Assembling and welding method for ship water diversion heel
During the ship's water heel assembly and welding process, the methods of prefabricated welding and butt welding, combined with the strategy of temporarily cutting the ship's outer plate, solved the installation and positioning problems during the loading and closing stage, achieved efficient water heel assembly and welding, and reduced rework and cost.
Patent Information
- Application Number
- CN202410889482.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
The existing ship water heel installation and welding method is difficult to ensure accurate installation and positioning during the loading and closing stage, resulting in frequent rework and high costs.
A new method of installation and welding is adopted. One section of the water heel is prefabricated and welded on the ship segment, and the other section of the water heel is welded and fixed after the two ship segments are docked. The outer plate of the ship is temporarily cut for positioning, closing and Welding to reduce the workload of steel plate groove creation and avoid accidental injuries caused by repeated groove creation and carbon planing root removal operations.
It reduces the difficulty of installation and positioning during the segmented loading and closing stage of the split heel, reduces rework and waste, improves the quality and efficiency of the assembly and welding process, and reduces construction costs.
Smart Images

Figure CN118752104A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of shipbuilding, and more particularly to a method for welding a ship watertight heel. Background Art
[0002] The watertight heel of a ship is a steel structure installed at the stern of a ship, and its main function is to ensure the navigation stability of the ship. For wide-body ships, due to their special structure, they are more likely to roll when sailing, so it is necessary to install a watertight heel to effectively divide the water flow on both sides of the hull, thereby improving its stability. Watertight heels generally have steel plate structures and box structures, among which the steel plate watertight heel structure is relatively simple and common. Compared with the ship plate structure of its perimeter, the plate thickness of the steel plate watertight heel structure is much larger, often more than 4 times the thickness of the ship plate of its perimeter, and the thickness can be ≥80mm. The modern shipbuilding model is basically to divide the construction into multiple sections first, and then gradually load and assemble the multiple sections to form a whole ship. According to the principle of ship section construction division and the distribution position of the watertight heel, the watertight heel is usually divided into different adjacent sections. This requires strict control of the welding accuracy and quality of the watertight heel segment prefabrication and loading and assembling stages, and a reasonable watertight heel welding method is particularly important.
[0003] The prior art is to divide the watertight heel into two parts, front and rear, according to the ship segment division diagram, and prefabricate them in advance with their respective segments. Figure 1-2 As shown, the watershed heel 1 is divided into a watershed heel segment I2 and a watershed heel segment II3. The watershed heel segment I2 is prefabricated on the ship segment I4, and the watershed heel segment II3 is prefabricated on the ship segment II5. Then, the front and rear segments are loaded and closed as a whole. The watershed heel is closed and welded to the seams and other structural closing seams during the loading and closing stage. In the existing watershed heel welding method, the watershed heel segment I2 and the watershed heel segment II3 are both completed in the segment prefabrication stage. When the two segments are loaded and closed, it is necessary to ensure that the center lines of the two segments are aligned, the height is flush, and the front and rear rib distances are equal. It is also necessary to consider whether the watershed heel is aligned, whether the gap exceeds the standard, etc. (many factors need to be considered). Once the watershed heel cannot be completely aligned in the loading and closing position or the gap exceeds the standard, the watershed heel needs to be partially disassembled and repositioned for welding, which is difficult to rework, has a long cycle, and has a high comprehensive construction cost.
[0004] Therefore, it is urgent to design a novel ship water separation heel welding method to solve the above-mentioned problems. Summary of the invention
[0005] The technical problem to be solved by the present invention is to address the above-mentioned shortcomings of the prior art. The purpose of the present invention is to provide a method for welding a watertight heel of a ship, which can reduce the difficulty of installation and positioning during the loading and closure stage of sections with watertight heels, reduce related rework and waste, and ensure that the quality and efficiency of the welding process of the watertight heel of the ship are improved.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a method for assembling and welding a watertight heel of a ship, wherein one section of the watertight heel is prefabricated and welded to one section of the ship segment to form a whole, and the other section of the watertight heel is butt-welded to one section of the watertight heel after the two sections of the ship segment are butt-jointed, and finally the other section of the watertight heel is welded and fixed to the other section of the ship segment.
