Quickly-chargeable polyanion sodium battery positive electrode material and preparation method thereof
Through the preparation method of modified polyanionic cathode materials by co-doping of anions and cations, the Na4Fe3-xVx(PO4)2P2O7 electrode material was prepared using the solution gel method and spray drying method, which solved the problem of electronic conductivity and ionic conductivity of sodium-ion battery cathode materials. The problem of low efficiency has been solved, and the tap density of the material has been improved and the feasibility of industrial application has been achieved.
Patent Information
- Application Number
- CN202410806108.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing sodium-ion battery cathode materials have low electronic conductivity and ionic conductivity, and insufficient tap density, which limits their industrial application.
Using the preparation method of anion and cation co-doping modified polyanion cathode materials, the spherical structure Na4Fe3-xVx(PO4)2P2O7 electrode material was prepared through solution gel method and spray drying method to improve the tap density of the material.
It improves the tap density of the material, reduces production costs and time, is suitable for large-scale continuous production, and shows good charge and discharge performance and long cycle stability.
Smart Images

Figure CN118754079A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrode materials, and in particular relates to a fast-chargeable polyanion sodium positive electrode material, and also relates to a preparation method of the fast-chargeable polyanion sodium positive electrode material. Background Art
[0002] Due to the relative shortage of lithium ion resources in my country, the lithium resource reserves account for only 7.26% of the world's total, and the resource distribution is extremely uneven. The abundance of sodium in the earth's crust is 2.3%, ranking sixth among all elements, significantly higher than the 0.0017% of lithium. In addition, sodium ion batteries have the advantages of low resource cost and safety and environmental protection, and have broad application prospects in the field of large-scale energy storage. As an important part of sodium ion batteries, positive electrode materials play a decisive role in battery performance and other aspects.
[0003] However, at present, there are relatively few studies on sodium-ion batteries. Since the development of sodium-ion battery electrode materials is still in its early stages and there are few positive and negative electrode materials with good performance, most of the research is still devoted to the research of materials. The positive electrode materials of sodium-ion batteries are mainly composed of layered transition metal oxides, Prussian blue analogs, polyanion compounds, tunnel oxides, and amorphous materials. Among them, NVFPP (NVFPP), a material in the polyanion compound, has the advantages of high safety, low cost and environmental friendliness, but its low electronic conductivity and ionic conductivity as well as low tap density limit its practical application in industrialization. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a fast-chargeable polyanion sodium positive electrode material, which can improve the tap density of the material.
[0005] Another object of the present invention is to provide a fast-chargeable polyanion sodium positive electrode material.
[0006] The technical solution adopted by the present invention is to prepare a method for modifying a polyanion positive electrode material by co-doping anions and cations, which is specifically implemented by the following steps:
[0007] Step 1, mixing and stirring a sodium source, a phosphorus source and an iron source to dissolve at a preset temperature to obtain a mixed solution A;
[0008] Step 2, adding deionized water at a preset temperature to the vanadium source, stirring according to preset conditions, and obtaining a mixed solution B after the vanadium source is fully dissolved;
[0009] Step 3, slowly dripping the mixed solution A into the solution B at a uniform speed, stirring thoroughly during the dripping, generating a gray flocculent precipitate at the moment of dripping, and forming a mixture C after the dripping is completed;
[0010] Step 4, placing the mixture C in a water bath and evaporating it under preset conditions until the solution changes from completely gray to cyan blue;
[0011] Step 5, spray-drying the product of step 4 and placing it in a drying oven for vacuum drying, and grinding the dried material for later use;
[0012] Step 6: Place the ground material into a tube furnace for calcination, and after natural cooling, obtain Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Electrode material.
[0013] Another technical solution of the present invention is characterized in that:
[0014] The preset temperature in step 1 is 70° C., and the preset conditions of steps 1 and 2 are stirring at a speed of 250 r / min for 30 min.
[0015] The stirring speed during sufficient stirring in step 3 is 300 r / min.
[0016] The preset conditions in step 4 are: stirring at a speed of 300 r / min in a water bath at a temperature of 70°C.
[0017] The drying conditions for vacuum drying in step 5 are: vacuum drying at 80° C. for 12 h.
[0018] The calcination conditions in the tubular furnace in step 6 are: in an argon-hydrogen mixed gas atmosphere, the temperature is increased to 600° C. at a heating rate of 5° C. / min and maintained for 8 h.
