition is high, which limits their concentration in sunscreen formulations.

[0015] To avoid this problem, it is of course possible to reduce the amount of inorganic screening agent used, but the resulting composition, while certainly giving a film of acceptable transparency on the skin, no longer provides adequate protection in the UV range, which greatly limits the benefit of this option.

[0016] Furthermore, in addition to a noticeable whitening, the high use of these UV screeners results in an unpleasant sensation after application to the skin, particularly in cases where these products are used in large quantities and regularly, resulting in a feeling of roughness and dryness of the skin.

[0017] Consumers are increasingly seeking products that are effective yet easy to apply, provide comfort for longer periods of time and have pleasing sensory properties.

[0018] Public Content

[0019] Therefore, there is still a need for inorganic UV screening agents (sunscreens) which provide effective light protection and do not have the above-mentioned disadvantages.

[0020] In particular, there remains a need for inorganic UV screening agents that are able to effectively block UV rays, in particular the UVA and UVB ranges, especially UVB rays, have high transparency in visible light, do not whiten the keratinous material to which they are applied, and have good cosmetic properties.

[0021] There is a particular need for mineral UV screeners other than titanium dioxide or zinc oxide that would prove to be equally effective, be transparent, not cause a harsh and dry feel to the skin, and be easy to formulate, especially at high concentrations.

[0022] The object of the present invention is in particular to propose novel mineral UV screening agents which can meet these expectations. Summary of the invention

[0024] Thus, according to its first aspect, the present invention relates to the use of bismuth oxycarbonate particles having the empirical formula (BiO) 2-x (CO3) for filtering ultraviolet radiation, where -0.4 < x < 0.6, and the maximum average size of said particles is less than 400 nm.

[0025] Preferably, the maximum average size of said particles is less than or equal to 300 nm.

[0026] Preferably, the bismuth oxycarbonate particles are crystalline.

[0027] According to a preferred embodiment, the present invention relates to the use of said particles for filtering UVB radiation.

[0028] Surprisingly and as will be apparent from the following examples, the inventors have found that bismuth oxycarbonate particles having a specific size as required by the present invention have excellent efficacy in filtering ultraviolet radiation, in particular UVB rays, and high transparency in the visible light range, and enable the compositions containing them to provide satisfactory cosmetic properties for consumers.

[0029] For the purposes of the present invention, "high transparency in the visible light range" means that the particles have a high transmittance for rays between 400 - 780 nm.

[0030] For the purposes of the present invention, "efficacy in filtering ultraviolet radiation" means that the threshold absorbance of the particles in the UV range in a dispersion medium containing said particles is greater than 0.5, preferably greater than or equal to 1.0, and more preferably greater than or equal to 1.5. The higher the threshold absorbance, the higher the efficacy in filtering UV radiation.

[0031] UVB radiation means radiation in the wavelength range 280 - 320 nm. UVA radiation means radiation in the wavelength range 320 - 400 nm. Visible light means radiation in the wavelength range 400 - 780 nm.

[0032] Thus, for the purposes of the present invention, a "UV screening agent (sunscreen)" is intended to denote any compound that filters ultraviolet (UV) radiation in the wavelength range 280 - 400 nm. A "UVB screening agent" is intended to denote any compound that filters ultraviolet (UV) radiation in the wavelength range 280 - 320 nm. A "UVA screening agent" is intended to denote any compound that filters ultraviolet (UV) radiation in the wavelength range 320 - 400 nm.

[0033] To the best knowledge of the inventors, this efficacy of bismuth subcarbonate particles, especially crystalline bismuth subcarbonate particles, has been characterized for the first time. No one has ever proposed using bismuth subcarbonate particles in a cosmetic composition to effectively filter UV radiation, especially UVB radiation.

[0034] The bismuth subcarbonate particles required according to the invention are especially used for protecting horny materials, especially the skin and hair, from UV radiation, especially in cosmetic compositions for sun protection, hair care or treatment, and the makeup field.

[0035] Thus, according to another aspect, the invention also relates to a non-therapeutic cosmetic method for filtering UV radiation, especially UVB radiation, which comprises applying at least a composition comprising bismuth subcarbonate particles as defined above to horny materials.

[0036] "Horny materials" especially means the skin (including the scalp), lips, and keratin fibers, such as hair, eyelashes, eyebrows, especially the skin and / or hair, and preferably the skin.

[0037] According to another aspect thereof, the invention also relates to a composition, especially a cosmetic composition, which at least comprises:

[0038] i) Bismuth subcarbonate particles having the empirical formula (BiO) 2-x (CO3), where -0.4 < x < 0.6, and the maximum average size of said particles is less than 400 nm;

[0039] ii) at least one aqueous phase and / or at least one fatty phase; and

[0040] iii) at least one compound selected from the following: a) a UV screening agent other than the bismuth subcarbonate particles i), b) a colorant, c) a cosmetic active agent for caring for horny materials, d) a surfactant, e) a thickener, and mixtures thereof.

[0041] The term "at least one (at least a kind of)" is equivalent to "one or more (one kind or more kinds)".

[0042] The expressions "between... -...", "comprising... - (to)...", "... - (to)... form", and "the range is... - (to)..." should be understood as including these limitations (end values), unless otherwise specified.

[0043] After reading the following description and examples, other features, variations, and advantages of the composition of the invention will become more clearly apparent. Detailed Description of the Invention

[0045] The invention relates to the use of bismuth subcarbonate particles of formula (I) as a reagent for filtering ultraviolet radiation, especially UVB radiation.

[0046] Bismuth oxycarbonate particles

[0047] As described above, the bismuth oxycarbonate particles of the present invention have the empirical formula (BiO) 2-x (CO3), where -0.4 < x < 0.6. The value of x can be determined in particular by elemental analysis.

[0048] Preferably, x is equal to 0, and the empirical formula of the bismuth oxycarbonate particles is (BiO)2(CO3).

[0049] The bismuth oxycarbonate particles of the present invention can be crystalline or amorphous.

[0050] According to one embodiment of the present invention, the bismuth oxycarbonate particles are amorphous.

[0051] According to a preferred embodiment of the present invention, the bismuth oxycarbonate particles are crystalline.

[0052] It should be understood that the bismuth oxycarbonate particles can consist of a mixture of several bismuth oxycarbonate particles having different empirical formulas and / or different shapes.

[0053] Thus, the bismuth oxycarbonate particles can be a mixture of amorphous particles and crystalline particles.

[0054] For the purposes of the present invention, "crystalline" means an ordered arrangement of atoms forming the bismuth oxycarbonate particles. In other words, crystalline bismuth oxycarbonate particles are organized materials.

[0055] In contrast, "amorphous" particles are particles in which the atoms are disordered. The atoms of such particles do not exhibit any organization at the microscopic level.

[0056] Preferably, the crystalline particles required according to the present invention have the crystal phase of bismutite, called layered, and it has alternating [Bi2O2] 2+ and [CO3] 2- layers.

[0057] Such particles crystallize in the orthorhombic system with the space group Imm2.

[0058] The bismutite crystal structure of bismuth oxycarbonate can have the following lattice parameters: and V 晶格 = 0.204 nm 3 . This particular atomic arrangement can in particular enable the growth of anisotropic objects.

[0059] When the elongation coefficient R between the length L of the particles and the thickness e of the particles (i.e., R = L / e) is greater than 2, the particles are considered "anisotropic".

[0060] Particle size

[0061] According to the present invention, the empirical formula (BiO) 2-x The maximum average size of the crystalline or amorphous (preferably crystalline) bismuth carbonate particles of (CO3) is less than 400 nm, wherein -0.4 <x<0.6。

[0062] Preferably, the maximum average dimension of the particles is less than or equal to 300 nm.

[0063] "Average size" is intended to represent the number average of particle size. Particle size can be determined by transmission electron microscopy, for example, using a Hitachi HT 7700 microscope, especially at an accelerating voltage of 100 kV, by scanning electron microscopy or by BET method to measure specific surface area, or using a laser particle size analyzer. Number average can be calculated by analyzing the image obtained using software (such as ImageJ software) (C Schneider, WS Rasband, KW Eliceiri, NIH Image to ImageJ: 25 years of image analysis, Nat. Methods. 9 (2012) 671–675).

[0064] The average dimension is selected from the group consisting of average length L, average width l, average thickness e or average diameter d.

[0065] The "largest average dimension" of a particle is intended to mean the largest average dimension of a surface (eg, a face) that can be measured between two diametrically opposed points on a single particle.

[0066] The "length" L of a particle is the largest dimension of the particle observable in an image taken perpendicular to the plane in which the particle lies.

[0067] The "width" l and "thickness" e of a particle are the lengths of the major and minor axes, respectively, of the smallest possible ellipse that can inscribe the median cross-sectional area of ​​the particle.

[0068] The "diameter" d of a particle is the largest dimension observable along a line through the center of a circle or sphere.

[0069] Granular form

[0070] According to the present invention, the empirical formula (BiO) 2-x The bismuth carbonate particles of (CO3) may have any form, wherein -0.4 <x<0.6。

[0071] The form of the particles will depend inter alia on the method by which they are prepared and on the operating conditions.

[0072] Specifically, the particles of the present invention may be in the form of tubes, flakes, sheets, rods, balls, flowers, pompoms, threads, filaments, fibers, needles, cubes, or any mixture thereof.

[0073] The particles according to the invention can also be aggregated in the form of superstructures. For example, flakes, tubes and / or rods can be aggregated in the form of balls, flowers or pompoms.

[0074] According to a preferred embodiment, the particles of the invention are in the form of tubes, flakes and / or rods. Even more preferably, the particles of the invention are in the form of flakes and / or rods.

