Repreparation method and application of waste lithium iron phosphate
Through the wet grinding and precipitation reaction of waste lithium iron phosphate, combined with the hydrothermal aging method, the problem of unused resources in the decommissioning of lithium iron phosphate batteries is solved, efficient full recovery and low-cost remanufactured lithium iron phosphate are achieved, and environmental hazards are reduced. .
Patent Information
- Application Number
- CN202410839541.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-26
AI Technical Summary
In the current decommissioning treatment of lithium iron phosphate batteries, the extraction efficiency of metallic lithium is low and the iron and phosphorus resources cannot be effectively recycled, resulting in resource waste and environmental pollution. There is a lack of efficient full-component recycling process solutions.
Use waste lithium iron phosphate, grinding aids and oxidants to mix wet grinding. Through precipitation and reduction reactions, lithium phosphate and ferrous phosphate are extracted respectively. Combined with the hydrothermal aging method, the lithium iron phosphate can be remade, reducing the use of acid and alkali and energy consumption. , improve resource recycling efficiency.
It achieves efficient and complete recovery of valuable elements in lithium iron phosphate battery waste, reduces production costs and environmental hazards, improves resource utilization, and the resulting reconstituted lithium iron phosphate has excellent performance.
Smart Images

Figure CN118754080A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of waste resource recycling and relates to a method for remaking waste lithium iron phosphate and a use thereof. Background Art
[0002] With the rapid development of the global new energy vehicle industry, lithium iron phosphate batteries have become an important force in the electric vehicle battery market due to their excellent safety performance, long cycle charge and discharge life, environmental friendliness and relatively economical price advantages. The installed capacity of lithium iron phosphate batteries has surpassed that of ternary lithium batteries in recent years, demonstrating its advantages in the field of energy storage. However, the subsequent large-scale retirement of lithium iron phosphate batteries not only poses a potential threat to the environment, but also poses a severe challenge to resource recycling.
[0003] In recent years, the number of retired power batteries in my country has been increasing year by year. According to statistics, in 2022, the theoretical retirement volume has reached 700,000 tons, and the actual recycling volume is 330,000 tons; in 2023, the theoretical retirement volume has rapidly climbed to 810,000 tons, while the actual recycling volume is only 460,000 tons, and nearly half of them have not been effectively recycled, highlighting the imperfection of the recycling system and the lack of processing capacity. It is estimated that by 2026, retired power batteries will reach 968,000 tons, and by 2030, it will reach a huge scale of 3 million tons. It can be seen that establishing an efficient recycling and reuse mechanism has become a top priority.
[0004] At present, my country generally adopts the wet regeneration and recycling process for the treatment of retired lithium iron phosphate batteries. This process mainly involves multiple links such as battery disassembly, leaching extraction, impurity removal and material regeneration. Although the wet process has shown a certain efficiency in metal extraction, it faces many challenges in actual operation. First of all, from a technical perspective, the selective extraction of metallic lithium is the core link. The currently widely used process is the acid leaching process, which uses sulfuric acid with hydrogen peroxide or air / oxygen oxidants to achieve leaching. Although these methods can effectively extract lithium elements, a large number of bubbles will be generated during the leaching process, which not only reduces the reaction rate, but also increases energy consumption, seriously affecting the overall production efficiency and economic benefits. What is more noteworthy is that most of the current recycling processes focus on extracting lithium elements, and there is often a lack of effective recycling and reuse methods for the iron and phosphorus resources produced, resulting in a large amount of idle and wasted iron-phosphorus-carbon slag resources.
[0005] To sum up, there is still a need to build a simple and easy process plan that can achieve efficient recycling and reuse of all components of waste lithium iron phosphate. This is the key to achieving full-chain green recycling and efficient resource utilization of retired lithium iron phosphate batteries, and promoting the healthy development of the new energy industry. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for remaking waste lithium iron phosphate and its use. The remaking method comprises wet grinding of waste lithium iron phosphate, grinding aid and oxidant to obtain lithium extraction liquid and iron phosphorus carbon slag; lithium phosphate is precipitated by the lithium extraction liquid, and pure ferrous dihydrogen phosphate solution is gradually prepared by the iron phosphorus carbon slag, and then ferrous phosphate is precipitated; finally, the obtained lithium phosphate and ferrous phosphate can be used to react to obtain remade lithium iron phosphate. The remaking method can realize the efficient and complete recovery of valuable elements in lithium iron phosphate battery waste. Compared with the existing acid leaching technology, it can greatly reduce the amount of acid and alkali, and the reaction process is mild and controllable, the production cost is low, and the harm to the environment and human body is reduced.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for remaking waste lithium iron phosphate, comprising:
[0009] (1) mixing waste lithium iron phosphate, a grinding aid and an oxidant, and performing a first pulping wet grinding to obtain a lithium extraction liquid and iron-phosphorus-carbon slag;
[0010] (2) subjecting the lithium extraction solution to lithium precipitation reaction to obtain lithium phosphate and mother liquor; mixing the iron-phosphorus-carbon slag with phosphoric acid and subjecting the mixture to a second pulping wet grinding to obtain a ferrous dihydrogen phosphate solution and carbon powder slag;
[0011] (3) mixing the ferrous dihydrogen phosphate solution with iron powder and performing a reduction reaction to obtain a crude ferrous dihydrogen phosphate solution;
[0012] (4) subjecting the crude ferrous dihydrogen phosphate solution to an aluminum precipitation reaction to obtain an aluminum product and a purified ferrous dihydrogen phosphate solution;
[0013] (5) subjecting the purified ferrous dihydrogen phosphate solution to an iron precipitation reaction to obtain ferrous phosphate;
[0014] (6) The ferrous phosphate obtained in step (5) is mixed with the lithium phosphate obtained in step (2), slurried and subjected to hydrothermal aging reaction to obtain remade lithium iron phosphate.