[0019] Another technical solution adopted by the present invention is a fast-chargeable polyanion sodium positive electrode material, which has a uniform spherical structure.
[0020] The beneficial effects of the present invention are:
[0021] The present invention adopts a solution gel method (solid phase method) in combination with a spray drying method. With the aid of the spray drying technology, a solution or an emulsion can be directly dried into powder in a short time after being atomized, thereby preparing a spherical material and improving the tap density of the material. The cost is relatively low, the time consumption is short, and large-scale continuous production is easy. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7SEM images of materials;
[0023] Figure 2 The present invention Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 The charge and discharge curve of the material at 0.1C;
[0024] Figure 3 The present invention Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Long cycle data of the material's electrode at a current density of 1C. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] The present invention provides a method for preparing a fast-chargeable polyanion sodium positive electrode material, which is specifically implemented according to the following steps:
[0027] Step 1, mixing and stirring a sodium source, a phosphorus source and an iron source to dissolve at a preset temperature to obtain a mixed solution A;
[0028] The preset temperature in step 1 is 70°C, and the preset conditions in steps 1 and 2 are stirring at a speed of 250 r / min for 30 min;
[0029] Step 2, adding deionized water at a preset temperature to the vanadium source, stirring according to preset conditions, and obtaining a mixed solution B after the vanadium source is fully dissolved;
[0030] Step 3, slowly dripping the mixed solution A into the solution B at a uniform speed, stirring thoroughly during the dripping, generating a gray flocculent precipitate at the moment of dripping, and forming a mixture C after the dripping is completed;
[0031] The stirring speed during full stirring in step 3 is 300r / min;
[0032] Step 4, placing the mixture C in a water bath and evaporating it under preset conditions until the solution changes from completely gray to cyan blue;
[0033] The preset conditions in step 4 are: stirring at a speed of 300 r / min in a water bath at a temperature of 70°C;
[0034] Step 5, spray-drying the product of step 4 and placing it in a drying oven for vacuum drying, and grinding the dried material for later use;
[0035] The drying conditions of vacuum drying in step 5 are: vacuum drying at 80° C. for 12 h;
[0036] Step 6: Place the ground material into a tube furnace for calcination, and after natural cooling, obtain Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Electrode materials;
[0037] The calcination conditions in the tubular furnace in step 6 are: in an argon-hydrogen mixed gas atmosphere, the temperature is increased to 600° C. at a heating rate of 5° C. / min and maintained for 8 h.
[0038] The fast-chargeable polyanion sodium positive electrode material prepared by the present invention is a spherical structure with uniform morphology.
[0039] The fast-chargeable polyanion sodium positive electrode material prepared by the present invention; the positive electrode is composed of Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 The electrode material, Super-P and PVDF are composed in a ratio of 8:1:1. The diaphragm is made of glass fiber, the current collector is made of aluminum foil, the negative electrode is made of sodium sheet, and the electrolyte is 1M NaClO 4 , solvent is a mixture of EC and DEC, and the additive is FEC with a mass fraction of 2%.
[0040] Example 1
[0041] The method for preparing a fast-chargeable polyanion sodium positive electrode material is specifically implemented according to the following steps:
[0042] (1) Sodium hydroxide, hydrated sodium dihydrogen phosphate, and ferric nitrate are mixed in a beaker in a stoichiometric ratio of 1:8:4, a certain amount of deionized water heated to 70° C. is added thereto, and the mixture is placed on a stirring table and stirred at a speed of 250 r / min for 30 min to fully dissolve the materials, and a mixed solution A is obtained after the materials are fully dissolved;
[0043] (2) Take another beaker, add a mixed vanadium source of ammonium metavanadate and hydrated vanadyl sulfate in the same stoichiometric ratio as the phosphorus source (molar ratio 2:1), add a certain amount of deionized water heated to 70°C, place it on a stirring table and stir at a speed of 250 r / min for 30 min to fully dissolve the materials, and obtain a mixed solution B after full dissolution;
[0044] (3) Using a burette, the mixed solution A is slowly dripped into the solution B at a uniform speed, and the mixture is fully stirred at a speed of 300 r / min. A gray flocculent precipitate is generated at the moment of dripping, and a mixture C is formed after the dripping is completed;
[0045] (4) placing the mixture C formed in step (3) into a water bath with a preset temperature of 70° C. and stirring at a speed of 300 r / min until the color of the remaining solution in the beaker gradually changes from gray to cyan blue as the solution in the beaker evaporates;
[0046] (5) spray-drying the product of step (4) and placing it in a drying oven, vacuum drying it at 80° C. for 12 h, placing the dried material in an agate mortar, grinding it for 30 min, and setting it aside for later use;
[0047] (6) The ground material was placed in a tubular furnace for calcination. In an argon-hydrogen mixed gas atmosphere, the temperature was raised to 600°C at a rate of 2°C / min and maintained for 8 h. The purpose was to improve the crystallinity of the material. After natural cooling, a gray-green powder of Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Electrode material.