[0075] Thus, particles in the form of flakes or rods or tubes differ in particular from particles in the form of spheres or fibers or in the form of flowers, pompoms, threads, filaments, needles or cubes.

[0076] Of course, the particles of the present invention can be used in the form of a mixture. Specifically, the particles of the present invention can be used in the form of a mixture of flakes and / or rods and / or tubes in any ratio.

[0077] According to a preferred embodiment, the particles employed in the invention are predominantly or exclusively in the form of flakes.

[0078] Particles in the form of "flakes" have a length greater than their width, and a width greater than their thickness.

[0079] In particular, when they are in the form of flakes, the particles of the invention have:

[0080] - an average length L of 15-300 nm, in particular 30-250 nm, preferably 50-200 nm, more preferably 70-150 nm;

[0081] - an average width l of 10-250 nm, in particular 20-200 nm, preferably 30-150 nm, more preferably 50-120 nm;

[0082] - an average thickness e of 2-120 nm, in particular 5-100 nm, preferably 10-80 nm, more preferably 20-50 nm; and

[0083] -e <l<L。

[0084] According to a preferred embodiment, the particles employed in the invention are predominantly or exclusively in the form of rods.

[0085] Particles in the form of "rods" have the form of a solid cylinder whose length L is greater than its diameter d, or have the form of a prism whose base is a solid polygon, preferably a triangle or hexagon, and the diameter d of the circle contained in the polygonal base is less than the length L of the prism.

[0086] Specifically, when they are in rod form, whether cylindrical or prismatic, the particles of the invention have:

[0087] - an average length L of 30-300 nm, in particular 50-250 nm, preferably 70-230 nm, more preferably 70-140 nm;

[0088] - an average diameter d of 15-150 nm, in particular 20-130 nm, preferably 25-120 nm, more preferably 25-100 nm, and even more preferably 25-60 nm, and

[0089] -where L>d.

[0090] According to a preferred embodiment, the particles employed in the invention are predominantly or exclusively in the form of tubes.

[0091] Particles in the form of "tubes" have the form of a hollow cylinder and their length L is greater than their diameter d.

[0092] In particular, when they are in the form of tubes, the particles of the invention have:

[0093] - an average length L of 10-300 nm, in particular 20-250 nm, preferably 40-200 nm, more preferably 60-200 nm;

[0094] - an average diameter d of 2 to 30 nm, in particular 3 to 20 nm, and preferably 5 to 15 nm; and

[0095] -where L>d.

[0096] For the purposes of the present invention, "predominantly in the form of flakes / rods / tubes" is intended to mean that at least 50% by number, in particular at least 70% by number, or even at least 90% by number of the particles are in the form of flakes / rods / tubes, respectively.

[0097] Particle doping

[0098] According to a particular embodiment, the bismuth oxycarbonate particles of the invention may be doped.

[0099] In particular, the bismuth oxycarbonate particles of the present invention may be doped with one or more chemical elements capable of being inserted into the structure or partially replacing already existing elements.

[0100] The particles are doped by replacing all or part of the cations and / or all or part of the anions.

[0101] According to one particular embodiment, the doping portion concerns inserted cations or cations as substitutes for bismuth, involving a limit of 20% of the composition calculated on a bismuth basis.

[0102] According to this variant, the degree of doping is especially between 0.005 and 15%, preferably between 0.05 and 12%, more preferably between 0.1 and 10% and even more preferably between 0.5 and 6%.

[0103] In particular, the particles of the present invention may be doped with cations derived from elements selected from the group consisting of aluminum (Al), silicon (Si), scandium (Sc), titanium (Ti), vanadium (V), manganese (Mn), iron (Fe), copper (Cu), zinc (Zn), gallium (Ga), germanium (Ge), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), silver (Ag), indium (In), lanthanum (La), cerium (Ce), tantalum (Ta), tungsten (W) and / or gold (Au).

[0104] Preferably, the particles of the invention may be doped with cations derived from elements selected from titanium, vanadium, manganese, iron, copper, zinc, lanthanum and / or cerium, more preferably manganese, iron and / or cerium, and even more preferably manganese or iron.

[0105] According to a variant embodiment, the particles according to the invention are doped with cations derived from manganese, and the degree of doping is especially between 0.5 and 2%.

[0106] According to another variant embodiment, the particles according to the invention are doped with cations derived from iron, and the degree of doping is especially between 0.5 and 2%.

[0107] According to another particular embodiment, the doping involves partly or completely the insertion of anions or anions as substitutes for carbonate, involving a limit of 20% of the composition calculated as carbonate.

[0108] According to this variant, the degree of doping is especially 0.001-1%, preferably 0.002-0.5%, more preferably 0.003-0.2% and even more preferably 0.005-0.1%.

[0109] In particular, the particles of the invention may be doped with anions derived from the group consisting of fluorine (F), sulfur (S), chlorine (Cl), bromine (Br), iodine (I), and / or with polyatomic anions, in particular sulfate ions (SO4 2- ), sulfonate ion (S(=O)2-O - ), sulfite ion (SO3 2- ), phosphate ion (PO4 3- ) and / or iodate ions (IO3 - ).

[0110] Preferably, the particles of the present invention may be doped with S 2- 、SO3 2- 、SO4 2- , Cl - and / or -, more preferably doped with SO3 2- 、SO4 2- and / or Cl - , and more preferably doped with Cl - or SO4 2- .

[0111] According to a variant embodiment, the particles according to the invention are doped with anions derived from chloride, and the degree of doping is especially between 0.01 and 0.1%.

[0112] According to another variant embodiment, the particles according to the invention are doped with anions derived from iodine, and in particular the degree of doping is between 0.003 and 0.01%.

[0113] According to another variant embodiment, the particles according to the invention are doped with sulfate ions, especially in an amount of 0.005-0.1%.

[0114] According to another variant embodiment, the particles according to the invention are doped with cations, preferably cations from the group consisting of titanium, vanadium, manganese, iron, copper, zinc, lanthanum and / or cerium, more preferably manganese, iron and / or cerium, and even more preferably manganese or iron, and with anions, preferably anions from the group consisting of fluorine (F), sulfur (S), chlorine (Cl), bromine (Br), iodine (I), and / or with polyatomic anions, in particular sulfate ions (SO4 2- ), sulfonate ion (S(=O)2-O - ), sulfite ion (SO3 2- ), phosphate ion (PO4 3- ) and / or iodate ions (IO3 - ), more preferably doped with S 2- 、SO3 2- 、SO4 2- , Cl - and / or - , even more preferably doped with SO3 2- 、SO4 2- and / or Cl - , and particularly preferably doped with Cl - ,I - or SO4 2- .

[0115] According to a preferred embodiment, the bismuth oxycarbonate particles required according to the invention are undoped.

[0116] According to a further preferred embodiment, the bismuth oxycarbonate particles required according to the invention are doped.

[0117] According to a further preferred embodiment, the bismuth oxycarbonate particles required according to the invention are a mixture of doped particles and undoped particles.

[0118] Method for preparing particles

[0119] The bismuth oxycarbonate particles of the present invention can be obtained by any preparation method known to those skilled in the art.

[0120] For example, the synthesis of the bismuth oxycarbonate particles of the present invention is described in an article by Ni et al. (Fabrication, Modification and application of (BiO)2CO3-based photocatalysts: A review, Applied Surface Science, 365, 2016, 314-335).

[0121] Specifically, the particles of the present invention may be prepared by a solvothermal route, an electrochemical route, coprecipitation or under reflux, and are preferably prepared by a solvothermal route or under reflux.

[0122] According to a first variant embodiment, the particles of the invention are obtained by a solvothermal route, in particular from bismuth nitrate and various carbonizing agents (such as sodium carbonate, ammonium carbonate or urea) in polar protic solvents in the presence of polyols. This synthesis makes it possible to obtain bismuth oxycarbonate particles in the form of flakes and / or rods, the maximum dimension of which is 50-300 nm.

[0123] The following articles describe, inter alia, the synthesis of the particles by a solvent route: Cheng, G et al. (Shape-controlled solvothermal synthesis of bismuth subcarbonate nanomaterials, J. Solid State Chem. 183, 1878–1883 ​​(2010)), Ruan, MM et al. (Facile Green Synthesis of Highly Monodisperse Bismuth Subcarbonate Micropompons Self-assembled by Nanosheets: Improved Photocatalytic Performance, Acta Physico-Chimica Sinica, 33, 2017, 1033-1042), Quin et al. (Template-Free Fabrication of Bi2O3 and (BiO)2CO3 Nanotubes and Their Application in Water Treatment, Chem. Eur. J., 18, 2012, 16491–16497), Cheng, G et al. (Shape-controlled solvothermal synthesis of bismuth subcarbonate nanomaterials, J. Solid State Chem., 183, 2010, 1878–1883), Liu, YY et al. (Preparation, electronic structure, and photocatalytic properties of Bi2O2CO3nanosheet, Appl.Surf.Sci., 257, 2010, 172–175), Zheng et al (Synthetic Bi2O2CO3nanostructures: Novel photocatalyst with controlled special surface exposed, Journal of Molecular Catalysis A: Chemical, 2010, 317 (1-2), 34-40), Liu, SQ et al (The effects of citrate ion on morphology and photocatalytic activity of flower-like Bi2O2CO3, Ceram. Int., 40, 2014, 2343–2348) or Chen, R et al. (Bismuth subcarbonatenanparticles fabricated by water-in-oil microemulsion-assisted hydrothermal process exhibit anti-Helicobacter pylori properties, Mater. Res. Bull., 45, 2010, 654–658). .