[0007] Furthermore, the method comprises the following steps:
[0008] S1, cutting and processing the watershed heel according to the nodes to obtain watershed heel segment I and watershed heel segment II;
[0009] S2, prefabricate and weld the water-cutting heel section I onto the ship section I;
[0010] S3, temporarily cutting and shifting the outer plates of the ship corresponding to the ship section II on both sides of the location of the watertight heel section II, to obtain the temporary left outer plate of section II and the temporary right outer plate of section II;
[0011] S4, positioning and closing the ship section I in step S2 and the ship section II in step S3, and temporarily reinforcing them;
[0012] S5. Position and install the water-dividing heel segment II on the water-dividing heel segment I, and weld it firmly;
[0013] S6, performing nondestructive testing on the weld between the water heel section II and the water heel section I. After the test is qualified, proceed to step S7;
[0014] S7, move the temporary left outer plate of section II and the temporary right outer plate of section II in step S3 back to the ship section II on both sides of the location of the watertight heel section II, and weld them firmly;
[0015] S8. Weld the welds between the watertight heel section II and the temporary left outer plate of section II, the temporary right outer plate of section II, and the middle longitudinal plate;
[0016] S9. Welding of the welds corresponding to the joints of ship sections I and II;
[0017] S10. Welding of the internal structure of the joint of ship section I and ship section II and other remaining welds.
[0018] Further, the step S2 includes butt welding of the watertight heel section I and the center longitudinal plate and welding of the watertight heel section I and the ship outer plate of the ship section I, wherein:
[0019] The specific operation of the butt welding of the watershed heel segment I and the middle longitudinal plate is as follows: a single-sided groove is provided on the butt end face of the watershed heel segment I, a gap is left when the watershed heel segment I and the middle longitudinal plate are butt-jointed so that a first butt weld is formed with the single-sided groove, a ceramic liner is attached to the back of the first butt weld away from the single-sided groove after butt-jointing, and finally the first butt weld is welded;
[0020] The specific operation of welding the watertight heel section I with the ship outer plate of the ship section I is as follows: a downwardly arranged single-sided groove is provided on the butt joint end faces of the left outer plate of section I and the right outer plate of section I corresponding to the ship outer plate of the ship section I, a gap is left when the watertight heel section I is butt jointed with the left outer plate of section I and the right outer plate of section I so that a second butt weld is formed with the single-sided groove, and finally the second butt weld is welded.
[0021] Furthermore, the gap left when the watertight heel segment I is butt-jointed with the middle longitudinal plate, and the gap left when the watertight heel segment I is butt-jointed with the left outer plate of segment I and the right outer plate of segment I are both 4mm-8mm; the single-sided groove angle corresponding to the watertight heel segment I is 30±5°, and the single-sided groove angle corresponding to the left outer plate of segment I and the right outer plate of segment I is 45°.
[0022] Furthermore, the specific operations of step S5 are:
[0023] Symmetrical grooves are opened on both sides of the end face of the watershed heel segment II to form a symmetrical weld, and the end face of the watershed heel segment II is butted against the end face of the watershed heel segment I without a gap, and the symmetrical weld is welded.
[0024] Furthermore, the symmetrical groove angle corresponding to the watershed heel segment II is 45±5° 。
[0025] Furthermore, the specific operations of step S7 are:
[0026] Single-sided grooves are provided on the butt joint end faces of the temporary left outer plate of section II, the temporary right outer plate of section II and the ship outer plate of ship section II. When the temporary left outer plate of section II, the temporary right outer plate of section II and the ship outer plate of ship section II are butt jointed, gaps are left to form a fifth butt weld with the single-sided groove. After butt joint, a ceramic gasket is attached to the back of the fifth butt weld away from the single-sided groove, and finally the fifth butt weld is welded.
[0027] Furthermore, a gap of 4mm-8mm is left when the temporary left outer plate of section II, the temporary right outer plate of section II and the ship outer plate of ship section II are butt-jointed, and an angle of the fifth butt weld is 40±5°.