[0015] The reprocessing method of the present invention mixes lithium iron phosphate waste with a grinding aid and an oxidant, and extracts lithium by wet grinding. The process is short, the operation is simple, the slurry is close to neutral, the impurity leaching rate is low, and the obtained lithium extraction liquid does not need to be purified. Among them, the grinding aid mainly shortens the crushing time, saves energy consumption, and improves the grinding efficiency. In the wet grinding process, the molecules or particles collide, approach, and attract each other, and the powder is often easy to agglomerate, and the "reverse grinding" phenomenon occurs, that is, in the crushing process, when the material reaches a certain fineness and continues to grind, the phenomenon of grinding and becoming coarser will occur. The addition of a grinding aid can be firmly adsorbed on the cracks of the particles and can penetrate into the depth of the cracks. The new interface formed during the particle crushing process is quickly wrapped by the grinding aid, which hinders the recombination of the new interface and accelerates the crushing process. The role of the oxidant is mainly to oxidize lithium iron phosphate in the wet process to generate iron phosphate and release lithium ions. The present invention adopts phosphoric acid instead of sulfuric acid to dissolve the iron-phosphorus-carbon slag, which can reduce the introduction of impurity ions S, and adopts wet grinding to dissolve the iron-phosphorus-carbon slag, which can significantly improve the dissolution rate of ferrophosphorus; the reprocessing method of the present invention reduces and adjusts the value of ferric dihydrogen phosphate by iron powder, and at the same time, the iron powder reduces other heavy metal impurity ions in the solution, such as copper ions, and the obtained crude solution and impurities are easy to separate into solid and liquid, which can effectively improve the impurity removal effect; the present invention synthesizes the reprocessed lithium iron phosphate by hydrothermal aging method through the recycled lithium phosphate and ferrous phosphate, and the conditions are mild, and the product morphology, particle size, specific surface area, etc. can be further controlled by controlling the temperature, time, rotation speed and other conditions of the hydrothermal aging reaction, so that the obtained reprocessed lithium iron phosphate has excellent performance.
[0016] In the present invention, taking the mass of the obtained iron-phosphorus-carbon slag as 100%, the mass of ferric phosphate is preferably 55% to 75%, such as 55%, 58%, 60%, 63%, 65%, 68%, 70%, 72% or 75%, etc., preferably about 65%; the water content is 20% to 40%, such as 20%, 23%, 25%, 28%, 30%, 32%, 35%, 38% or 40%, etc., preferably about 30%; the carbon powder accounts for 1% to 10%, such as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., preferably about 5%, and at this time, adding phosphoric acid that does not react with carbon can ensure that the generated product is ferrous dihydrogen phosphate.
[0017] In the present invention, the hydrothermal aging reaction is mainly the hydrothermal reaction of ferrous phosphate and lithium phosphate to generate lithium iron phosphate. The aging reaction is a continuation of the hydrothermal reaction, which makes the hydrothermal reaction more thorough and the yield of lithium iron phosphate higher. At the same time, the aging reaction is also beneficial to the growth of the generated lithium iron phosphate particles and more uniform particle size. The aging and hydrothermal reactions can be transitioned and carried out uninterruptedly in one container.
[0018] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0019] As a preferred technical solution of the present invention, in step (1), the grinding aid includes at least one sulfate of sodium, potassium and ammonium, such as at least one of sodium sulfate, potassium sulfate or ammonium sulfate.
[0020] Preferably, the oxidant comprises at least one of sodium, potassium, and ammonium nitrate, hypochlorite, or hydrogen peroxide, such as sodium nitrate, potassium nitrate, ammonium nitrate, sodium hypochlorite, potassium hypochlorite, ammonium hypochlorite, or hydrogen peroxide.