[0124] The article by Hu, Y et al. (Simple hydrolysis route to synthesize Bi2O2CO3nanoplate from Bi nanopowder and its photocatalytic application, Materials Letters, 170, 2016, 72–75) describes, inter alia, the synthesis of the particles via an electrochemical route.

[0125] Chen, XY et al. (Controlled synthesis of bismuth oxo nanoscale crystals (BiOCl,Bi 12 O 17 The article (Cl2, α-Bi2O3, and (BiO)2CO3) by solution-phase methods, J. Solid State Chem., 180, 2007, 2510–2516) describes, inter alia, the synthesis of such particles by coprecipitation.

[0126] The article by Chen et al. (Fabrication of bismuth subcarbonate nanotube arrays from bismuth citrate, Chem. Commun., 2006, 2265-2267) describes, inter alia, the synthesis of such particles by reflux.

[0127] According to a preferred embodiment, the bismuth oxycarbonate particles required according to the invention are obtained by a solvothermal route (for example according to the method described by Cheng et al.) or under reflux (for example according to the method described by Chen et al.).

[0128] According to a preferred embodiment, the bismuth oxycarbonate particles required according to the present invention are obtained by a preparation process using one or more bismuth (III) complexes, one or more carbonating agents, one or more polyols and optionally one or more polar solvents other than polyols.

[0129] When the particles used according to the invention are doped, one or more additional reagents comprising the doping element may be added.

[0130] Specifically, the bismuth (III) complex is selected from bismuth nitrate and hydrated forms thereof, bismuth citrate and hydrated forms thereof, bismuth sulfate and hydrated forms thereof, and bismuth chloride and hydrated forms thereof.

[0131] The bismuth(III) complexes can also be obtained from bismuth minerals, for example elemental bismuth and / or bismuth oxide and / or bismuth sulfide.

[0132] Preferably, the bismuth (III) complex is bismuth (III) nitrate and its hydrated form with the chemical formula Bi(NO3)3·xH2O, preferably bismuth nitrate pentahydrate with the chemical formula Bi(NO3)3·5H2O.

[0133] In particular, the carbonating agent is selected from Li2CO3, Na2CO3, K2CO3, Rb2CO3, Cs2CO3, (NH4)2CO3, LiHCO3, NaHCO3, KHCO3, RbHCO3, CsHCO3, (NH4)HCO3, urea (NH2)2CO and urea derivatives, CO2, preferably selected from Na2CO3, K2CO3, (NH2)2CO, (NH4)2CO3, and more preferably selected from (NH2)2CO and / or (NH4)2CO3.

[0134] Polyols are compounds with multiple hydroxyl functions. They can be chosen in particular from diols, in particular ethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol; short-chain or long-chain diol polymers, for example polyethylene glycol, polypropylene glycol, polybutylene glycol; glycerol and its derivatives; or for example sugars, in particular glucose, fructose, sucrose, xylitol, mannitols such as D-mannitol, sorbitol or maltitol.

[0135] According to one embodiment, the bismuth oxycarbonate particles required according to the present invention are obtained by a preparation method using a polyol or a polyol mixture.

[0136] According to a first variant embodiment, polyols may also be used as solvent.The particles of the invention may then be obtained, for example, according to the process described below.

[0137] Solution A is formed by dissolving a bismuth (III) complex (preferably at a concentration of 0.001-0.5 M) in a polyol or a polyol mixture. Solution B is formed by partially or completely dissolving a carbonating agent (preferably 1-100 equivalents relative to bismuth) in a polyol or a polyol mixture or a polyol or a polyol mixture different from the polyol or polyol mixture used in solution A.

[0138] In the case of doping with cations, the dopant is preferably added to solution A. In the case of doping with anions, the dopant is preferably added to solution B.

[0139] In the case of doping with one or more cations and / or one or more anions, the cationic dopant is preferably added to solution A and the anionic dopant is preferably added to solution B. Solution A is subsequently added at ambient temperature to solution B. If the polyol or polyol mixture is not liquid at ambient temperature, all solids are mixed.

[0140] The resulting mixture was subsequently heated at 90-250° C. for a reaction time of 10 minutes and 48 hours. If the desired reaction temperature is greater than or equal to the boiling point of the solvent, an autoclave is used for the solvothermal synthesis.

[0141] Preferably, the reaction temperature is 95-200° C., and the reaction time is 1-24 hours, and more preferably the reaction temperature is 100-180° C., and the reaction time is 2-16 hours.

[0142] The resulting particles are separated from the reaction medium by centrifugation and washed by successive cycles of dispersion and centrifugation.

[0143] After drying in vacuo at 40-60°C, a white powder was obtained.

[0144] In the case of using polyols as solvent, the bismuth oxycarbonate particles obtained according to the invention are in the form of flakes, preferably with an average thickness e of 2 to 15 nm, and / or in the form of tubes.

[0145] According to another variant embodiment, the polyol is used only as an additive and not as a solvent.The particles of the invention can then be obtained, for example, according to the process described below.

[0146] Solution A is formed by dissolving a bismuth complex (preferably at a concentration of 0.001-0.5 M) and a polyol (preferably at a total polyol concentration of 0.01-5 M) in a solvent (preferably a polar solvent). Solution B is formed by partially or completely dissolving a carbonating agent (1-100 equivalents relative to the bismuth complex) in a polar solvent (miscible with the solvent in A), and the polar solvent is the same as or different from the solvent in solution A, preferably the same.

[0147] In the case of doping with cations, the dopant is preferably added to solution A. In the case of doping with anions, the dopant is preferably added to solution B.

[0148] In the case of doping with one or more cations and / or one or more anions, the cationic dopant is preferably added to solution A, and the anionic dopant is preferably added to solution B.

[0149] Solution A is then added to solution B at ambient temperature. The resulting mixture is then heated at 90-250°C for 10 minutes to 48 hours. If the desired reaction temperature is greater than or equal to the boiling point of the solvent, an autoclave is used for the solvothermal synthesis.

[0150] Preferably, the reaction temperature is 90-150° C. and the reaction time is 4-16 hours.

[0151] The resulting particles are separated from the reaction medium by centrifugation and washed by successive cycles of dispersion and centrifugation.

[0152] After drying in vacuo at 40-60°C, a white powder was obtained.

[0153] When polyols are used only as additives, they may be selected in particular from ethylene glycol, propylene glycol, glycerol and / or sugars, preferably sugars, more preferably D-mannitol.

[0154] According to this variant, the synthesis process employs a solvent other than a polyol, or a solvent mixture other than a polyol. In particular, the solvent or solvent mixture is chosen from polar solvents, preferably polar and protic solvents, such as water, C1-C6 alcohols such as ethanol or isopropanol, and mixtures thereof, and the solvent is even more preferably water.

[0155] In particular, when only polyol is selected as the additive and water as the solvent, the bismuth oxycarbonate particles of the present invention are preferably obtained in the form of flakes and / or rods.

[0156] Cosmetic composition

[0157] The bismuth oxycarbonate particles of the invention can be used in particular in compositions, especially cosmetic compositions.

[0158] Therefore, the present invention also relates to a composition, in particular a cosmetic composition, comprising at least:

[0159] i) particles of bismuth oxycarbonate as defined above,

[0160] ii) at least one aqueous phase and / or at least one fatty phase, and

[0161] iii) at least one compound selected from a) UV screening agents other than the bismuth oxycarbonate particles i), b) colorants, c) cosmetic active agents for caring for keratinous materials, d) surfactants, e) thickeners, and mixtures thereof.

[0162] The bismuth oxycarbonate particles may be present in the composition, preferably the cosmetic composition, in an amount of 0.5-40 wt %, preferably 1-30 wt %, still better 2-20 wt % relative to the total weight of the composition.

[0163] Water Phase

[0164] The compositions, especially cosmetic compositions, according to the invention may comprise at least one aqueous phase.

[0165] The aqueous phase may comprise water and optionally a water-soluble solvent.

[0166] In the present invention, the term "water-soluble solvent" means a compound that is liquid at ambient temperature and miscible with water (miscibility in water greater than 50% by weight at 25°C and atmospheric pressure).

[0167] The water-soluble solvents useful in the compositions of the present invention may also be volatile.

[0168] Among the water-soluble solvents that can be used in the composition of the present invention, mention may be made in particular of lower monohydric alcohols having 1 to 5 carbon atoms (e.g. ethanol and isopropanol), C2-C 32 Polyols, C3 and C4 ketones and C2-C4 aldehydes.

[0169] For the purposes of the present invention, "polyol" means any organic molecule containing at least two free hydroxyl groups.

[0170] The polyols suitable for the present invention may be saturated or unsaturated, linear, branched or cyclic alkyl type compounds carrying at least two -OH functional groups, in particular at least three -OH functional groups, more particularly at least four -OH functional groups in the alkyl chain.

[0171] Polyols which are advantageous for formulating the compositions of the invention are those which contain notably from 2 to 32 carbon atoms, preferably from 3 to 16 carbon atoms.

[0172] Advantageously, the polyol may, for example, be chosen from pentaerythritol, trimethylolpropane, caprylyl glycol, glycerol, polyglycerols (eg glycerol oligomers, such as diglycerol), polyethylene glycols, and mixtures thereof.

[0173] In particular, the composition of the invention may comprise 5 to 80 wt %, preferably 20 to 60 wt % of aqueous phase relative to the total weight of the composition.

[0174] Fat phase

[0175] The composition, especially the cosmetic composition, according to the invention may also comprise at least one fatty phase, especially an oily phase.

[0176] For the purposes of the present invention, “fatty phase” means the phase comprising at least one fatty substance and all the fat-soluble and lipophilic ingredients used to formulate the composition according to the invention.

