Chemically amplified positive photoresist composition for improving sensitivity and pattern profile
By adding components such as inorganic acids, oxidants, fluorine compounds, and pH adjusters to the etching solution composition, the problem that the existing technology cannot simultaneously inhibit the etching of the aluminum oxide film and the silicon oxide film and remove the molybdenum film is solved, and the molybdenum film is achieved. Effective etching and particle improvement for semiconductor manufacturing processes.
Patent Information
- Application Number
- CN202280092576.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2022-10-25
- Publication Date
- 2024-10-08
AI Technical Summary
The existing technology cannot effectively remove the molybdenum film and the denatured molybdenum film while suppressing the etching of the aluminum oxide film and the silicon oxide film. As a result, the etching solution composition cannot meet the etching requirements of the molybdenum film and may cause particle problems.
Using an etching solution composition containing inorganic acids, oxidants, fluorine compounds, pH regulators and specific additives, by adjusting the composition ratio, it can significantly inhibit the etching of the aluminum oxide film and silicon oxide film, and simultaneously remove the molybdenum film and denatured film quality, thereby achieving molybdenum Efficient etching of membranes.
It achieves the removal of molybdenum film and denatured molybdenum film while suppressing etching of aluminum oxide film and silicon oxide film, meets the etching requirements of molybdenum film, improves particle problems, and is suitable for semiconductor manufacturing processes.
Smart Images

Figure BDA0005010001540000061 
Figure BDA0005010001540000071 
Figure BDA00050100015400000924
Abstract
Description
Technical Field
[0001] The present invention relates to an etching liquid composition capable of etching a molybdenum film in a process of manufacturing a semiconductor device and an etching method using the same. Specifically, the present invention relates to an etching liquid composition capable of significantly suppressing the etching of an insulating film while removing a molybdenum film and a modified molybdenum film, thereby being able to fully etch the molybdenum film and an etching method using the same. Background Art
[0002] Generally, in the process of manufacturing semiconductors, molybdenum films (Mo) are used for gate electrodes, wirings, barrier layers, and buried contact holes or through holes of thin film transistors of semiconductor devices and liquid crystal displays.
[0003] In the process of manufacturing semiconductors, the molybdenum film (Mo) is used as a conductive metal and can be used alone or stacked with the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) and use.
[0004] In the process of manufacturing semiconductors, as a process for removing a molybdenum film (Mo), there are a dry etching process and a wet etching process, and there are cases where both are used simultaneously.
[0005] In this case, the aluminum oxide film (AlO x ) and silicon oxide film (SiO x The etching process of etching the molybdenum film (Mo) at the same time as etching ) is difficult to achieve using a dry etching process, so a wet etching process is required.
[0006] In addition, there is a need for a method that can remove the molybdenum film (Mo) and the molybdenum oxide film (MoO) generated during the etching process. x ) and the like.
[0007] Korean Patent Publication No. 10-2021-0051085 discloses a technology related to an etching solution composition for etching a molybdenum film (Mo) and a pattern forming method using the same.
[0008] However, the above patent document discloses that a fluorine compound is used to prevent an aluminum oxide film (AlO) from being oxidized during etching of a molybdenum film (Mo) as an etching target film. x ) and silicon oxide film (SiO x ) damage, but does not specifically disclose the simultaneous removal of the molybdenum oxide film (MoO x ) and other modified molybdenum films.
[0009] That is, according to the prior art, since it is only possible to suppress the aluminum oxide film (AlO x ) and silicon oxide film (SiOx ) is etched while etching the molybdenum film (Mo), but the molybdenum oxide film (MoO) generated during the etching of the molybdenum film (Mo) cannot be removed at the same time. x ) and the like, and therefore, there is ultimately a problem in that an etching solution composition that satisfies the etching requirements for the molybdenum film (Mo) cannot be provided. Summary of the invention
[0010] Technical issues to be solved
[0011] The present invention aims to solve the problem that the etching solution composition in the prior art can only suppress the formation of aluminum oxide film (AlO) when performing various wet etching processes on molybdenum film (Mo). x ) and silicon oxide film (SiO x ) is etched while the molybdenum film (Mo) is etched, but the molybdenum oxide film (MoO x ) and the like to generate particles, the present invention aims to provide a method for significantly suppressing the formation of particles in the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) can be removed by etching the molybdenum film (Mo) and the molybdenum oxide film (MoO x ) etc., thereby being able to meet the requirements of etching the molybdenum film (Mo), and being not only widely applicable to semiconductor manufacturing processes, but also being able to improve the etching liquid composition that causes the problem of particle generation.
[0012] Another object of the present invention is to provide an etching method using the etching solution composition.