[0021] Preferably, the mass percentage concentration of the hydrogen peroxide is 15% to 27.5%, for example, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27% or 27.5%.
[0022] Preferably, the amount of the grinding aid is 0.2 to 2 times the mass of the waste lithium iron phosphate, for example, 0.2 times, 0.5 times, 0.8 times, 1 times, 1.2 times, 1.4 times, 1.6 times, 1.8 times or 2 times the mass of the waste lithium iron phosphate.
[0023] Preferably, the amount of the oxidant is 0.2 to 3 times the mass of the waste lithium iron phosphate, for example, 0.2 times, 0.5 times, 0.8 times, 1 times, 1.2 times, 1.4 times, 1.6 times, 1.8 times, 2 times, 2.2 times, 2.4 times, 2.6 times, 2.8 times or 3 times the mass of the waste lithium iron phosphate.
[0024] Preferably, the pulping time of the first pulping wet grinding is 0.5 to 2 h, for example, 0.5 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h.
[0025] Preferably, the solid content of the slurry in the first pulping wet grinding is 10% to 30%, for example, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, etc.
[0026] Preferably, the feed rate of the first pulping wet grinding is 5% to 15% / min of the total mass of the pulp, such as 5% / min, 8% / min, 10% / min, 12% / min or 15% / min.
[0027] Preferably, the wet grinding speed of the first pulping wet grinding is 1000-3000rpm, for example, 1000rpm, 1200rpm, 1400rpm, 1600rpm, 1800rpm, 2000rpm, 2200rpm, 2400rpm, 2600rpm, 2800rpm or 3000rpm, and the wet grinding time is 0.5-5h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, etc.
[0028] As a preferred technical solution of the present invention, in step (2), the lithium extraction solution is mixed with a phosphate source to carry out the lithium precipitation reaction.
[0029] Preferably, the phosphate source comprises at least one of sodium, potassium and ammonium phosphates, such as at least one of sodium phosphate, potassium phosphate or ammonium phosphate.
[0030] The reprocessing method of the present invention adopts the phosphate source, such as sodium phosphate, to mix with a lithium extraction solution to precipitate lithium to prepare lithium phosphate, and has a high direct lithium recovery rate, which is convenient for the subsequent preparation of lithium iron phosphate.
[0031] Preferably, the dosage of the phosphate source is 1.1 to 1.5 times the theoretical reaction amount for reacting with the lithium element in the lithium extraction solution, for example, 1.1 times, 1.2 times, 1.3 times, 1.4 times or 1.5 times.
[0032] Preferably, the temperature of the lithium precipitation reaction is 85-95°C, for example, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C or 95°C, etc.; the time is 0.1-2h, for example, 0.1h, 0.3h, 0.5h, 0.8h, 1h, 1.2h, 1.4h, 1.6h, 1.8h or 2h, etc.
[0033] Preferably, the pH value of the lithium precipitation reaction is 12-13, for example, 12, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9 or 13.
[0034] Preferably, after the lithium precipitation reaction, solid-liquid separation, drying and pulverization are sequentially performed to obtain the lithium phosphate.
[0035] Preferably, the mother liquor is recycled to step (1) as the grinding aid.
[0036] As a preferred technical solution of the present invention, the amounts of the phosphoric acid and the iron-phosphorus-carbon slag are controlled according to the ratio of the molar amount of phosphate in the phosphoric acid to the molar amount of the iron element in the iron-phosphorus-carbon slag (3-4.5):1, for example, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1 or 4.5:1.
[0037] The chemical formula of the ferrous dihydrogen phosphate generated in the present invention is Fe(H2PO4)3. Therefore, based on the molar ratio of the iron element to the phosphate in the ferrous dihydrogen phosphate being 3:1, the phosphate is controlled to be 20% to 50% excessive to add phosphoric acid, that is, the ratio of the molar amount of the phosphate in the phosphoric acid to the molar amount of the iron element in the iron-phosphorus-carbon slag is preferably (3 to 4.5):1. It should also be noted that the present invention does not limit the specific concentration of phosphoric acid. The concentration and amount of phosphoric acid should be determined according to the specific amount of iron-phosphorus-carbon slag and the required molar ratio of the above-mentioned iron element to the phosphate. Phosphoric acid with a mass percentage concentration of 20% to 85% can be reasonably selected and applied to the present invention.
[0038] Preferably, the pulping time of the second pulping wet grinding is 0.5 to 2 h, for example, 0.5 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h or 2 h.
[0039] Preferably, the solid content of the slurry in the second pulping wet grinding is 20% to 40%, for example, 20%, 23%, 25%, 28%, 30%, 33%, 35%, 38% or 40%.