[0177] Preferably, the fatty phase comprises at least one oil, especially a cosmetic oil.

[0178] The term "oil" means a water-immiscible, non-aqueous compound that is liquid at room temperature (25°C) and atmospheric pressure (760 mmHg).

[0179] The fatty phase may comprise at least one volatile or nonvolatile hydrocarbon-based oil and / or fatty substance, preferably a volatile and / or nonvolatile silicone oil and / or a volatile or nonvolatile fluorinated oil.

[0180] As nonvolatile hydrocarbon-based oils, mention may be made especially of hydrocarbon-based oils of vegetable origin, synthetic ethers having 10 to 40 carbon atoms, linear or branched hydrocarbons of mineral or synthetic origin, synthetic esters, fatty alcohols which are liquid at room temperature and have a branched and / or unsaturated carbon chain having 12 to 26 carbon atoms, C 12 -C 22 Higher fatty acids, carbonates, and mixtures thereof.

[0181] As volatile hydrocarbon-based oils, mention may especially be made of hydrocarbon-based oils having 8 to 16 carbon atoms.

[0182] The non-volatile silicone oils may especially be chosen from non-volatile polydimethylsiloxanes (PDMS) and phenylated silicone oils. As volatile silicone oils, mention may be made, for example, of volatile linear or cyclic silicone oils.

[0183] Volatile fluorinated oils such as nonafluoromethoxybutane, decafluoropentane, tetradecafluorohexane, dodecafluoropentane, and mixtures thereof may also be used.

[0184] The oil phase may also contain other fatty substances mixed with the oil or dissolved in the oil. Other fatty substances that may be present in the oil phase may be, for example, fatty acids, waxes, gums, pasty compounds or mixtures thereof.

[0185] a) UV screening agent

[0186] According to one particular embodiment, the composition of the invention comprises a) at least one UV screening agent other than the bismuth oxycarbonate particles required for the invention and defined above.

[0187] For the purposes of the present invention, "UV screening agent other than bismuth oxycarbonate particles" is intended to mean any UV screening agent, the chemical nature of which differs from the bismuth oxycarbonate particles required by the present invention and defined above.

[0188] Therefore, the bismuth oxycarbonate particles of the present invention can be used alone or in combination with a) other UV screening agents (particularly selected from organic and / or inorganic UV screening agents).

[0189] Therefore, the cosmetic composition may also contain one or more additional UV screening agents selected from hydrophilic, lipophilic or insoluble organic UV screening agents and / or mineral UV screening agents.

[0190] By "hydrophilic UV screening agent" is meant any cosmetic or dermatological organic or inorganic compound for filtering UV radiation, which can be completely dissolved in molecular form in a liquid aqueous phase or can be present in the liquid aqueous phase in a colloidal suspension, for example in the form of micelles.

[0191] “Lipophilic UV screening agent” is understood to mean any cosmetic or dermatological organic or inorganic compound for filtering UV radiation which can be completely dissolved in molecular form in the liquid fatty phase or can be present in the liquid fatty phase in a colloidal suspension, for example in the form of micelles.

[0192] By "insoluble UV screening agent" is meant any cosmetic or dermatological organic or inorganic compound used for filtering UV radiation, which has a solubility of less than 0.5 wt % in water and in most organic solvents (e.g. liquid paraffin, fatty alcohol benzoates and fatty acid triglycerides, e.g. Miglyo1 sold by Dynamit Nobel ) has a solubility of less than 0.5 wt %. This solubility, measured at 70° C., is defined as the amount of product dissolved in the solvent in equilibrium with the excess solid in the suspension after returning to ambient temperature. It can be easily assessed in the laboratory.

[0193] Additional organic UV screening agents are chosen especially from:

[0194] - cinnamic acid compounds, especially ethylhexyl methoxycinnamate,

[0195] - anthranilic acid compounds, especially menthyl anthranilate,

[0196] - salicylic acid compounds, especially homosalate and ethylhexyl salicylate,

[0197] - dibenzoylmethane compounds, especially butyl methoxydibenzoylmethane,

[0198] - benzyl camphor compounds, in particular 3-benzylidene camphor, 4-methylbenzylidene camphor, benzyl camphor sulfonic acid and terephthalylidene dicamphor sulfonic acid,

[0199] - benzophenone compounds, in particular oxybenzone and n-hexyl 2-(4-diethylamino-2-hydroxybenzoyl)benzoate,

[0200] -β,β-diphenylacrylate compounds, especially octocrylene,

[0201] - triazine compounds, in particular phenylene bis-diphenyl triazine, bis-ethylhexyloxyphenol methoxyphenyl triazine, ethylhexyl triazone and diethylhexyl butyramide triazone.

[0202] - benzotriazole compounds, especially drometrizole trisiloxane,

[0203] - benzalmalonate compounds, especially those mentioned in US Pat. No. 5,624,663, especially polysilicone-15,

[0204] - benzimidazole derivatives, especially phenylbenzimidazole sulfonic acid,

[0205] - imidazoline compounds, especially ethylhexyl dimethoxybenzylidene dioxyimidazoline propionate,

[0206] - bisbenzoxazolyl compounds, such as those described in patents EP0669323 and US2463264, especially disodium phenyldibenzimidazole tetrasulfonate,

[0207] - para-aminobenzoic acid compounds, in particular PABA, ethylhexyl dimethyl PABA and PEG-25 PABA,

[0208] - methylenebis(hydroxyphenylbenzotriazole) compounds, such as those described in applications US 5237071, US 5166355, GB 2303549, DE 19726184 and EP 0893119, in particular methylenebis-benzotriazole tetramethylbutylphenol,

[0209] - benzoxazole compounds, such as those described in patent applications EP0832642, EP1027883, EP1300137 and DE10162844, in particular 2,4-bis-[5-1(dimethylpropyl)benzoxazol-2-yl-(4-phenyl)-imino]-6-(2-ethylhexyl)-imino-1,3,5-triazine,

[0210] - polymeric and silicone screening agents, such as those described in particular in application WO 93 / 04665,

[0211] - dimers derived from α-alkylstyrenes, such as those described in patent application DE 19855649,

[0212] -4,4-diarylbutadiene compounds, such as those described in applications EP0967200, DE 19746654, DE 19755649, EP1008586, EP1133980 and EP0133981, in particular 1,1-dicarboxy(2,2'-dimethylpropyl)-4,4-diphenylbutadiene, and

[0213] - A mixture thereof.

[0214] Inorganic UV screening agents are generally mineral UV screening agents, in particular chosen from metal oxides.

[0215] The metal oxide may especially be chosen from titanium oxide, zinc oxide, iron oxide, zirconium oxide and cerium oxide, and mixtures thereof.

[0216] The metal oxide particles may be coated or uncoated.

[0217] More particularly, the coated particles are titanium oxide particles coated with silica, titanium oxide particles coated with silica and iron oxide, titanium oxide particles coated with silica and alumina, titanium oxide particles coated with alumina, titanium oxide particles coated with alumina and aluminum stearate, titanium oxide particles coated with silica, alumina and alginic acid, titanium oxide particles coated with alumina and aluminum laurate, titanium oxide particles coated with iron oxide and iron stearate, titanium oxide particles coated with zinc oxide and zinc stearate, titanium oxide particles coated with silica and alumina and treated with siloxane, titanium oxide particles coated with silica, titanium oxide particles coated with alumina, titanium oxide particles coated with aluminum stearate and treated with silica. Titanium oxide particles treated with oxane, titanium oxide particles coated with silica and treated with siloxane, titanium oxide particles coated with alumina and treated with siloxane, titanium oxide particles coated with triethanolamine, titanium oxide particles coated with stearic acid, titanium oxide particles coated with sodium hexametaphosphate, or TiO2 treated with octyltrimethylsilane, TiO2 treated with polydimethylsiloxane, anatase / rutile TiO2 treated with polydimethylhydrogensiloxane, TiO2 coated with triethylhexanoic acid, titanium oxide particles coated with aluminum stearate and alumina, TiO2 coated with aluminum stearate, titanium oxide particles coated with alumina and siloxane, TiO2 coated with lauroyl lysine, or TiO2 treated with C 9-15 Fluorophosphate and aluminum hydroxide coated TiO2.

[0218] The metal oxides may optionally be doped.

[0219] In this regard, mention may be made of TiO 2 particles doped with at least one transition metal, such as iron, zinc or manganese, more particularly manganese.

[0220] The doped particles can be in the form of a dispersion, preferably an oily dispersion. The oil present in the oily dispersion is preferably selected from triglycerides, including capric / caprylic triglycerides. The oily dispersion of titanium oxide particles may also contain one or more dispersants, such as sorbitol esters or polyoxyalkylated glycerol fatty acid esters. More specifically, an oily dispersion of TiO2 particles doped with manganese in capric / caprylic triglycerides in the presence of tri-PPG-3 myristyl ether citrate and polyglyceryl-3 polyricinoleate and isostearic sorbate may be mentioned.

[0221] Mention may also be made of mixtures of metal oxides, especially mixtures of titanium dioxide and cerium dioxide coated with silica, including mixtures of equal weights of titanium dioxide and cerium dioxide, and mixtures of titanium dioxide and zinc dioxide coated with alumina, silica and siloxane or with alumina, silica and glycerol.

[0222] b) Colorants

[0223] According to one particular embodiment, the composition of the invention comprises b) at least one colorant.

[0224] In general, "colorant" is intended to mean any compound capable of coloring a composition, ie any compound that absorbs in the visible spectrum and thus appears to the human eye as having a color such as yellow, orange, red, violet, blue or green.

[0225] Preferably, the composition of the present invention comprises at least one pigment.

