Processing method of titanium target material

The titanium target is gradually milled with specific tools and parameters, which solves the problem of the stress layer on the surface of the titanium target and achieves normal use and efficient processing during the sputtering process.

CN118751973APending Publication Date: 2024-10-11HEFEI FENGKE JINGSHENG ELECTRONIC MATERIALS CO LTD

Patent Information

Application Number
CN202410811752.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The stress layer formed during the machining process of the titanium target affects its use on the sputtering machine and leads to abnormal discharge phenomena. Existing technology cannot effectively solve this problem.

Method used

Use specific tools (R245, D20, R3.5) to gradually mill the welding surface, sputtering surface, outline and R angle of the titanium target. The specific steps include the first milling process, the second milling process, and the outline. Milling and R-angle milling, reduce residual stress by adjusting tool models and parameters.

Benefits of technology

The treated titanium target surface has small residual stress, high flatness, and small deformation. It can be used normally during the sputtering process and is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a processing method of a titanium target material. The processing method comprises the following steps: (1) carrying out first milling treatment on a welding surface of the titanium target material by adopting an R245 cutter; (2) carrying out second milling treatment on the sputtering surface of the titanium target treated in the step (1) by adopting an R245 cutter; (3) milling the outline of the titanium target material treated in the step (2) by adopting a D20 cutter; and (4) the R angle of the titanium target treated in the step (3) is milled through an R3.5 cutter, and machining of the titanium target is completed. According to the machining method, the welding face, the sputtering face, the outline and the R angle of the titanium target material are sequentially treated and machined by adopting the specific tool and combining specific tool parameters, and the machined and treated titanium target material is small in surface residual stress, high in flatness, small in deformation quantity and suitable for large-scale popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target material processing, and in particular to a method for processing a titanium target material. Background Art

[0002] During the machining process of titanium targets, a stress layer will be formed on the surface due to the milling of the tool on the machining surface. This stress layer will affect the use of the target on the sputtering machine and cause abnormal discharge.

[0003] CN113458729A discloses a method for preparing a planar special-shaped titanium target assembly, which comprises the following steps: turning and threading the end face of the titanium target blank, processing the titanium target blank into a desired shape, and obtaining a titanium target material; processing a groove on the surface of a back plate, wherein the groove matches the shape of the titanium target material; assembling the titanium target material and the back plate, and sequentially performing sheath welding and hot isostatic pressing welding; and leveling the welded titanium target material and the back plate to obtain the planar special-shaped titanium target assembly. The titanium target assembly prepared by the preparation method has high dimensional accuracy, good target flatness, high welding bonding rate and bonding strength, and the welding structure is suitable for targets of different thickness designs.

[0004] CN113547334A discloses a polygonal target material and a processing method thereof, the processing method comprising the following steps: turning a thread on the welding surface of the target material, and turning a welding groove on the welding surface of the back plate; assembling the processed target material and the back plate and performing hot isostatic pressing welding to obtain a welding assembly; turning a groove on the back of the back plate of the welding assembly, and then sequentially performing external turning and external milling on the welding assembly to obtain a polygonal target material assembly. The method adopts the method of welding first and then external milling, which can avoid the problem of two millings in the traditional method, and reduce the milling amount by increasing the turning amount, thereby improving production efficiency; in the method, turning a groove on the back of the back plate after welding can correct the flatness of the deformed target material after welding, and the control of the turning thickness during external turning can avoid the target material residue at the weld position after turning; the method is easy to operate, has a high target material production qualification rate, uses less raw materials, and has a low cost.

[0005] CN115319163A discloses a mechanical processing method for a molybdenum alloy blank, which comprises: providing a molybdenum alloy blank; milling the surface of the molybdenum alloy blank using a machining tool; the machining tool comprises a blade of grade 1010 or a tungsten steel end mill. The mechanical processing method for the molybdenum alloy blank can avoid the generation of an alloy layer on the surface of the molybdenum alloy blank after milling, which causes abnormal internal structure of the material after hot isostatic pressing, by selecting a specific tool; by optimizing the machining parameters during the machining process, the machined molybdenum alloy blank can meet the material performance requirements after sintering.