[0048] Example 2
[0049] The method for preparing a fast-chargeable polyanion sodium positive electrode material is specifically implemented according to the following steps:
[0050] (1) Sodium hydroxide, hydrated sodium dihydrogen phosphate, and ferric nitrate are mixed in a beaker in a stoichiometric ratio of 1:8:4, a certain amount of deionized water heated to 70° C. is added thereto, and the mixture is placed on a stirring table and stirred at a speed of 250 r / min for 30 min to fully dissolve the materials, and a mixed solution A is obtained after the materials are fully dissolved;
[0051] (2) Take another beaker, add a mixed vanadium source of ammonium metavanadate and hydrated vanadyl sulfate in the same stoichiometric ratio as the phosphorus source (molar ratio of 1:2), add a certain amount of deionized water heated to 70°C, place it on a stirring table and stir at a speed of 250 r / min for 30 min to fully dissolve the materials, and obtain a mixed solution B after full dissolution;
[0052] (3) Using a burette, the mixed solution A is slowly dripped into the solution B at a uniform speed, and the mixture is fully stirred at a speed of 300 r / min. A gray flocculent precipitate is generated at the moment of dripping, and a mixture C is formed after the dripping is completed;
[0053] (4) placing the mixture C formed in step (3) into a water bath with a preset temperature of 60° C. and stirring at a speed of 300 r / min until the color of the remaining solution in the beaker gradually changes from gray to cyan blue as the solution in the beaker evaporates;
[0054] (5) spray-drying the product of step (4) and placing it in a drying oven, vacuum drying it at 80° C. for 12 h, placing the dried material in an agate mortar, grinding it for 30 min, and setting it aside for later use;
[0055] (6) The ground material was placed in a tubular furnace for calcination. In an argon-hydrogen mixed gas atmosphere, the temperature was raised to 700°C at a rate of 2°C / min and maintained for 8 h. The purpose was to improve the crystallinity of the material. After natural cooling, a gray-green powder of Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Electrode material.
[0056] Example 3
[0057] The method for preparing a fast-chargeable polyanion sodium positive electrode material is specifically implemented according to the following steps:
[0058] (1) Sodium hydroxide, hydrated sodium dihydrogen phosphate, and ferric nitrate are mixed in a beaker in a stoichiometric ratio of 1:8:4, a certain amount of deionized water heated to 70° C. is added thereto, and the mixture is placed on a stirring table and stirred at a speed of 250 r / min for 30 min to fully dissolve the materials, and a mixed solution A is obtained after the materials are fully dissolved;
[0059] (2) Take another beaker, add a mixed vanadium source of ammonium metavanadate and hydrated vanadyl sulfate in the same stoichiometric ratio as the phosphorus source (molar ratio 2:1), add a certain amount of deionized water heated to 70°C, place it on a stirring table and stir at a speed of 250 r / min for 30 min to fully dissolve the materials, and obtain a mixed solution B after full dissolution;
[0060] (3) Using a burette, the mixed solution A is slowly dripped into the solution B at a uniform speed, and the mixture is fully stirred at a speed of 300 r / min. A gray flocculent precipitate is generated at the moment of dripping, and a mixture C is formed after the dripping is completed;
[0061] (4) placing the mixture C formed in step (3) into a water bath with a preset temperature of 60° C. and stirring at a speed of 300 r / min until the color of the remaining solution in the beaker gradually changes from gray to cyan blue as the solution in the beaker evaporates;
[0062] (5) spray-drying the product of step (4) and placing it in a drying oven, vacuum drying it at 80° C. for 12 h, placing the dried material in an agate mortar, grinding it for 30 min, and setting it aside for later use;
[0063] (6) The ground material was placed in a tubular furnace for calcination. In an argon-hydrogen mixed gas atmosphere, the temperature was raised to 700°C at a rate of 5°C / min and maintained for 6 h. The purpose was to improve the crystallinity of the material. After natural cooling, a gray-green powder of Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 Electrode material.