[0226] "Pigments" are understood to be white or colored mineral or organic particles which are insoluble in the liquid lipophilic and hydrophilic phases and which serve to color and / or opacify the composition containing them. More specifically, the pigments have little or no solubility in aqueous-alcoholic media.

[0227] Pigments that can be used are chosen in particular from the organic and / or mineral pigments known in the art, in particular those described in Kirk-Othmer's Encyclopedia of Chemical Technology and in Ullmann's Encyclopedia of Industrial Chemistry (Ullmann's Encyclopedia of Industrial Chemistry "Pigment organics", 2005 Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim 10.1002 / 14356007.a20 371 and ipso facto "Pigments, Inorganic, 1. General" 2009 Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim 10.1002 / 14356007.a20_243.pub3).

[0228] These pigments may be in the form of pigment powders or pastes. They may be coated or uncoated.

[0229] The pigments may be selected, for example, from mineral pigments, organic pigments, lakes, pigments with special effects (such as mother-of-pearl or glitter flakes), and mixtures thereof.

[0230] The pigment may be a mineral pigment. The term "mineral pigment" refers to any pigment that meets the definition in the chapter on inorganic pigments of Ullmann's Encyclopedia. Among the mineral pigments that can be used in the present invention, mention may be made of iron oxides, chromium oxides, manganese violet, ultramarine, chromium hydrate, ferric blue and titanium oxide.

[0231] The pigment may be an organic pigment.

[0232] The term "organic pigment" refers to any pigment that meets the definition in the chapter on organic pigments of Ullmann's Encyclopedia.

[0233] The organic pigments may in particular be chosen from nitroso, nitro, azo, xanthene, quinoline, anthraquinone, phthalocyanine, metal complex type, isoindolinone, isoindolinone, quinacridone, peronone, perylene, diketopyrrolopyrrole, thioindigo, dioxazine, triphenylmethane or quinophthalone compounds.

[0234] Preferably, the pigment suitable for the present invention is selected from carbon black, iron oxide (especially red, brown or black iron oxide), and mica coated with iron oxide, triarylmethane pigments (especially blue and violet triarylmethane pigments, such as BLUE 1LAKE), azo pigments (especially red azo pigments, such as D&C RED 7), alkali metal salts of Lisol Red (such as calcium salt of Lisol Red B); more preferably, the pigment used is selected from red iron oxide and azo pigments, especially red azo pigments, such as D&C RED 7.

[0235] The colorant may be present in the composition of the present invention in an amount of 0.001-10 wt%, preferably 0.005-5 wt%, relative to the total weight of the composition.

[0236] According to a particular embodiment of the invention, the amount of pigments is between 0.5 and 40%, preferably between 1 and 20%, relative to the weight of the composition according to the invention comprising them.

[0237] c) Cosmetic active agents

[0238] According to one particular embodiment, the composition according to the invention comprises c) at least one cosmetic active agent for caring for keratinous materials, preferably for caring for the skin.

[0239] In particular, the cosmetic active agent may be at least one hydrophilic active agent and / or at least one lipophilic active agent, preferably a hydrophilic active agent.

[0240] "Hydrophilic active agent" refers to a water-soluble or water-dispersible active agent that is capable of forming hydrogen bonds.

[0241] As cosmetic active agents, mention may be made, for example, of moisturizers, depigmenting agents, desquamating agents, humectants, anti-aging agents, mattifying agents, healing agents, antibacterial agents, vitamins and their derivatives or precursors, antioxidants, sunscreens, free radical scavengers, anti-pollution agents, tanning agents, anti-glycation agents, sedatives, deodorants, essential oils, NO synthase inhibitors, agents for stimulating the synthesis of dermal or epidermal macromolecules and / or for preventing their degradation, agents for stimulating fibroblast proliferation, agents for stimulating keratinocyte proliferation, muscle relaxants, refreshing agents, tightening agents, pro-pigmenting agents, keratolytic agents, diluents, agents acting on cellular energy metabolism, insect repellents, substance P antagonists or CRGP antagonists, agents for preventing hair loss, and mixtures thereof.

[0242] The active agent may be chosen especially from:

[0243] - vitamins and their derivatives, in particular their esters, such as nicotinamide (3-pyridinecarboxamide), niacinamide (vitamin B3), tocopherol (vitamin E) and its esters (such as tocopherol acetate), ascorbic acid and its derivatives (vitamin C), retinol (vitamin A),

[0244] - moisturizers or humectants, for example urea, hydroxyurea, glycerol, polyglycerol, glyceryl glucoside, diglyceryl glucoside, polyglyceryl glucoside, xylosyl glucoside and plant extracts (especially extracts of tea, mint, orchid, soy, aloe vera, honey), and in particular glycerol;

[0245] -C-glycoside compound, preferably hydroxypropyltetrahydropyrantriol (or bosine);

[0246] - Antioxidant compounds;

[0247] - anti-aging active agents, such as hyaluronic acid compounds, especially sodium hyaluronate, salicylic acid compounds, especially 5-n-octanoylsalicylic acid (octanoylsalicylic acid), adenosine, C-β-D-xylopyranoside-2-hydroxypropane and the sodium salt of (3-hydroxy-2-pentylcyclopentyl)acetic acid;

[0248] - keratolytic agents such as lactic acid or glycolic acid; and

[0249] - A mixture thereof.

[0250] Such active agents may be present in the composition of the invention in an amount of 0.05-10 wt%, preferably 1.0-8.0 wt%, relative to the total weight of the composition.

[0251] d) Surfactants

[0252] According to one particular embodiment, the composition according to the invention comprises d) at least one surfactant.

[0253] Surfactant can be selected from nonionic, anionic, cationic and amphoteric surfactants and mixtures thereof. Reference can be made to Kirk-Othmer Encyclopedia of Chemical Technology, Vol. 22, pp. 333-432, 3rd edition, 1979, Wiley's definition of the emulsifying properties and functions of surfactants, particularly the 347-377 pages of this reference about anionic, amphoteric and nonionic surfactants.

[0254] Examples of amphoteric surfactants suitable for the present invention are especially chosen from betaines, preferably from alkyl betaines (especially lauryl betaine), N-alkylamidobetaines and their derivatives (especially cocamidopropyl betaine, lauramidopropyl betaine and N-disodium N-carboxyethoxyethyl N-cocamidoethyl aminoacetate), sultaines (especially cocoamidopropyl hydroxysultaine), and mixtures thereof.

[0255] The nonionic surfactants may especially be chosen from alkyl and polyalkyl esters of poly(ethylene oxide), oxyalkylenated alcohols, alkyl and polyalkyl ethers of poly(ethylene oxide), optionally polyoxyethylenated alkyl and polyalkyl esters of sorbitol, optionally polyoxyethylenated alkyl and polyalkyl ethers of sorbitol (in particular alkyl and polyalkyl esters of sucrose), optionally polyoxyethylenated alkyl and polyalkyl esters of glycerol, and optionally polyoxyethylenated alkyl and polyalkyl ethers of glycerol, gemini surfactants, cetyl alcohol, stearyl alcohol, and mixtures thereof.

[0256] The anionic surfactant may be selected from alkyl ether sulfates, carboxylates, amino acid derivatives, sulfonates, isethionates, taurates, sulfosuccinates, alkyl sulfoacetates, phosphates and alkyl phosphates, polypeptides, C 10 -C 30 and especially C 16 -C 25 Metal salts of fatty acids (especially metal stearates and behenates), and mixtures thereof.

[0257] The cationic surfactant may be selected from alkyl imidazolines For example, isostearyl ethylimide Ethyl sulfate, ammonium salts, such as (C 12-30 -alkyl)-tri(C 1-4 -alkyl) ammonium halide, such as N,N,N-trimethyl-1-docosahexanedimmonium chloride (or behenyltrimethylammonium chloride).

[0258] The silicone surfactant may be selected from dimethicone copolyols or silicone elastomers.

[0259] The composition of the present invention may comprise 0.01-2.0 wt%, preferably 0.05-1.5 wt%, more preferably 0.1-1.0 wt% of a surfactant relative to the total weight of the composition.

[0260] e) Thickener

[0261] According to one particular embodiment, the composition of the invention comprises e) at least one thickener, sometimes also called gelling agent or viscosity modifier.

[0262] The thickener may be synthetic, natural or of natural origin, preferably natural or of natural origin.

[0263] Such thickeners may more particularly be chosen from natural polymers or polymers of natural origin, in particular polymers of plant origin.

[0264] These gelling agents are preferably hydrophilic, ie, soluble or dispersible in water.

[0265] Advantageously, the thickener is chosen from modified or natural polysaccharides, in particular modified or unmodified starch, fructan, gellan gum, dextran, amylose, amylopectin, glycogen, pullulan, dextran, cellulose and its derivatives, in particular methylcellulose, hydroxyalkylcellulose, ethylhydroxyethylcellulose and carboxymethylcellulose, mannan, xylan, lignin, arabinan, galactan, galacturonic acid, alginate-based compounds, chitin, chitosan, glucuronoxylan, arabinoxylan, xyloglucan, glucomannan, pectin acid and pectin, arabinogalactan, carrageenan, agar, Aminoglucans, gum arabic, gum sclerotium, gum tragacanth, gum ghatti, gum karaya, locust bean gum, konjac gum, galactomannans (e.g. guar gum and their nonionic derivatives, in particular hydroxypropyl guar gum, and their ionic derivatives), biopolysaccharide gums of microbial origin (in particular scleroglucan or xanthan gum), mucopolysaccharides, carboxyvinyl polymers, polyacrylamides, polymers and copolymers of 2-acrylamido-2-methylpropanesulfonic acid, optionally crosslinked and / or neutralized water-soluble or water-dispersible silicone derivatives (e.g. acrylic siloxanes, polyether siloxanes and cationic siloxanes), and mixtures thereof.