[0028] Furthermore, the step S8 includes butt welding of the watertight heel segment II and the middle longitudinal plate and welding of the watertight heel segment II and the temporary left outer plate of segment II and the temporary right outer plate of segment II, wherein:
[0029] The specific operation of the butt welding between the watershed heel segment II and the middle longitudinal plate is as follows: a single-sided groove is provided on the butt end face of the watershed heel segment II, a gap is left when the watershed heel segment II and the middle longitudinal plate are butt-jointed so that a third butt weld is formed with the single-sided groove, a ceramic liner is attached to the back of the third butt weld away from the single-sided groove after butt-jointing, and finally the third butt weld is welded;
[0030] A single-sided groove arranged upward is opened on the butt joint end faces of the temporary left outer plate of Section II and the temporary right outer plate of Section II. When the watershed heel Section II is butt jointed with the temporary left outer plate of Section II and the temporary right outer plate of Section II, a gap is left so that it forms a fourth butt weld with the single-sided groove, and finally the fourth butt weld is welded.
[0031] Furthermore, the gap left when the watertight heel segment II is butt-jointed with the middle longitudinal plate, and the gap left between the watertight heel segment II and the temporary left outer plate of segment II and the temporary right outer plate of segment II are all 4mm-8mm; the single-sided groove angle corresponding to the watertight heel segment II is 30±5°, and the single-sided groove angle corresponding to the temporary left outer plate of segment II and the temporary right outer plate of segment II is 30±5°.
[0032] Beneficial Effects
[0033] Compared with the prior art, the present invention has the following advantages:
[0034] 1. The assembly and welding method of the present invention prefabricates and installs one section of the watershed heel, and welds and fixes the other section of the watershed heel after the two sections of the ship are butt-jointed. The method of bulk assembly and welding of the other section of the watershed heel can reduce the difficulty of installation and positioning during the loading and closing stage of the sections with the watershed heel, reduce related rework and waste, and ensure that the quality and efficiency of the ship watershed heel assembly and welding process are improved.
[0035] 2. The welding method of the present invention optimizes the welding nodes and welding timing of the watershed heel, temporarily cuts and shifts some segmented outer plates, reduces the workload of opening the steel plate groove in the watershed heel area, avoids repeated opening of grooves during the welding process, prevents accidental damage to the opposite groove surface during repeated opening of grooves, avoids carbon planing and related grinding work in a small space, reduces the difficulty of welding operation, and improves the welding quality and welding efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a longitudinal cross-sectional view of the water heel region in the prior art;
[0037] Figure 2It is a cross-sectional view of the closing position in the prior art;
[0038] Figure 3 A longitudinal cross-sectional view of the water heel region of the present invention;
[0039] Figure 4 for Figure 3 Schematic diagram of the cross-sectional structure of AA;
[0040] Figure 5 for Figure 3 Schematic diagram of the cross-sectional structure of the middle BB;
[0041] Figure 6 for Figure 3 Schematic diagram of the cross-sectional structure of the CC;
[0042] Figure 7 for Figure 3 Schematic diagram of the cross-sectional structure of the middle DD;
[0043] Figure 8 It is a schematic diagram of the structure when two water-dividing heels are butt-jointed in the present invention;
[0044] Fig. 9 It is a schematic diagram of the structure of temporarily cutting and shifting the outer plate of a ship in the present invention;
[0045] Fig.10 It is a schematic diagram of the structure when the temporary right outer plate of Section II in the present invention is butted against the outer plate of the ship;
[0046] Fig.11 It is a welding flow chart of the present invention.
[0047] Among them: 1-water divider, 2-water divider section I, 3-water divider section II, 4-ship section I, 5-ship section II, 6-temporary left outer plate of section II, 7-temporary right outer plate of section II, 8-middle longitudinal plate, 9-first butt weld, 10-ceramic liner, 11-ship outer plate, 12-left outer plate of section I, 13-temporary right outer plate of section I, 14-second butt weld, 15-third butt weld, 16-fourth butt weld, 17-symmetric weld, 18-fifth butt weld. DETAILED DESCRIPTION
[0048] The present invention will be further described below with reference to the specific embodiments in the accompanying drawings.