[0013] Solutions to the problem
[0014] The etching solution composition according to the present invention comprises an inorganic acid, an oxidizing agent, a fluorine compound, a pH adjusting agent, an additive represented by the following chemical formula 1, and a balance of water, and can significantly inhibit the formation of an aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) is etched to remove the molybdenum film (Mo) and the modified film (molybdenum oxide film (MoO x )), thereby finally satisfying the etching of the molybdenum film (Mo).
[0015] The inorganic acid contained in the etching solution composition of the present invention may be any one selected from the group consisting of sulfuric acid, phosphoric acid, polyphosphoric acid, hydrochloric acid, p-toluenesulfonic acid, and a mixture thereof.
[0016] The content of the inorganic acid may be 0.1 to 10 wt % relative to the total weight of the etching solution composition.
[0017] Furthermore, the oxidant contained in the etching solution composition of the present invention may be any one selected from the group consisting of hydrogen peroxide, nitric acid, ammonium nitrate, ammonium phosphate, ammonium persulfate, periodic acid, urea-hydrogen peroxide, tert-butyl hydroperoxide and 2-butane peroxide.
[0018] At this time, the content of the oxidant may be 0.001 to 5 wt % relative to the total weight of the etching solution composition.
[0019] Furthermore, the fluorine compound contained in the etching solution composition of the present invention may be any one selected from the group consisting of hydrofluoric acid, ammonium fluoride, tetrafluoroboric acid, and hexafluorosilicate.
[0020] At this time, the content of the fluorine compound may be 0.001 to 3 wt % relative to the total weight of the etching solution composition.
[0021] Furthermore, the pH adjuster contained in the etching solution composition of the present invention may be any one selected from the group consisting of phosphates and sulfates.
[0022] At this time, the content of the pH adjuster may be 0.1 to 10 wt % relative to the total weight of the etching solution composition.
[0023] In addition, the additive contained in the etching solution composition of the present invention is represented by the following chemical formula 1, and the content of the compound represented by the chemical formula 1 may be 0.0001 to 2 wt % relative to the total weight of the etching solution composition.
[0024] [Chemical formula 1]
[0025] F(CF 2 CF 2 )xCH 2 CH 2 OH
[0026] (In the above Chemical Formula 1, x may be an integer ranging from 1 to 10.)
[0027] In order to maintain the molybdenum film (Mo) and the modified film quality (molybdenum oxide film (MoO x )) while suppressing the etching rate of the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ), the etching liquid composition can adjust the composition components and composition ratio of the composition, in particular, can adjust the content of the additive represented by Chemical Formula 1, thereby being able to etch the molybdenum film (Mo) and the modified film (molybdenum oxide film (MoO x )) while suppressing the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) etching.
[0028] The temperature of the etching process of the etching solution composition can be room temperature to 60°C. In order to increase the stability of the etching process, the inorganic acid and the remaining components can be mixed in the equipment and used. When mixed outside the equipment, they can be mixed and used just before starting the etching process.
[0029] Effects of the Invention
[0030] The etching solution composition of the present invention has the effect of solving the following problem, that is, when a plurality of wet etching processes are performed on a molybdenum film (Mo) according to the etching solution composition of the prior art, only the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) is etched while the molybdenum film (Mo) is etched, but the molybdenum oxide film (MoO x ) and other problems of the generation of particles by the modified molybdenum film, and a method for significantly inhibiting the generation of particles by the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) can be removed by etching the molybdenum film (Mo) and the molybdenum oxide film (MoO x ) and the like, thereby being able to meet the requirements for etching of molybdenum film (Mo), and being not only widely applicable to semiconductor manufacturing processes, but also an etching liquid composition and an etching method using the same that can improve the problem of particle generation. DETAILED DESCRIPTION
[0031] Best Mode for Carrying Out the Invention
[0032] The present invention is described in further detail below. Unless otherwise defined, all technical and scientific terms used in the specification of the present invention have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0033] Generally, the nomenclature used in the specification of the present invention is well known and commonly used in the technical field to which the present invention belongs. Throughout the specification of the present invention, if a part is mentioned to "include" a certain constituent element, in the absence of a special contrary record, it means that other constituent elements may also be included rather than excluding other constituent elements.
[0034] According to an embodiment of the present invention, the etching composition is an etching solution composition comprising an inorganic acid, an oxidizing agent, a fluorine compound, a pH adjusting agent, an additive and a balance of water, which can significantly inhibit the oxidation of aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) is etched to remove the molybdenum film (Mo) and the modified film (molybdenum oxide film (MoO x )), thereby finally satisfying the etching of the molybdenum film (Mo).
[0035] The inorganic acid contained in the etching solution composition according to an embodiment of the present invention may be any one selected from the group consisting of sulfuric acid, phosphoric acid, polyphosphoric acid, hydrochloric acid, p-toluenesulfonic acid, and a mixture thereof.