[0266] The thickener may be present in the composition of the present invention in an amount of 0.05-5.0 wt%, particularly 0.3-4.0 wt%, more particularly 0.4-2.5 wt%, relative to the total weight of the composition.

[0267] Excipients

[0268] The composition of the present invention may also contain at least one auxiliary material commonly used in the cosmetic field, which is selected from fragrances, film-forming polymers, pH adjusters (acids or bases, such as citric acid, tartaric acid or oxalic acid), chelating agents, preservatives, softeners, sweeteners, defoaming agents, fillers, trace elements, propellants, and mixtures thereof.

[0269] It goes without saying that a person skilled in the art will carefully choose this or these optional additional compounds and / or their amounts such that the advantageous properties of the composition of the invention are not or not substantially adversely affected by the envisaged addition.

[0270] Of course, a person skilled in the art will carefully select the optional additional compound(s) and / or their amounts such that the advantageous properties of the particles of the invention are not or not substantially adversely affected by the envisaged addition.

[0271] As mentioned above, the composition of the present invention may be a cosmetic, and is preferably a cosmetic.

[0272] The compositions of the invention are generally suitable for topical administration to the skin and therefore generally comprise a physiologically acceptable medium, ie a medium that is compatible with the skin.

[0273] Cosmetically acceptable media are preferred, ie, media having a pleasing color, smell, and feel and not causing any unacceptable discomfort (ie, stinging or tightness) that would tend to deter the user from applying the composition.

[0274] Presentation form of the composition

[0275] Compositions, especially cosmetic compositions, containing the particles of the invention can be prepared according to techniques known to those skilled in the art.

[0276] According to the intended application, they may be in any conventional presentation form and are suitable for topical application, ie, application to the surface of the relevant keratinous material.

[0277] The cosmetic composition may be in the form of a hydrogel or a hydro-alcoholic gel.

[0278] They may be in the form of simple or complex (O / W, W / O, O / W / O or W / O / W) emulsions, for example creams, milks or gel-creams.

[0279] They may also be in anhydrous form, for example in the form of an oil.

[0280] By "anhydrous composition" is meant a composition containing less than 5% by weight of water, or even less than 2% of water, still better still less than 1% of water, and in particular no water, wherein the water is not added during the preparation of the composition, but corresponds to the residual water provided by the mixed ingredients.

[0281] The cosmetic composition can be used, for example, as a makeup product.

[0282] The cosmetic composition can be used, for example, as a face and / or body care and / or sun protection product having a liquid to semi-liquid consistency and having the appearance of a relatively thick white or pigmented cream, pomade, lotion, gel-cream, water solution, serum, paste or mousse. It can optionally be applied to the skin in aerosol form. It can also be in solid form, for example in the form of a stick.

[0283] The cosmetic composition may be in the form of a product for caring for the skin or semi-mucous membranes, such as a protective or beauty care composition for the face, lips, hands, feet, wrinkles or body, such as a day cream, a night cream, a day serum, a night serum, a make-up remover, a make-up base, a protective or care body lotion, an after-sun lotion, a skin or scalp care lotion, a gel or foam, a serum, a mask or an after-shave composition).

[0284] The composition may be applied by hand or using an applicator.

[0285] In particular, the cosmetic composition has an SPF greater than 5, preferably greater than 10.

[0286] "SPF" (i.e., sun protection factor) measures the level of protection against UV rays. It is mathematically expressed as the ratio of the UV radiation dose required to reach the threshold of causing erythema when using an anti-UV screener to the UV radiation dose required to reach the threshold of causing erythema when not using an anti-UV screener. Therefore, the higher the SPF of a composition, the higher the sun protection provided by the composition. More specifically, the term "SPF" is defined in the article "A new substrate to measure sunscreen protection factors throughout the ultraviolet spectrum, J. Soc. Cosmet. Chem., 40, 127-133 (May / June 1989).

[0287] In particular, the cosmetic composition also has a PPD of greater than 3, preferably greater than 7.

[0288] "PPD" (Persistent Pigment Darkening) is an indicator characterizing the protection against UVA rays. In particular, PPD measures the skin color observed 2 - 4 hours after exposure to UVA rays. Since 1996, the Japan Cosmetic Industry Association (JCIA) has adopted this method as the official test procedure for the UVA labeling of products and it is often used by test laboratories in Europe and the United States (Japan Cosmetic Industry Association Technical Bulletin, Standard for Measuring UV - A Protection Effect, January 1, 1996).

[0289] Cosmetic uses and methods

[0290] The present invention also relates to a non - therapeutic cosmetic method for filtering UV radiation (especially UVB radiation), which method comprises applying at least a composition comprising bismuth oxycarbonate particles as defined above to a keratinous material.

[0291] According to another aspect thereof, the present invention also relates to the non - therapeutic cosmetic use of a cosmetic composition comprising bismuth oxycarbonate particles as defined above for preventing the appearance of darker and / or more pigmented spots on the skin, especially on the face, neck, arms, hands and / or shoulders, which cause uneven skin color.

[0292] The present invention also relates to a non - therapeutic cosmetic method for limiting skin darkening and / or improving skin color and / or skin color uniformity, which method comprises applying at least one cosmetic composition comprising bismuth oxycarbonate particles as defined above to the surface of a keratinous material.

[0293] The present invention additionally relates to the non - therapeutic cosmetic use of a cosmetic composition comprising bismuth oxycarbonate particles as defined above for preventing premature aging of the skin, especially on the face, neck, arms, hands and / or shoulders.

[0294] The present invention also relates to a non - therapeutic cosmetic method for preventing and / or treating signs of aging of a keratinous material, which method comprises applying at least one cosmetic composition comprising bismuth oxycarbonate particles as defined above to the surface of a keratinous material.

[0295] According to one aspect thereof, the present invention relates to bismuth oxycarbonate particles having the empirical formula (BiO) 2-x (CO3) as a reagent for filtering UV radiation, especially UVB radiation, wherein - 0.4 < x < 0.6 and the maximum average size of said particles is less than 400 nm.

[0296] For the purposes of the present invention, "prevent" or "prevention" means at least partially reducing the risk of a given phenomenon, such as signs of aging of keratinous material or the appearance of darker and / or more pigmented spots on the skin, which leads to uneven skin color, and / or premature skin aging.

[0297] The percentages in the specification and examples are all by weight. The ingredients are mixed in an order and under conditions that can be easily determined by a person skilled in the art.

[0298] The present invention will now be described by means of the following examples which are of course intended to be non-limiting illustrations of the present invention.

[0299] BRIEF DESCRIPTION OF THE DRAWINGS

[0300] Figure 1 An electron micrograph of bismuth oxycarbonate particles A is depicted.

[0301] Figure 2 An electron micrograph of bismuth oxycarbonate particles B is depicted.

[0302] Figure 3 An electron micrograph of bismuth oxycarbonate particles C is depicted.

[0303] Figure 4 An electron micrograph of bismuth oxycarbonate particles D is depicted.

[0304] Figure 5 An electron micrograph of bismuth oxycarbonate particles E is depicted.

[0305] Figure 6 An electron micrograph of bismuth oxycarbonate particles F is depicted.

[0306] Figure 7 An electron micrograph of bismuth oxycarbonate particles G is depicted.

[0307] Figure 8 An electron micrograph of a bismuth oxycarbonate particle G' is depicted.

[0308] Fig. 9 An electron micrograph of bismuth oxycarbonate particles H is depicted.

[0309] Fig.10 An electron micrograph of bismuth oxycarbonate particles H' is depicted.

[0310] Fig.11 An electron micrograph of bismuth oxycarbonate particles I is depicted.

[0311] Fig.12 An electron micrograph of bismuth oxycarbonate particles J is depicted.

[0312] Fig.13An electron micrograph of bismuth oxycarbonate particles K is depicted.

[0313] Fig.14 An electron micrograph of bismuth oxycarbonate particles L is depicted.

[0314] Fig.15 An electron micrograph of bismuth oxycarbonate particles M is depicted.

[0315] Fig.16 The UV-visible absorption spectra of product A and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.01% of the particles.

[0316] Fig.17 The UV-visible absorption spectra of product B and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.01% of the particles.

[0317] Fig.18 The UV-visible absorption spectra of product C and two commercial references, namely TiO2 from Tayca's MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%.

[0318] Fig.19 The UV-visible absorption spectra of product D and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.01% of the particles.

[0319] Fig. 20 The UV-visible absorption spectra of Product E and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%.

[0320] Fig.21 The UV-visible absorption spectra of Product F and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%.

[0321] Fig. 22The UV-visible absorption spectra of Product G and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%.

[0322] Fig.23 The UV-visible absorption spectra of product G' and two commercial references, namely TiO2 from Tayca's MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.005% of particles (the spectrophotometer was clearly saturated at 0.01%).

[0323] Fig.24 The UV-visible absorption spectra of product H and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.01% of the particles.

[0324] Fig.25 The UV-visible absorption spectra of the product H' and of two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of 0.01% of the particles.

[0325] Fig.26 The UV-visible absorption spectra of Product I and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of the particles of 0.01%.

[0326] Fig. 27 The UV-visible absorption spectra of Product J and two commercial references, namely TiO2 from Tayca as MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%.

[0327] Fig.28 The UV-visible absorption spectra of product K and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of the particles of 0.01%.