[0049] A method for assembling and welding a ship watertight heel comprises the following steps: prefabricating and welding one section of the watertight heel and one section of the ship segment to form a whole; butting the other section of the watertight heel against the two sections of the ship segment and then butting and welding the other section of the watertight heel on one section of the watertight heel; and finally, welding and fixing the other section of the watertight heel to the other section of the ship segment.
[0050] The assembly and welding method of the present invention prefabricates and installs one section of the watershed heel, and welds and fixes the other section of the watershed heel after the two sections of the ship are butt-jointed. The method adopts a bulk assembly and welding method for the other section of the watershed heel, which can reduce the difficulty of installation and positioning during the loading and closing stage of the sections with the watershed heel, reduce related rework and waste, and ensure that the quality and efficiency of the ship watershed heel assembly and welding process are improved.
[0051] like Figure 3-11 As shown, in this embodiment, the water cutter 1 is divided into two water cutter segments, which are respectively installed in two ship segments. The method includes the following steps:
[0052] S1, cut and process the watershed heel 1 according to the nodes to obtain watershed heel segment I2 and watershed heel segment II3;
[0053] S2, prefabricate and weld the water-break heel section I2 onto the ship section I4 to form a whole, which is convenient for subsequent assembly and closure;
[0054] S3, the ship outer plates 11 corresponding to the ship sections II5 on both sides of the location of the watershed heel section II3 are temporarily cut and displaced locally to obtain the temporary left outer plate 6 of the section II and the temporary right outer plate 7 of the section II; as shown in the figure, the ship outer plates 11 on both sides of the location of the watershed heel section II3 are temporarily cut and displaced to avoid the welding of the watershed heel section II3 in a narrow space, reduce labor intensity, improve welding quality, and achieve that the butt joint of the watershed heel section II3 is not hindered by the ship outer plate 11 of the ship section II5 when passing through the ship outer plate 11 area, and can be continuously welded from bottom to top, avoiding frequent arc extinction and arc starting (a large number of joints) when passing through the ship outer plate 11 area, thereby improving welding quality and efficiency; and without the obstruction of the ship outer plate 11 of the ship section II5, the welding sight is wider, and at the same time, it is also avoided that the gap between the ship outer plate 11 and the watershed heel section II3 is too large, which leads to the quality accident of partially cutting and replacing the outer plate;
[0055] S4, positioning and closing the ship section I4 in step S2 and the ship section II5 in step S3, and temporarily reinforcing them; specifically, when the two ship sections are loaded and closed, the center lines of the two ship sections are first aligned, the heights are flush, and the distances between the front and rear ribs are equal. Then, the positions of the ship sections I4 and II5 can be positioned by means of pads, etc., to ensure that the closing of the two ship sections meets the design standards;
[0056] S5, positioning and installing the watershed heel segment II3 on the watershed heel segment I2, and welding them firmly; specifically, aligning the watershed heel segment II3 with the watershed heel segment I2, and adjusting the gap (few factors need to be considered, low positioning difficulty, high positioning efficiency), the way of positioning and installing the two watershed heel segments separately can avoid the watershed heel not being able to be completely aligned or the gap exceeding the standard in the loading and closing position, and there is no need to partially disassemble the watershed heel for re-positioning and welding, which has low construction difficulty, short period, and low comprehensive construction cost;
[0057] S6, perform nondestructive testing on the weld between the watertight heel section II3 and the watertight heel section I2. After the test is qualified, proceed to step S7 to ensure the welding quality. At the same time, since there is no obstruction from the ship outer plate 11 of the ship section II5, the test is more convenient and the test accuracy can be guaranteed;
[0058] S7, move the temporary left outer plate 6 of section II and the temporary right outer plate 7 of section II in step S3 back to the ship section II5 on both sides of the location of the watertight heel section II3, and weld them firmly to ensure the sealing of the ship;
[0059] S8, welding the welds between the watershed heel segment II3 and the segment II temporary left outer plate 6, the segment II temporary right outer plate 7, and the middle longitudinal plate 8 to achieve installation and fixation of the watershed heel segment II3;
[0060] S9, welding the welds corresponding to the closing joints of ship section I4 and ship section II5 to achieve welding and fixing of the two ship sections;
[0061] S10, welding the internal structure of the closing joint of ship section I4 and ship section II5 and other remaining welds, such as: welding the position of the slow welding zone of the butt weld of the closing joint of the outer plate, etc., to complete the welding work of the ship's watertight heel.