[0036] At this time, the content of the inorganic acid may be 0.1 to 10 wt % relative to the total weight of the etching solution composition.
[0037] Furthermore, the oxidant contained in the etching solution composition of the present invention may be any one selected from the group consisting of hydrogen peroxide, nitric acid, ammonium nitrate, ammonium phosphate, ammonium persulfate, periodic acid, urea-hydrogen peroxide, tert-butyl hydroperoxide and 2-butane peroxide.
[0038] The content of the oxidant may be 0.001 to 5 weight % relative to the total weight of the etching solution composition.
[0039] Furthermore, the fluorine compound contained in the etching solution composition of the present invention may be any one selected from the group consisting of hydrofluoric acid, ammonium fluoride, tetrafluoroboric acid, and hexafluorosilicate.
[0040] The content of the fluorine compound may be 0.001 to 3 wt % relative to the total weight of the etching solution composition.
[0041] Furthermore, the pH adjuster contained in the etching solution composition of the present invention may be any one selected from the group consisting of phosphates and sulfates.
[0042] The pH adjuster may be contained in an amount of 0.1 to 10 wt % relative to the total weight of the etching solution composition.
[0043] In addition, the additive contained in the etching solution composition of the present invention is represented by the following chemical formula 1, and the content of the compound represented by the chemical formula 1 may be 0.0001 to 2 wt % relative to the total weight of the etching solution composition.
[0044] [Chemical formula 1]
[0045] F(CF 2 CF 2 )xCH 2 CH 2 OH
[0046] (In the above Chemical Formula 1, x may be an integer ranging from 1 to 10.)
[0047] According to one embodiment of the present invention, it relates to an etching solution composition and an etching method using the same, which etches a molybdenum film and a modified molybdenum film while suppressing the etching of an aluminum oxide film and a silicon oxide film. The composition is characterized in that, relative to the total weight of the composition, the composition is composed of 0.1 to 10 weight % of an inorganic acid, 0.001 to 5 weight % of an oxidizing agent, 0.001 to 3 weight % of a fluorine compound, 2 to 4 weight % of a pH adjusting agent, 0.0001 to 2 weight % of an additive, and the remainder of water.
[0048] In order to maintain the molybdenum film (Mo) and the modified film quality (molybdenum oxide film (MoO x )) while suppressing the etching rate of the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ), the etching liquid composition can adjust the composition components and composition ratio of the composition, in particular, can adjust the content of the additive represented by Chemical Formula 1, thereby being able to etch the molybdenum film (Mo) and the modified film (molybdenum oxide film (MoO x )) while suppressing the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) etching.
[0049] The temperature of the etching process of the etching solution composition can be room temperature to 60°C. In order to increase the stability of the etching process, the inorganic acid and the remaining components can be mixed in the equipment and used. When mixed outside the equipment, they can be mixed and used just before starting the etching process.
[0050] Modes for Carrying Out the Invention
[0051] Examples 1 to 22 and Comparative Examples 1 to 9
[0052] The etching liquid compositions of Examples and Comparative Examples were added to each experimental beaker equipped with a magnetic bar according to the composition ratio described in [Table 1], and then the top of the beaker was sealed and stirred at 400 rpm for 30 minutes at room temperature to prepare etching liquid compositions.
[0053] [Table 1]
[0054]
[0055]
[0056] A-1: Phosphoric acid
[0057] A-2: Sulfuric acid
[0058] B-1: Hydrogen Peroxide
[0059] B-2: Periodic acid
[0060] C-1: Hexafluorosilicate
[0061] C-2: Ammonium fluoride
[0062] C-3: Tetrabutylammonium fluoride
[0063] D-1: Phosphate
[0064] E-1: In chemical formula 1, x=3
[0065] E-2: In chemical formula 1, x=4
[0066] E-3: In chemical formula 1, x=5
[0067] E-4: In chemical formula 1, x=6
[0068] E-5: In chemical formula 1, x=7
[0069] F-1: Deionized water
[0070] Experimental Examples 1 to 22 and Comparative Experimental Examples 1 to 9
[0071] The etching solutions prepared in Examples 1 to 22 and Comparative Examples 1 to 9 were measured to determine the effects of the etching solutions on the molybdenum film (Mo), the modified film quality (molybdenum oxide film (MoO x ))、aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) and the results are shown in Table 2 according to Experimental Examples 1 to 22 and Comparative Experimental Examples 1 to 9.
[0072] First, for measurement, a molybdenum film (Mo) and an aluminum oxide film (AlO) were prepared by deposition using the CVD method in the same manner as in the semiconductor manufacturing process. x ) and silicon oxide film (SiO x ) wafer.