[0006] However, the above methods still fail to effectively solve the residual stress on the target surface, which often leads to abnormalities in the target during the sputtering process. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for processing a titanium target material. By adopting a specific tool and sequentially processing the tool parameters to process the welding surface, sputtering surface, outer contour and R angle of the titanium target material, the residual stress on the surface of the titanium target material is solved, thereby ensuring the normal use of the titanium target material.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for processing a titanium target material, the processing method comprising the following steps:

[0010] (1) The first milling process is performed on the welding surface of the titanium target using an R245 tool;

[0011] (2) performing a second milling process on the sputtering surface of the titanium target material processed in step (1) using an R245 tool;

[0012] (3) milling the outer contour of the titanium target material processed in step (2) using a D20 tool;

[0013] (4) Use an R3.5 tool to mill the R angle of the titanium target material processed in step (3) to complete the processing of the titanium target material.

[0014] The titanium target material processing method of the present invention uses an R245 tool to mill the welding surface and sputtering surface of the titanium target material, then uses a D20 tool to mill the outer contour of the titanium target material, and finally uses an R3.5 tool to mill the R angle of the titanium target material. The titanium target material surface after processing has small residual stress, high flatness, and small deformation, and can be used normally during the sputtering process. In the processing method of the present invention, when the tool used in each step is changed, the titanium target material processing effect will be deteriorated, the flatness will be reduced, and the residual stress will be large, which will cause the target material to be abnormal during the sputtering process.

[0015] Preferably, in the first milling process of step (1), the cutter disc is equipped with 8 to 10 blades, for example, 8, 9 or 10 blades.

[0016] The first milling processing tool model of the present invention is 12T3K-MM2030+Santak.

[0017] Preferably, the tool speed of the first milling process in step (1) is 200-240 r / min, for example, it can be 200 r / min, 205 r / min, 210 r / min, 220 r / min, 225 r / min, 230 r / min, 235 r / min or 240 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the feed rate of the first milling process in step (1) is 500-700 mm / min, for example, it can be 500 mm / min, 550 mm / min, 580 mm / min, 600 mm / min, 650 mm / min, 670 mm / min or 700 mm / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, in the second milling process of step (2), the cutter disc is equipped with 3 to 5 blades, for example, 3, 4 or 5 blades.

[0020] The second milling tool model of the present invention is 12T3K-MM2030+Santak.

[0021] Preferably, in step (2), the tool speed of the second milling process is 200-240 r / min, for example, it can be 200 r / min, 205 r / min, 210 r / min, 215 r / min, 220 r / min, 225 r / min, 230 r / min or 240 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the feed rate of the second milling process in step (2) is 100-200 mm / min, for example, it can be 100 mm / min, 105 mm / min, 130 mm / min, 150 mm / min, 170 mm / min, 190 mm / min or 200 mm / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the tool speed of the outer contour of the titanium target material after milling step (2) is 1700-1900r / min, for example, it can be 1700r / min, 1750r / min, 1800r / min, 1850r / min, 1880r / min or 1900r / min, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the feed rate is 900-1100mm / min, for example, it can be 900mm / min, 950mm / min, 1000mm / min, 1050mm / min, 1070mm / min or 1100mm / min, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] The model of the tool used to mill the outer contour of the titanium target material after the milling step (2) in the present invention is tungsten steel + Siemens.

[0025] Preferably, the tool speed of the R angle of the titanium target material after the milling step (3) is 2500-3000 r / min, for example, it can be 2500 r / min, 2600 r / min, 2700 r / min, 2800 r / min, 2900 r / min, 2950 r / min or 3000 r / min, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the feed rate is 900-1000 mm / min, for example, it can be 900 mm / min, 910 mm / min, 930 mm / min, 950 mm / min, 970 mm / min, 990 mm / min or 1000 mm / min, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] The tool model of the R angle of the titanium target material after milling step (3) in the present invention is R3.5*75*D10MM+Santa, which means that the tool inner diameter is 3.5mm, the length is 75mm, and the diameter is 10mm.