[0064] The above positive electrode materials, Super-P and PVDF are composed in a ratio of 8:1:1. The separator is made of glass fiber, the current collector is made of aluminum foil, the negative electrode is made of sodium sheet, and the electrolyte is 1M NaClO 4 , solvent EC and DEC mixture, additive is 2% by mass FEC. Assemble 2032 button cells.
[0065] like Figure 1 As shown, Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 SEM images of materials;
[0066] like Figure 2 As shown, Na 4 Fe 3-x V x (PO 4 ) 2 P 2 O 7 The charge and discharge curve of the material at 0.1C; From the charge and discharge curve of the sample between 2.0-4.3V, two symmetrical working voltage platforms can be observed, which are around 2.8V and 3.2V, respectively, corresponding to the insertion and extraction of Na. Its charge and discharge platform is longer, and more Na embedded and extracted provides more capacity. At 0.1C, the discharge specific capacity can reach about 107mAh / g, which is close to the theoretical specific capacity (130mAh / g).
[0067] like Figure 3 As shown, Na 4 Fe 3-x V x (PO 4 )2 P 2 O 7 The long cycle data of the material's electrode at a current density of 1C proves the excellent stability of the sample. In addition, the coulombic efficiency of the sample is basically maintained at 100%, indicating that the reaction requires less charge and the current utilization efficiency is high.
Claims
1. A method for preparing a fast-chargeable polyanion sodium positive electrode material, characterized in that: Please follow the steps below to implement: Step 1, mixing and stirring a sodium source, a phosphorus source and an iron source to dissolve at a preset temperature to obtain a mixed solution A; Step 2, adding deionized water at a preset temperature to the vanadium source, stirring according to preset conditions, and obtaining a mixed solution B after the vanadium source is fully dissolved; Step 3, slowly dripping the mixed solution A into the solution B at a uniform speed, stirring thoroughly during the dripping, generating a gray flocculent precipitate at the moment of dripping, and forming a mixture C after the dripping is completed; Step 4, placing the mixture C in a water bath and evaporating it under preset conditions until the solution changes from completely gray to cyan blue; Step 5, spray-drying the product of step 4 and placing it in a drying oven for vacuum drying, and grinding the dried material for later use; Step 6: Place the ground material into a tube furnace for calcination, and after natural cooling, obtain Na4Fe 3-x V x (PO4)2P2O7 electrode material.
2. The method for preparing the fast-chargeable polyanion sodium positive electrode material according to claim 1, characterized in that: The preset temperature in step 1 is 70° C., and the preset conditions for steps 1 and 2 are stirring at a rotation speed of 250 r / min for 30 min.
3. The method for preparing the fast-chargeable polyanion sodium positive electrode material according to claim 1, characterized in that: The stirring speed during sufficient stirring in step 3 is 300 r / min.
4. The method for preparing the fast-chargeable polyanion sodium positive electrode material according to claim 1, characterized in that: The preset conditions in step 4 are: stirring at a speed of 300 r / min in a water bath at a temperature of 70° C.
5. The method for preparing the fast-chargeable polyanion sodium positive electrode material according to claim 1, characterized in that: The drying conditions of the vacuum drying in step 5 are: vacuum drying at 80° C. for 12 h.
6. The method for preparing the fast-chargeable polyanion sodium positive electrode material according to claim 1, characterized in that: The calcination conditions in the tubular furnace in step 6 are: in an argon-hydrogen mixed gas atmosphere, the temperature is increased to 600° C. at a heating rate of 5° C. / min and maintained for 8 hours.
7. A fast-chargeable polyanion sodium cathode material prepared according to any one of claims 1 to 6, characterized in that: Its morphology is a uniform spherical structure.
Citation Information
Patent Citations
Use of bismuth-doped lithium vanadium phosphate positive pole material in lithium ion battery
CN106505196A
Preparation method of fluorine-containing polyanionic positive electrode material and fluorine-containing polyanionic positive electrode material
CN114572958A
Polyanion sodium battery positive electrode material, low-temperature water bath preparation method thereof and application of polyanion sodium battery positive electrode material in positive electrode material
CN117585661A