[0073] In addition, the surface of the molybdenum film (Mo) was heat treated at 500°C for 30 minutes to form a modified film (molybdenum oxide film (MoO x ))MoO x / Mo wafer.
[0074] Before etching, the thickness before etching was measured using a scanning electron microscope. Then, in a quartz stirring tank stirred at 300 rpm, the molybdenum film (Mo), the modified film (molybdenum oxide film (MoO x ))、aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) wafer and perform an etching process for 1 minute.
[0075] After etching is completed, it is washed with ultrapure water, and then the residual etching solution and moisture are completely dried using a drying device.
[0076] For the dried wafer specimens, the film thickness after etching was measured using a scanning electron microscope. The difference in film thickness before and after etching was calculated, and the thickness of the molybdenum film (Mo), the modified film (molybdenum oxide film (MoO x ))、aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) Etching amount for 1 minute.
[0077] <Evaluation Criteria>
[0078] Molybdenum film (Mo)
[0079] ◎: Etching rate above
[0080] ○: Etching rate is ~less than
[0081] △: Etching rate is ~less than
[0082] ×: Etching rate the following
[0083] Molybdenum oxide film (MoO x )
[0084] ◎: Etching rate above
[0085] ○: Etching rate is ~less than
[0086] *△: Etching rate is less than
[0087] ×: Etching rate the following
[0088] Alumina film (AlO x )
[0089] ◎: Etching rate is less than
[0090] ○: Etching rate is ~less than
[0091] △: Etching rate is ~less than
[0092] ×: Etching rate above
[0093] Silicon oxide film (SiO x )
[0094] ◎: Etching rate is less than
[0095] ○: Etching rate is ~less than
[0096] △: Etching rate is ~less than
[0097] ×: Etching rate above
[0098] [Table 2]
[0099]
[0100]
[0101]
[0102] As shown in Table 2, the results of Experimental Examples 1 to 22 show that the molybdenum film (Mo) and the modified film quality (molybdenum oxide film (MoO x )) while significantly suppressing the etching amount of aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) etching effect.
[0103] In contrast, the results of Comparative Experimental Examples 1 to 9 show that although the molybdenum film (Mo) and the modified film quality (molybdenum oxide film (MoO x )) but cannot significantly suppress the etching amount of the aluminum oxide film (AlO x ) and silicon oxide film (SiO x ) and therefore cannot be used as the etching solution of the present invention.
[0104] The specific parts of the invention of this application are described in detail above. For those skilled in the art, it is obvious that these specific technologies are only preferred embodiments and the scope of the invention is not limited thereby. Therefore, the actual scope of the invention of this application is defined by the claims and their equivalents.
Claims
1. An etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing the etching of an aluminum oxide film and a silicon oxide film, wherein: The etching solution composition comprises an inorganic acid, an oxidant, a fluorine compound, a pH adjuster, an additive, and water.
2. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: Relative to the total weight of the composition, the etching solution composition consists of 0.1 to 10 wt % of an inorganic acid, 0.001 to 5 wt % of an oxidant, 0.001 to 3 wt % of a fluorine compound, 2 to 4 wt % of a pH adjuster, 0.0001 to 2 wt % of an additive, and the balance of water.
3. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: The inorganic acid is any one selected from the group consisting of sulfuric acid, phosphoric acid, polyphosphoric acid, hydrochloric acid, p-toluenesulfonic acid, and a mixture thereof.
4. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: The oxidant is any one selected from the group consisting of hydrogen peroxide, nitric acid, ammonium nitrate, ammonium phosphate, ammonium persulfate, periodic acid, urea-hydrogen peroxide, tert-butyl hydroperoxide and 2-butane peroxide.
5. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: The fluorine compound is any one selected from the group consisting of hydrofluoric acid, ammonium fluoride, tetrafluoroboric acid and hexafluorosilicate.
6. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: The pH adjuster is selected from the group consisting of phosphates and sulfates.
7. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 1, characterized in that: The additive is a compound represented by the following chemical formula 1, [Chemical formula 1] F(CF2CF2) x CH2CH2OH In the above Chemical Formula 1, x is a natural number ranging from 1 to 10.
8. The etching solution composition for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 7, characterized in that: In the case where the additive is a compound represented by the Chemical Formula 1, x is an integer ranging from 3 to 7.
9. An etching method for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film, wherein: The method uses the etching solution composition according to any one of claims 1 to 8.
10. The etching method for etching a molybdenum film and a modified molybdenum film while suppressing etching of an aluminum oxide film and a silicon oxide film according to claim 9, characterized in that: The etching rate of molybdenum film is Above, the etching rate of molybdenum oxide film is Above, the etching rate of aluminum oxide film is less than The etching rate of silicon oxide film is less than