[0027] The present invention preferably sets the tool speed and feed rate in the first milling process, the second milling process, the outer contour of the titanium target material after milling step (2), and the R angle of the titanium target material after milling step (3) within a specific range to ensure that the titanium target material after treatment has excellent performance. When the tool speed and feed rate are small, the milling effect is poor, and the titanium target material obtained finally has a large flatness and a large deformation; when the tool speed and feed rate are large, it is not conducive to the subsequent processing steps, and the titanium target material obtained finally has poor performance.

[0028] As a preferred technical solution of the present invention, the processing method comprises the following steps:

[0029] (1) using an R245 tool, model 12T3K-MM2030+Santak, to perform a first milling process on the welding surface of the titanium target material at a tool speed of 200 to 240 r / min and a feed rate of 500 to 700 mm / min; in the first milling process, the cutter head is equipped with 8 to 10 blades;

[0030] (2) using an R245 tool, model 12T3K-MM2030+Santak, to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 200 to 240 r / min and a feed rate of 100 to 200 mm / min; in the second milling process, the cutter head is equipped with 3 to 5 blades;

[0031] (3) using a D20 tool, model tungsten steel + Siemens, to mill the outer contour of the titanium target material processed in step (2) at a tool speed of 1700 to 1900 r / min and a feed rate of 900 to 1100 mm / min;

[0032] (4) Using an R3.5 tool, model R3.5*75*D10MM+Santak, the R angle of the titanium target material processed in step (3) is milled at a tool speed of 2500-3000 r / min and a feed rate of 900-1000 mm / min to complete the processing of the titanium target material.

[0033] Compared with the prior art, the present invention has at least the following beneficial effects:

[0034] (1) The titanium target material processing method provided by the present invention uses a specific tool and tool parameters to process the titanium target material, thereby ensuring the normal use of the titanium target material;

[0035] (2) The titanium target material processing method provided by the present invention adopts a specific tool speed and feed rate to process the titanium target material, which is simple to operate. The residual stress on the surface of the titanium target material after processing is small, the flatness is high, and the deformation is small, which is suitable for large-scale promotion. DETAILED DESCRIPTION

[0036] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0037] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0038] Example 1

[0039] This embodiment provides a method for processing a titanium target material, and the processing method comprises the following steps:

[0040] (1) using an R245 tool, model 12T3K-MM2030+Santak, to perform a first milling process on the welding surface of the titanium target material at a tool speed of 240 r / min and a feed rate of 600 mm / min; in the first milling process, the cutter head is equipped with 10 blades;

[0041] (2) using an R245 tool, model 12T3K-MM2030+Santak, to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 240 r / min and a feed rate of 200 mm / min; in the second milling process, the cutter head is equipped with 3 blades;

[0042] (3) using a D20 tool, model tungsten steel + Siemens, at a tool speed of 1800 r / min and a feed rate of 1000 mm / min to mill the outer contour of the titanium target material processed in step (2);

[0043] (4) Using an R3.5 tool, model R3.5*75*D10MM+Santak, the R angle of the titanium target material processed in step (3) was milled at a tool speed of 3000 r / min and a feed rate of 1000 mm / min to complete the processing of the titanium target material.

[0044] Example 2

[0045] This embodiment provides a method for processing a titanium target material, and the processing method comprises the following steps:

[0046] (1) using an R245 tool, model 12T3K-MM2030+Santak, to perform a first milling process on the welding surface of the titanium target at a tool speed of 220 r / min and a feed rate of 580 mm / min; in the first milling process, the cutter head is equipped with 8 blades;

[0047] (2) using an R245 tool, model 12T3K-MM2030+Santak, to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 230 r / min and a feed rate of 170 mm / min; in the second milling process, the cutter head is equipped with 4 blades;

[0048] (3) using a D20 tool, model tungsten steel + Siemens, at a tool speed of 1750 r / min and a feed rate of 950 mm / min to mill the outer contour of the titanium target material processed in step (2);

[0049] (4) Using an R3.5 tool, model R3.5*75*D10MM+Santak, the R angle of the titanium target material processed in step (3) was milled at a tool speed of 2700 r / min and a feed rate of 930 mm / min to complete the processing of the titanium target material.