[0062] Preferably, step S2 includes butt welding the watertight heel section I2 and the center longitudinal plate 8 and welding the watertight heel section I2 and the ship outer plate 11 of the ship section I4, wherein:
[0063] like Figure 4As shown, it is a node diagram of the butt joint between the watershed heel segment I2 and the middle longitudinal plate 8. The specific operation of the butt welding between the watershed heel segment I2 and the middle longitudinal plate 8 is: a single-sided groove is opened on the butt end face of the watershed heel segment I2, and a gap is left when the watershed heel segment I2 and the middle longitudinal plate 8 are butt jointed so that a first butt weld 9 is formed with the single-sided groove. After butt joint, a ceramic liner 10 is attached to the back of the first butt weld 9 away from the single-sided groove, and finally the first butt weld 9 is welded. In this welding process, only the watershed heel is grooved, and the middle longitudinal plate 8 at the corresponding position does not need to be grooved. The groove opening The workload is small. During the stage of positioning and welding of the water divider, it is often necessary to trim and cut the allowance to adjust the position. At this time, only the allowance cutting is required for the middle longitudinal plate without a groove, and there is no need to open a groove. The cutting flame will not be aimed at the water divider, and it is not easy to accidentally damage the groove surface and the beveled area. The construction process is simple, the construction quality is good, and the efficiency is high. In addition, a single-sided and single-sided groove with a gap is used to ensure full penetration welding of the welding node without root cleaning. There is no need for carbon arc air planing and root cleaning + grinding during welding. The noise and dust pollution during the construction process are small, which is beneficial to health and environmental protection, and the labor intensity is low.
[0064] like Figure 5 As shown, it is a node diagram of the watershed heel segment I2 butting with the middle longitudinal plate 8 and the ship outer plate 11. The specific operation of welding the watershed heel segment I2 with the ship outer plate 11 of the ship segment I4 is as follows: a single-sided groove arranged downward is provided on the butting end faces of the left outer plate 12 of the segment I and the right outer plate 13 of the segment I corresponding to the ship outer plate 11 of the ship segment I4. When the watershed heel segment I2 butts with the left outer plate 12 of the segment I and the right outer plate 13 of the segment I, a gap is left to form a second butt weld 14 with the single-sided groove, and finally the second butt weld 14 is welded. In this welding process, a single-sided groove is arranged downward. Since this node is welded in the segment production stage, the segment in this area is generally reverse-built with the platform as the base surface or horizontally built with the bow transverse wall as the base surface, and the groove is facing downward for easy welding construction.
[0065] Preferably, the gap left when the watershed heel segment I2 is butt-jointed with the middle longitudinal plate 8, and the gap left when the watershed heel segment I2 is butt-jointed with the left outer plate 12 of segment I and the right outer plate 13 of segment I are both 4mm-8mm; the single-sided groove angle corresponding to the watershed heel segment I2 is 30±5°, and the single-sided groove angle corresponding to the left outer plate 12 of segment I and the right outer plate 13 of segment I is 45°. The gap and groove angle are reasonably optimized to facilitate welding and further improve the welding quality.
[0066] Preferably, Figure 8 As shown, it is a node diagram for docking the watershed heel segment I2 and the watershed heel segment II3. The specific operation of step S5 is:
[0067] Symmetrical grooves are provided on both sides of the end face of the watershed heel segment II3 to form symmetrical welds 17 , and the end face of the watershed heel segment II3 is butted against the end face of the watershed heel segment I2 without any gap, and the symmetrical welds 17 are welded.
[0068] In this embodiment, since the joints of the watershed heel segment I2 and the watershed heel segment II3 are both of original thickness, the thickness is large. When single-sided single-sided groove welding with a gap is adopted, the asymmetry of the weld shape is seriously amplified, and the welding stress and welding deformation are difficult to control. In addition, increasing the root gap will greatly increase the cross-sectional area of the weld, the welding filling amount will greatly increase, the welding material and labor costs will increase significantly, and the welding stress and deformation will also increase. At the same time, in order to reduce the workload of the groove opening of the watershed heel and realize the flushing of the bow end of the watershed heel segment I2 and the bow end of the ship outer plate 11, a single-sided double-sided groove welding method without a gap is adopted to facilitate the welding construction of the watershed heel to the joint.