[0328] Fig.29The UV-visible absorption spectra of product L and two commercial references, namely TiO2 from Tayca as MT-100TV, and (BiO)2(CO3) from Alfa Aesar are depicted. The spectra were obtained for a weight concentration of the particles of 0.01%.

[0329] Fig.30 The UV-visible absorption spectra of product M and two commercial references, namely TiO2 from Tayca MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a weight concentration of the particles of 0.01%.

[0330] Fig.31 The UV-visible absorption spectra of product N and two commercial references, namely TiO2 from Tayca's MT-100TV, and (BiO)2(CO3) from Alfa Aesar, are depicted. The spectra were obtained for a particle weight concentration of 0.01%. Example

[0331] Example 1: Synthesis of Bismuth Oxycarbonate Particles of the Present Invention

[0332] Example 1.A: Solvothermal synthesis of crystalline particles A using (NH4)2CO3 and D-mannitol (0.25M) at 100°C

[0333] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M) and D-mannitol (0.25 M) was prepared in 50 ml of water and stirred until each reagent was completely dissolved.

[0334] 10 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) are then added. A white solid precipitates out. The mixture is then transferred to an autoclave-type reactor made of Teflon and heated at 100° C. for 12 hours.

[0335] Product A was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0336] Product A was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0337] Example 1.B: Solvothermal synthesis of crystalline particles B using urea and D-mannitol (0.25 M) at 120°C

[0338] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M) and D-mannitol (0.25 M) was prepared in 50 ml of water and stirred until each reagent was completely dissolved.

[0339] 10 ml of saturated urea solution (90 equivalents relative to bismuth) are then added. A white solid precipitates out. The mixture is then transferred to an autoclave-type reactor made of Teflon and heated at 120° C. for 12 hours.

[0340] Product B was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0341] Product B was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0342] Example 1.C: Solvothermal synthesis of crystalline particles C using (NH4)2CO3 and D-mannitol (0.1 M) at 150°C

[0343] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M) and D-mannitol (0.1 M) was prepared in 50 ml of water and stirred until each reagent was completely dissolved.

[0344] 10 ml of a supersaturated ammonium carbonate solution (21 equivalents relative to bismuth) are then added. A white solid precipitates out. The mixture is then transferred to an autoclave-type reactor made of Teflon and heated at 150° C. for 12 hours.

[0345] Product C was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0346] The product C was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0347] Example 1.D: Synthesis of crystalline particles D using (NH4)2CO3 and D-mannitol (0.1M) reflux at 100°C

[0348] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04M) and D-mannitol (0.1M) was prepared in 50 ml of water and stirred until each reagent was completely dissolved. Subsequently, 10 ml of supersaturated ammonium carbonate solution (21 equivalents relative to bismuth) was added. A white solid precipitated out. The mixture was then refluxed at 100°C for 8 hours.

[0349] Product D was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0350] The product D was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0351] Example 1.E: Synthesis of manganese-doped crystalline particles E using (NH4)2CO3 and D-mannitol (0.1M) reflux at 100°C

[0352] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), manganese nitrate hydrate Mn(NO3)3·xH2O (0.004 M) and D-mannitol (0.1 M) was prepared in 50 ml of water and stirred until each reagent was completely dissolved.

[0353] 10 ml of supersaturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A white solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0354] Product E was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0355] Product E was isolated as a pale pink-white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry. Elemental analysis of the product showed a Bi / Mn molar ratio of 95:5.

[0356] Example 1.F: Synthesis of a mixture of amorphous and crystalline particles F using urea and propylene glycol reflux at 170°C

[0357] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.015 M) was prepared in 130 ml of propylene glycol until all reagents were completely dissolved.

[0358] 10 ml of a solution of urea in propylene glycol (20 equivalents relative to bismuth) are subsequently added. The mixture is heated at 180° C. for 1 hour.

[0359] Product F was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0360] Product F was isolated and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0361] Example 1.G: Synthesis of iron-doped crystalline particles G using (NH4)2CO3 and D-mannitol (0.1 M) at 100°C

[0362] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), ferric nitrate Fe(NO3)3·9H2O (0.002 M) and D-mannitol (0.1 M) was prepared in 150 ml of water and stirred until each reagent was completely dissolved.

[0363] 30 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A yellow solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0364] The product G was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60°C.

[0365] The product G was isolated as a light yellow powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0366] Example 1. G': Synthesis of iron-doped crystalline particles G' using (NH4)2CO3 and D-mannitol (0.5M) at 100°C

[0367] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), ferric nitrate Fe(NO3)3·9H2O (0.002 M) and D-mannitol (0.5 M) was prepared in 150 ml of water and stirred until each reagent was completely dissolved.

[0368] 30 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A yellow solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0369] The product G' was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60 °C.

[0370] The product G' was isolated as a light yellow powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0371] Example 1.H: Synthesis of chlorine-doped crystalline particles H using (NH4)2CO3 and D-mannitol (0.1 M) at 100°C

[0372] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), potassium chloride KCl (0.004 M) and D-mannitol (0.1 M) was prepared in 150 ml of water and stirred until each reagent was completely dissolved.

[0373] 30 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A white solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0374] The product H was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60 °C.

[0375] The product H was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0376] Example 1. H': Synthesis of chlorine-doped crystalline particles H' using (NH4)2CO3 and D-mannitol (0.5M) at 100°C

[0377] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), potassium chloride KCl (0.004 M) and D-mannitol (0.5 M) was prepared in 150 ml of water and stirred until each reagent was completely dissolved.

[0378] 30 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A white solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0379] The product H' was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60 °C.

[0380] The product H' was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0381] Example 1.I: Synthesis of iodine-doped crystalline particles I using (NH4)2CO3 and D-mannitol (0.1 M) at 100°C

[0382] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M), iodine chloride KI (0.004 M) and D-mannitol (0.1 M) was prepared in 150 ml of water and stirred until each reagent was completely dissolved.

[0383] 30 ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) were subsequently added. A white solid precipitated out. The mixture was then refluxed at 100° C. for 8 hours.

[0384] The product I was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60°C.

[0385] The product I was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0386] Example 1.J: Synthesis of crystalline particles doped with sulfate ions using (NH4)2CO3 and D-mannitol (0.1 M) at 100°C

[0387] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04M), ammonium sulfate (NH4)2SO4 (0.004M) and D-mannitol (0.1M) was prepared in 150ml of water and stirred until each reagent was completely dissolved. Subsequently, 30ml of saturated ammonium carbonate solution (21 equivalents relative to bismuth) was added. A white solid precipitated out. The mixture was then refluxed at 100°C for 8 hours.

[0388] Product J was isolated by centrifugation and washed alternately in water and ethanol for 3 times, and then dried in an oven at 60 °C.

[0389] The product J was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0390] Example 1.K: Solvothermal synthesis of crystalline particles K using Na2CO3 and D-mannitol (0.5M) at 150°C

[0391] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M) and D-mannitol (0.5 M) was prepared in 25 ml of water and stirred until each reagent was completely dissolved.

[0392] 5 ml of saturated sodium carbonate solution were added. A white solid precipitated out. The mixture was subsequently transferred to an autoclave-type reactor made of Teflon and heated at 150° C. for 12 hours.

[0393] The product K was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60 °C.

[0394] The product K was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0395] Example 1.L: Solvothermal synthesis of crystallized particles L using Na2CO3 and glycerol / water mixture at 150°C

[0396] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04M) was prepared in 25 ml of a glycerol / water mixture (3:2 v / v) and stirred until the reagents were completely dissolved. 5 ml of a saturated sodium carbonate solution was added. A white solid precipitated out. The mixture was then transferred to an autoclave type reactor made of Teflon and heated at 150°C for 12 hours.

[0397] The product L was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0398] The product L was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0399] Example 1.M: Solvothermal synthesis of crystallized particles M using Na2CO3 and ethylene glycol at 150°C

[0400] A solution of bismuth nitrate pentahydrate Bi(NO3)3·5H2O (0.04 M) was prepared in 25 ml of ethylene glycol and stirred until the reagents were completely dissolved. Then 5 ml of saturated sodium carbonate solution was added. A white solid precipitated out. The mixture was then transferred to an autoclave type reactor made of Teflon and heated at 150°C for 12 hours.

[0401] The product M was isolated by centrifugation and washed alternately in water and ethanol for 5 times, and then dried in an oven at 60°C.

[0402] The product M was isolated as a white powder and characterized by transmission electron microscopy and by UV / Vis spectrophotometry.

[0403] Example 2: Morphology and size of bismuth oxycarbonate particles of the present invention

[0404] The morphology of the particles of each product prepared in Example 1 was determined by direct observation using transmission electron microscopy.

[0405] 1-5 mg of dry particles were dispersed in 10 ml of absolute ethanol and treated in an ultrasonic bath for 2 min.

[0406] 5 μl of the dispersion was then placed on a viewing grid (copper with a surface carbon layer) and dried in ambient air.

[0407] Observations were performed using a Hitachi HT 7700 transmission electron microscope at an accelerating voltage of 100 kV.

[0408] Figure 1-15 Images of product AM prepared in Example 1 are presented.

[0409] The average size was obtained by measuring the particle size by image analysis using the software ImageJ (C Schneider, WS Rasband, KW Eliceiri, NIH Image to ImageJ: 25 years of image analysis, Nat. Methods. 9 (2012) 671-675).

[0410] The results are summarized in Table 1 below.

[0411] Table 1

[0412]

[0413] The bismuth oxycarbonate particles synthesized by the present invention are all in the following forms: tubes, flakes, rods and / or mixtures thereof. The maximum size of each particle is less than 400 nm.