[0050] Example 3

[0051] This embodiment provides a method for processing a titanium target material, and the processing method comprises the following steps:

[0052] (1) using an R245 tool, model 12T3K-MM2030+Santak, to perform a first milling process on the welding surface of the titanium target material at a tool speed of 200 r / min and a feed rate of 500 mm / min; in the first milling process, the cutter head is equipped with 9 blades;

[0053] (2) using an R245 tool, model 12T3K-MM2030+Santak, to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 200 r / min and a feed rate of 100 mm / min; in the second milling process, the cutter head is equipped with 4 blades;

[0054] (3) using a D20 tool, model tungsten steel + Siemens, at a tool speed of 1750 r / min and a feed rate of 1100 mm / min to mill the outer contour of the titanium target material processed in step (2);

[0055] (4) Using an R3.5 tool, model R3.5*75*D10MM+Santak, the R angle of the titanium target material processed in step (3) was milled at a tool speed of 2500 r / min and a feed rate of 900 mm / min to complete the processing of the titanium target material.

[0056] Example 4

[0057] This embodiment provides a method for processing a titanium target material, and the processing method comprises the following steps:

[0058] (1) using an R245 tool, model 12T3K-MM2030+Santak, to perform a first milling process on the welding surface of the titanium target with a tool speed of 230 r / min and a feed rate of 700 mm / min; in the first milling process, the cutter head is equipped with 8 blades;

[0059] (2) using an R245 tool, model 12T3K-MM2030+Santak, to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 210 r / min and a feed rate of 190 mm / min; in the second milling process, the cutter head is equipped with 5 blades;

[0060] (3) using a D20 tool, model tungsten steel + Siemens, at a tool speed of 1900 r / min and a feed rate of 900 mm / min to mill the outer contour of the titanium target material processed in step (2);

[0061] (4) Using an R3.5 tool, model R3.5*75*D10MM+Santak, the R angle of the titanium target material processed in step (3) was milled at a tool speed of 2800 r / min and a feed rate of 9600 mm / min to complete the processing of the titanium target material.

[0062] Example 5

[0063] This embodiment provides a method for processing a titanium target material. The processing method is the same as that of Embodiment 1 except that the rotation speed of the first milling process in step (1) is 180 r / min.

[0064] Example 6

[0065] This embodiment provides a method for processing a titanium target material. The processing method is the same as that of Embodiment 1 except that the rotation speed of the first milling process in step (1) is 260 r / min.

[0066] Example 7

[0067] This embodiment provides a method for processing a titanium target material. The processing method is the same as that of Embodiment 1 except that the feed rate of the second milling process in step (2) is 80 mm / min.

[0068] Example 8

[0069] This embodiment provides a method for processing a titanium target material. The processing method is the same as that of Embodiment 1 except that the feed rate of the second milling process in step (2) is 220 mm / min.

[0070] Comparative Example 1

[0071] This comparative example provides a method for processing a titanium target material. The processing method is the same as that of Example 1 except that a D20 tool is used in the first milling process in step (1).

[0072] Comparative Example 2

[0073] This comparative example provides a method for processing a titanium target material. The processing method is the same as that of Example 1 except that in step (3), an R3.5 tool is used to mill the outer contour of the titanium target material processed in step (2).

[0074] The flatness and deformation of the titanium targets after processing in the above embodiments and comparative examples were measured, and the results are shown in Table 1.

[0075] Table 1

[0076] Flatness / mm Deformation / mm Example 1 0.1 0.05 Example 2 0.15 0.04 Example 3 0.13 0.02 Example 4 0.2 0.05 Example 5 0.5 0.25 Example 6 0.8 0.45 Example 7 0.85 0.39 Example 8 0.76 0.36 Comparative Example 1 0.02 0.01 Comparative Example 2 0.03 0.02

[0077] From Table 1 we can see that:

[0078] (1) Based on Examples 1 to 4, it can be seen that the titanium target material processing method provided by the present invention is simple to operate, and the residual stress on the surface of the titanium target material after processing is small, the flatness is high and the deformation is small, which is suitable for large-scale promotion;