[0069] Preferably, the symmetrical groove angle corresponding to the water break heel segment II3 is 45±5°, and the groove angle is reasonably optimized to facilitate welding and further improve the welding quality.
[0070] Preferably, Fig.10 As shown, it is a docking node diagram when the temporary left outer plate 6 of segment II and the temporary right outer plate 7 of segment II are moved back. The specific operation of step S7 is:
[0071] Single-sided grooves are provided on the butt joint end faces of the temporary left outer plate 6 of section II, the temporary right outer plate 7 of section II, and the ship outer plate 11 of ship section II5. When the temporary left outer plate 6 of section II, the temporary right outer plate 7 of section II, and the ship outer plate 11 of ship section II5 are butt jointed, gaps are left to form a fifth butt weld 18 with the single-sided groove. After butt jointing, a ceramic liner 10 is attached to the back of the fifth butt weld 18 away from the single-sided groove, and finally the fifth butt weld 18 is welded. The single-sided welding and double-sided forming welding process method with a ceramic liner attached to the root can further improve the welding quality.
[0072] Furthermore, the gap between the temporary left outer plate 6 of section II, the temporary right outer plate 7 of section II and the ship outer plate 11 of ship section II5 is 4mm-8mm, and the angle of the fifth butt weld 18 is 40±5°. Reasonable optimization of the gap and groove angle can facilitate welding and further improve the welding quality.
[0073] Preferably, Figure 6 As shown, it is a node diagram when the watershed heel segment II3 is butted with the middle longitudinal plate 8, the temporary left outer plate 6 of segment II, and the temporary right outer plate 7 of segment II. Step S8 includes butt welding of the watershed heel segment II3 and the middle longitudinal plate 8 and welding of the watershed heel segment II3 and the temporary left outer plate 6 of segment II and the temporary right outer plate 7 of segment II, wherein:
[0074] The specific operation of the butt welding between the watershed heel segment II3 and the middle longitudinal plate 8 is as follows: the middle longitudinal plate 8 and the remainder at the corresponding position of the watershed heel segment II3 are cut, a single-sided groove is opened on the butt end face of the watershed heel segment II3, a gap is left when the watershed heel segment II3 is butt-jointed with the middle longitudinal plate 8 so that it forms a third butt weld 15 with the single-sided groove, a ceramic liner 10 is attached to the back of the third butt weld 15 away from the side of the single-sided groove after butt-jointing, and finally the third butt weld 15 is welded; in this welding process, only the watershed heel is grooved, and the middle longitudinal plate 8 at the corresponding position does not need to be grooved The workload of opening the groove is small. During the stage of welding and positioning of the water divider, it is often necessary to trim the allowance and adjust the position. At this time, only the allowance cutting of the middle longitudinal plate without the groove is required, and there is no need to open the groove. The cutting flame will not be aimed at the water divider, and it is not easy to accidentally damage its groove surface and the beveled area. The construction process is simple, the construction quality is good, and the efficiency is high. In addition, a single-sided and single-sided groove with a gap is used to avoid root cleaning and fully penetrate the welding node. There is no need for carbon arc air planing root cleaning + grinding during welding. The noise and dust pollution during the construction process are small, which is beneficial to health and environmental protection, and the labor intensity is low.
[0075] A single-sided groove arranged upward is provided on the butt end faces of the temporary left outer plate 6 of the segment II and the temporary right outer plate 7 of the segment II. When the watershed heel segment II3 is butt-jointed with the temporary left outer plate 6 of the segment II and the temporary right outer plate 7 of the segment II, a gap is left so that the watershed heel segment II3 and the temporary left outer plate 6 of the segment II and the temporary right outer plate 7 form a fourth butt weld 16 with the single-sided groove. Finally, the fourth butt weld 16 is welded. In this welding process, the grooves of the temporary left outer plate 6 of the segment II and the temporary right outer plate 7 of the segment II are arranged upward. Since the node is welded in the stage of segment loading and closing, the segment outer plates in this area are cut and bulked. During the welding construction, the segments are in an upright state, and the grooves are facing upward to facilitate the welding construction. Step S8 also includes symmetrically welding the vertical fillet welds between the watershed heel II3 and the transverse ribs.