[0414] Example 3: Preparation of a dispersion containing the crystallized bismuth oxycarbonate particles A of the present invention

[0415] A dispersion of the crystallized bismuth oxycarbonate particles A of Example 1.A was prepared in a water / propylene glycol / Tween 20 / xanthan gum mixture.

[0416] The water / propylene glycol / Tween 20 / xanthan gum mixture was added at ambient temperature directly to an accurately weighed mass of Granule A powder. The suspension was then stirred for 10 minutes using a magnetic stirrer, exposed to ultrasound for 15 minutes, and then stirred again by magnetic stirring for 16 hours.

[0417] Table 2 shows the weight percentage of each component relative to the total weight of the composition.

[0418] Table 2

[0419] Compound Dispersion of the present invention Example 1. Oxycarbonate particles A 0.1 Xanthan gum 0.1 Polysorbate 20 (sold as Tween 20 by Acros Organics) 0.3 Propylene glycol 49.75 water 49.75

[0420] The dispersion obtained was fluid and white in color.

[0421] Example 3': Preparation of a dispersion N comprising the crystallized bismuth oxycarbonate particles A of the invention

[0422] A dispersion of crystalline bismuth oxycarbonate particles A of Example 1.A and titanium dioxide MT-100-TV was prepared in a water / propylene glycol / Tween 20 / Basic Red 51 mixture.

[0423] The water / propylene glycol / Tween 20 / Basic Red 51 mixture was added directly to accurately weighed masses of Granule A powder and titanium dioxide MT-100-TV at ambient temperature. The suspension was then stirred for 10 minutes using a magnetic stirrer, exposed to ultrasound for 15 minutes, and then stirred again by magnetic stirring for 16 hours.

[0424] The dispersion was then diluted to 0.01 wt% (or 0.005 wt% of particles A of Example 1.A and 0.005 wt% of titanium dioxide) with water / propylene glycol / Tween 20 medium. The resulting dispersion was then stirred for 20 minutes with magnetic stirring before absorbance measurement.

[0425] Table 2' shows the weight percentage of each component relative to the total weight of the composition.

[0426] Table 2'

[0427] Compound Dispersion N of the present invention Example 1. Oxycarbonate particles A 2 <![CDATA[Nano-TiO2 treated with aluminum hydroxide and stearic acid (MT-100-TV sold by Tayca)]]> 2 Basic Red 51 (including 13.5% NaCl) 0.05 Polysorbate 20 (sold as Tween 20 by Acros Organics) 0.29 Propylene glycol 47.83 water 47.83

[0428] The dispersion obtained was viscous and light orange in color.

[0429] Example 4: Preparation of dispersions containing bismuth oxycarbonate particles or titanium dioxide particles

[0430] Separate dispersions of bismuth oxycarbonate particles AM from Example 1, crystalline bismuth oxycarbonate particles not according to the invention, and titanium dioxide particles were prepared in a water / propylene glycol / Tween 20 mixture.

[0431] First, a 0.10 wt% dispersion of each was prepared by adding a water / propylene glycol / Tween 20 mixture to an accurately weighed mass of each particle powder.

[0432] Each dispersion was exposed to ultrasound for 15 minutes and then stirred with a magnetic stirrer for 16 hours.

[0433] They were then diluted to 0.01 wt% (or 0.005 wt% of particles G') and stirred again with magnetic stirring for 20 minutes before absorbance measurement.

[0434] Table 3' shows the weight percentage of each component relative to the total weight of the dispersion.

[0435] Table 3'

[0436]

[0437] The resulting dispersions were fluid and white, except for dispersions G and G' which were light yellow.

[0438] Example 5: Absorption spectra of bismuth oxycarbonate particles of the present invention and commercial particles

[0439] The UV-visible absorption spectrum of the bismuth oxycarbonate particles according to the invention prepared according to Example 1 was generated and compared with the absorption spectra of two nanoscale references ((BiO)2CO3, Alfa Aesar, flakes, average size: L, l≈500 nm and e=50 nm; and nano-TiO2 treated with aluminum hydroxide and stearic acid, MT-100TV from Tayca).

[0440] An absorption spectrum was obtained for the dispersion prepared in Example 4 by UV-Vis spectroscopy.

[0441] The quartz cell used for absorbance measurement had a side length of 1 cm. The spectrophotometer used was a Genesys 10S from Thermo Fischer Scientific.

[0442] Above a predetermined threshold UV absorbance measurement, particles are considered effective in filtering UV radiation. In particular, particles having a UV absorbance threshold greater than 0.5 in a dispersion medium containing the particles are considered effective in filtering UV radiation.

[0443] The absorption spectrum is Figure 16-30 Presented in.

[0444] The results are summarized in Table 4 below.

[0445] Table 4

[0446]

[0447] In the entire UV range of 220-400 nm, especially in the UVB range, the absorption spectrum of the bismuth oxycarbonate particles of the present invention is similar to the absorption spectrum of TiO2 particles.

[0448] The absorption spectrum also shows that the bismuth oxycarbonate particles of the present invention have high transparency in the visible light range of 400-780 nm.

[0449] (BiO)2CO3 from Alfa Aesar has a constant absorbance value of 0.2. This absorbance is low and shows that bismuth oxycarbonate particles with a size greater than 400 nm cannot filter the entire UV range sufficiently.

[0450] In contrast, the use of the bismuth oxycarbonate particles of the present invention shows improved UV ray absorptivity and thus effectively filters UV rays.

[0451] Example 6: Absorption spectra of bismuth oxycarbonate particles of the present invention and commercial particles

[0452] The UV-visible absorption spectrum of the bismuth oxycarbonate particles according to the invention prepared according to Example 1 was generated and compared with the absorption spectra of two nanoscale references ((BiO)2CO3, Alfa Aesar, flakes, average size: L, l≈500 nm and e=50 nm; and nano-TiO2 treated with aluminum hydroxide and stearic acid, MT-100TV from Tayca).

[0453] Absorption spectra were obtained by UV-Vis spectroscopy for the dispersion prepared in Example 3'.

[0454] The quartz cell used for absorbance measurement had a side length of 1 cm. The spectrophotometer used was a Genesys 10S from Thermo Fischer Scientific.

[0455] Above a predetermined threshold UV absorbance measurement, particles are considered effective in filtering UV radiation. In particular, particles having a UV absorbance threshold greater than 0.5 in a dispersion medium containing the particles are considered effective in filtering UV radiation.

[0456] The absorption spectrum is Fig.31 Presented in.

[0457] The results are summarized in Table 5 below.

[0458] Table 5

[0459]

[0460] Absorption spectrum ( Fig.31 ) show that the bismuth oxycarbonate particles of the present invention, when used in combination with a colorant, exhibit effective filtering of UV rays.

Claims

1. Use of bismuth oxycarbonate particles having the empirical formula (BiO) 2-x (CO3), where -0.4 < x < 0.6, and the maximum average size of the particles is less than 400 nm, for filtering ultraviolet radiation.

2. The use according to claim 1, for filtering UVB radiation.

3. The use according to claim 1 or 2, wherein the bismuth oxycarbonate particles are crystalline.

4. The use according to any one of the preceding claims, wherein the bismuth oxycarbonate particles have the formula (BiO)2(CO3).

5. The use according to any one of the preceding claims, wherein the maximum average size of the particles is less than or equal to 300 nm.

6. The use according to any one of the preceding claims, wherein the particles are in the form of tubes, flakes and / or rods.

7. The use according to any one of the preceding claims, wherein the particles are mainly or solely in the form of flakes, and have an average length L of 15 - 300 nm, especially 30 - 250 nm, an average width l of 10 - 250 nm, especially 20 - 200 nm, and an average thickness e of 2 - 120 nm, especially 5 - 100 nm, and e < l < L.

8. The use according to any one of claims 1 - 6, wherein the particles are mainly or solely in the form of rods, and have an average length L of 30 - 300 nm, especially 50 - 250 nm, a diameter d of 15 - 150 nm, especially 20 - 130 nm, and L > d.

9. The use according to any one of claims 1 - 6, wherein the particles are mainly or solely in the form of tubes, and have an average length L of 10 - 300 nm, especially 20 - 250 nm, a diameter d of 2 - 30 nm, especially 3 - 20 nm, and L > d.

10. The use according to any one of the preceding claims, wherein the particles are doped, especially doped with cations of elements selected from titanium, vanadium, manganese, iron, copper, zinc, lanthanum and / or cerium, more preferably doped with cations of elements selected from manganese, iron and / or cerium, even more preferably doped with cations of elements from manganese or iron; and / or doped with anions selected from S 2- , SO3 2- , SO4 2- , Cl - and / or I - , preferably doped with anions selected from SO3 2- , SO4 2- and / or Cl - , more preferably doped with anions selected from Cl - or SO42- anion doping.

11. The use according to any one of claims 1 to 9, wherein the particles are undoped.

12. A composition, especially a cosmetic composition, comprising at least: i) bismuth oxycarbonate particles as defined in any one of claims 1 to 11, ii) at least one aqueous phase and / or at least one fatty phase, and iii) at least one compound selected from the group consisting of a) UV screening agents other than the bismuth oxycarbonate particles i), b) colorants, c) cosmetic active agents for caring for keratinous materials, d) surfactants, e) thickeners, and mixtures thereof.

13. The composition according to the preceding claim, comprising 0.5-40 wt%, preferably 1-30 wt%, even more preferably still 2-20 wt% of bismuth oxycarbonate particles, relative to the total weight of the composition.

14. A non-therapeutic cosmetic method for filtering UV radiation, in particular UVB radiation, comprising at least a composition comprising a composition having the empirical formula (BiO) 2-x A cosmetic composition of bismuth carbonate particles (CO3) is applied to keratinous material, wherein -0.4