[0079] (2) It can be seen from the combination of Example 1 and Examples 5 to 6 that the rotation speed of the first milling process in Example 5 is relatively low, and the rotation speed of the first milling process in Example 6 is relatively high, both of which lead to an increase in the flatness of the titanium target after processing, but also an increase in the deformation, which affects the normal use of the titanium target during the sputtering process;

[0080] (3) It can be seen from the combination of Example 1 and Examples 7 to 8 that the feed amount of the second milling process in Example 7 is relatively small, and the feed amount of the second milling process in Example 8 is relatively large, both of which result in a relatively small flatness and an increased deformation of the titanium target after processing, affecting the normal use of the titanium target during the sputtering process;

[0081] (4) It can be seen from Example 1 and Comparative Examples 1 to 2 that the first milling process in Comparative Example 1 uses a D20 tool, and the contour of the titanium target after processing in Comparative Example 2 uses an R3.5 tool, both of which result in a smaller flatness of the titanium target after processing, affecting the normal use of the titanium target during the sputtering process.

[0082] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for processing a titanium target, characterized in that: The processing method comprises the following steps: (1) The first milling process is performed on the welding surface of the titanium target using an R245 tool; (2) performing a second milling process on the sputtering surface of the titanium target material processed in step (1) using an R245 tool; (3) milling the outer contour of the titanium target material processed in step (2) using a D20 tool; (4) Use an R3.5 tool to mill the R angle of the titanium target material processed in step (3) to complete the processing of the titanium target material.

2. The processing method according to claim 1, characterized in that: Step (1) In the first milling process, the cutter disc is equipped with 8 to 10 blades.

3. The processing method according to claim 1 or 2, characterized in that: In step (1), the tool speed of the first milling process is 200 to 240 r / min.

4. The processing method according to any one of claims 1 to 3, characterized in that: The feed rate of the first milling process in step (1) is 500-700 mm / min.

5. The processing method according to any one of claims 1 to 4, characterized in that: Step (2) In the second milling process, the cutter disc is equipped with 3 to 5 blades.

6. The processing method according to any one of claims 1 to 5, characterized in that: Step (2) The tool speed of the second milling process is 200-240 r / min.

7. The processing method according to any one of claims 1 to 6, characterized in that: Step (2) The feed rate of the second milling process is 100-200 mm / min.

8. The processing method according to any one of claims 1 to 7, characterized in that: The tool speed of the outer contour of the titanium target material processed in the milling step (2) is 1700-1900 r / min; the feed rate is 900-1100 mm / min.

9. The processing method according to any one of claims 1 to 8, characterized in that: The tool speed of the R angle of the titanium target material processed in the milling step (3) is 2500-3000 r / min; the feed rate is 900-1000 mm / min.

10. The processing method according to any one of claims 1 to 9, characterized in that: The processing method comprises the following steps: (1) using an R245 tool to perform a first milling process on the welding surface of the titanium target material at a tool speed of 200 to 240 r / min and a feed rate of 500 to 700 mm / min; in the first milling process, the cutter head is equipped with 8 to 10 blades; (2) using an R245 tool to perform a second milling process on the sputtering surface of the titanium target material treated in step (1) at a tool speed of 200 to 240 r / min and a feed rate of 100 to 200 mm / min; in the second milling process, the cutter head is equipped with 3 to 5 blades; (3) using a D20 tool, milling the outer contour of the titanium target material processed in step (2) at a tool speed of 1700 to 1900 r / min and a feed rate of 900 to 1100 mm / min; (4) Using an R3.5 tool, the R angle of the titanium target material processed in step (3) is milled at a tool speed of 2500 to 3000 r / min and a feed rate of 900 to 1000 mm / min to complete the processing of the titanium target material.

Citation Information

Patent Citations

  • Target material machining technology

    CN111299669A

  • Machining method for improving flatness of target material

    CN111889769A

  • Machining method for Quantum series target material

    CN113319342A

  • Long-life sputtering target material and preparation method therefor

    WO2024088252A1

Cited By

  • Machining method of titanium target

    CN119216640A

  • Machining method of molybdenum-niobium target material

    CN120055338A