[0076] Furthermore, the gap between the watershed heel segment II3 and the middle longitudinal plate 8, and the gap between the watershed heel segment II3 and the segment II temporary left outer plate 6 and the segment II temporary right outer plate 7 are all 4mm-8mm; the single-sided groove angle corresponding to the watershed heel segment II3 is 30±5°, and the single-sided groove angle corresponding to the segment II temporary left outer plate 6 and the segment II temporary right outer plate 7 is 30±5°. Reasonable optimization of the gap and groove angle can facilitate welding and further improve the welding quality.
[0077] The welding method in this embodiment optimizes the welding nodes and welding timing of the watershed heel, temporarily cuts and shifts some segmented outer plates, reduces the workload of opening the steel plate grooves in the watershed heel area, avoids repeated opening of grooves during the welding process, prevents accidental damage to the opposite groove surface during repeated opening of grooves, avoids carbon planing and related grinding work in a small space, reduces the difficulty of welding operations, and improves welding quality and efficiency.
[0078] The above are only preferred embodiments of the present invention. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the structure of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for welding a ship's watertight heel, characterized in that: The method comprises the following steps: prefabricating and welding one watertight heel and one ship section into a whole; butting the other watertight heel against the two ship sections and then butting and welding the other watertight heel on one of the watertight heels; and finally, welding and fixing the other watertight heel to the other ship section.
2. The method for welding a ship watertight heel according to claim 1, characterized in that: The method comprises the following steps: S1, cutting and processing the watershed heel (1) according to the nodes to obtain watershed heel segment I (2) and watershed heel segment II (3); S2, prefabricate and weld the water-cutting heel section I (2) onto the ship section I (4); S3, temporarily cutting and shifting the ship outer plate (11) corresponding to the ship section II (5) on both sides of the location of the watertight heel section II (3) to obtain a temporary left outer plate (6) for section II and a temporary right outer plate (7) for section II; S4, positioning and closing the ship section I (4) in step S2 and the ship section II (5) in step S3, and temporarily reinforcing them; S5. Position and install the water-distributing heel segment II (3) on the water-distributing heel segment I (2) and weld it firmly; S6, performing nondestructive testing on the weld between the water-break heel section II (3) and the water-break heel section I (2), and if the test is qualified, proceed to step S7; S7, move the temporary left outer plate (6) of section II and the temporary right outer plate (7) of section II in step S3 back to the ship section II (5) on both sides of the location of the watertight heel section II (3), and weld them firmly; S8, welding the welds between the watershed heel section II (3) and the temporary left outer plate (6) of section II, the temporary right outer plate (7) of section II, and the middle longitudinal plate (8); S9, welding the welds corresponding to the joints of ship section I (4) and ship section II (5); S10. Welding of the internal structure of the joint of ship section I (4) and ship section II (5) and other remaining welds.
3. The method for welding a ship watertight heel according to claim 2, characterized in that: The step S2 comprises butt welding of the cutter heel section I (2) and the center longitudinal plate (8) and welding of the cutter heel section I (2) and the ship outer plate (11) of the ship section I (4), wherein: The specific operation of the butt welding of the watershed heel segment I (2) and the middle longitudinal plate (8) is as follows: a single-sided groove is provided on the butt end face of the watershed heel segment I (2); a gap is left when the watershed heel segment I (2) and the middle longitudinal plate (8) are butt-jointed so that a first butt weld (9) is formed with the single-sided groove; after butt-jointing, a ceramic liner (10) is attached to the back of the first butt weld (9) on the side away from the single-sided groove; and finally, the first butt weld (9) is welded; The specific operation of welding the watertight heel section I (2) to the ship outer plate (11) of the ship section I (4) is as follows: a single-sided groove arranged downward is provided on the butt joint end faces of the left outer plate (12) of the section I and the right outer plate (13) of the section I corresponding to the ship outer plate (11) of the ship section I (4); when the watertight heel section I (2) is butt jointed with the left outer plate (12) of the section I and the right outer plate (13) of the section I, a gap is left so that a second butt joint weld (14) is formed with the single-sided groove; and finally the second butt joint weld (14) is welded.
4. The method for welding a ship watertight heel according to claim 3, characterized in that: The gap left when the watershed heel segment I (2) is butt-jointed with the middle longitudinal plate (8), and the gap left when the watershed heel segment I (2) is butt-jointed with the left outer plate (12) of segment I and the right outer plate (13) of segment I are both 4mm-8mm; the single-sided groove angle corresponding to the watershed heel segment I (2) is 30±5°, and the single-sided groove angle corresponding to the left outer plate (12) of segment I and the right outer plate (13) of segment I is 45°.
5. The method for welding a ship watertight heel according to claim 2, characterized in that: The specific operation of step S5 is: Symmetrical grooves are provided on both sides of the end face of the watershed heel segment II (3) to form a symmetrical weld (17), and the end face of the watershed heel segment II (3) is butt-jointed with the end face of the watershed heel segment I (2) without a gap, and the symmetrical weld (17) is welded.
6. The method for welding a ship's watertight heel according to claim 5, characterized in that: The symmetrical groove angle corresponding to the water heel segment II (3) is 45±5° 。 7. The method for welding a ship watertight heel according to claim 2, characterized in that: The specific operation of step S7 is: Single-sided grooves are provided on the butt-jointed end faces of the temporary left outer plate (6) of section II, the temporary right outer plate (7) of section II, and the outer plate (11) of the ship section II (5). When the temporary left outer plate (6) of section II, the temporary right outer plate (7) of section II, and the outer plate (11) of the ship section II (5) are butt-jointed, a gap is left to form a fifth butt weld (18) with the single-sided groove. After butt-jointing, a ceramic liner (10) is attached to the back of the fifth butt weld (18) at a side away from the single-sided groove, and finally the fifth butt weld (18) is welded.
8. The method for welding a ship watertight heel according to claim 7, characterized in that: When the temporary left outer plate (6) of section II and the temporary right outer plate (7) of section II are butt-jointed with the ship outer plate (11) of ship section II (5), the gap left is 4mm-8mm, and the angle of the fifth butt weld (18) is 40±5°.
9. The method for welding a ship watertight heel according to claim 2, characterized in that: The step S8 comprises butt welding of the watertight heel segment II (3) and the middle longitudinal plate (8) and welding of the watertight heel segment II (3) and the segment II temporary left outer plate (6) and the segment II temporary right outer plate (7), wherein: The specific operation of the butt welding of the watershed heel segment II (3) and the middle longitudinal plate (8) is as follows: a single-sided groove is provided on the butt end face of the watershed heel segment II (3); a gap is left when the watershed heel segment II (3) and the middle longitudinal plate (8) are butt-jointed so that a third butt weld (15) is formed with the single-sided groove; after butt-jointing, a ceramic liner (10) is attached to the back of the third butt weld (15) on the side away from the single-sided groove; and finally, the third butt weld (15) is welded; A single-sided groove arranged upward is provided on the butt joint end faces of the temporary left outer plate (6) of the segment II and the temporary right outer plate (7) of the segment II. When the watershed heel segment II (3) is butt jointed with the temporary left outer plate (6) of the segment II and the temporary right outer plate (7), a gap is left so that a fourth butt joint weld (16) is formed with the single-sided groove. Finally, the fourth butt joint weld (16) is welded.
10. The method for welding a ship watertight heel according to claim 9, characterized in that: The gap left when the watershed heel segment II (3) and the middle longitudinal plate (8) are butted together, and the gap left between the watershed heel segment II (3) and the segment II temporary left outer plate (6) and the segment II temporary right outer plate (7) are all 4 mm-8 mm; the single-sided groove angle corresponding to the watershed heel segment II (3) is 30±5°, and the single-sided groove angle corresponding to the segment II temporary left outer plate (6) and the segment II temporary right outer plate (7) is 30±5°.