[0040] Preferably, the feed rate of the second pulping wet mill is 5% to 15% / min of the total mass of the pulp, such as 5% / min, 8% / min, 10% / min, 12% / min or 15% / min.
[0041] Preferably, the wet grinding speed of the second pulping wet grinding is 1000-3000rpm, for example, 1000rpm, 1200rpm, 1400rpm, 1600rpm, 1800rpm, 2000rpm, 2200rpm, 2400rpm, 2600rpm, 2800rpm or 3000rpm, and the wet grinding time is 0.5-5h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, etc.
[0042] As a preferred technical solution of the present invention, in step (3), the end point pH value of the reduction reaction is 2-3, for example, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3.
[0043] Preferably, the reduction reaction time is 3 to 5 h, for example, 3 h, 3.3 h, 3.5 h, 3.8 h, 4 h, 4.3 h, 4.5 h, 4.8 h or 5 h.
[0044] As a preferred technical solution of the present invention, in step (4), the crude ferrous dihydrogen phosphate solution is mixed with at least one fluoride salt of sodium, potassium, and ammonium, such as at least one of sodium fluoride, potassium fluoride, or ammonium fluoride, preferably sodium fluoride, to carry out the aluminum precipitation reaction.
[0045] Preferably, the amount of the fluoride salt used is 0.5 to 2 times the theoretical reaction amount of the fluoride salt reacting with the aluminum element in the crude ferrous dihydrogen phosphate solution, for example, 0.2 times, 0.4 times, 0.6 times, 0.8 times, 1 times, 1.2 times, 1.4 times, 1.6 times, 1.8 times or 2 times, etc.
[0046] When the present invention uses sodium fluoride to precipitate aluminum, the obtained aluminum product is cryolite; when the present invention uses potassium fluoride to precipitate aluminum, the obtained aluminum product is potassium cryolite; when the present invention uses ammonium fluoride to precipitate aluminum, the obtained aluminum product is ammonium hexafluoroaluminate.
[0047] Preferably, the aluminum precipitation reaction time is 1 to 3 hours, for example, 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h or 3 h.
[0048] As a preferred technical solution of the present invention, in step (5), the purified ferrous dihydrogen phosphate solution is mixed with an alkali source to carry out the iron precipitation reaction.
[0049] Preferably, the alkali source comprises a carbonate and / or hydroxide of at least one of sodium, potassium and ammonium, preferably at least one of sodium carbonate, potassium carbonate or ammonium carbonate.
[0050] In the present invention, the alkali source mainly functions to adjust the pH value, such as sodium hydroxide, ammonia water and sodium carbonate. However, the alkalinity of sodium hydroxide / potassium hydroxide is stronger than that of sodium carbonate, and local over-alkalinity is likely to occur during the adjustment process to generate ferrous hydroxide, resulting in a lower purity of the generated ferrous phosphate. It is preferred to use a corresponding alkali solution with a mass percentage concentration of 1% to 10%. When ammonia water is used, ammonia gas is easily volatilized during the adjustment process, resulting in a poor operating environment. Therefore, it is further preferred that the alkali source uses a carbonate source, that is, at least one carbonate of sodium, potassium and ammonium.
[0051] Preferably, the pH value of the iron precipitation reaction is 5 to 7, for example, 5, 5.2, 5.4, 5.6, 5.8, 6, 6.2, 6.4, 6.6, 6.8 or 7.
[0052] Preferably, the iron precipitation reaction time is 1 to 3 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours or 3 hours.
[0053] As a preferred technical solution of the present invention, in step (6), the hydrothermal aging reaction is carried out under an inert atmosphere.
[0054] Preferably, the temperature of the hydrothermal aging reaction is 90-200°C, for example 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, and the time is 10-30h, for example 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h or 30h, etc.
[0055] Preferably, after the hydrothermal aging reaction is completed, the resulting product is dried at 80-120°C, such as 80°C, 90°C, 100°C, 110°C or 120°C, for 4-8h, such as 4h, 5h, 6h, 7h or 8h, to obtain the remade lithium iron phosphate.
[0056] In a second aspect, the present invention provides a remanufactured lithium iron phosphate obtained according to the remanufacturing method described in the first aspect.
[0057] In a third aspect, the present invention provides a lithium-ion battery comprising the remanufactured lithium iron phosphate described in the second aspect.
[0058] Due to space limitations and to avoid redundancy, the present invention does not list all point values within the above numerical range one by one, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0059] Compared with the prior art solutions, the present invention has at least the following beneficial effects:
[0060] The reprocessing method of the present invention can realize the efficient and complete recovery of valuable elements in lithium iron phosphate battery waste. Compared with the existing acid leaching technology, it can greatly reduce the amount of acid and alkali used, and the reaction process is mild and controllable, the production cost is low, and the harm to the environment and human body is reduced. The obtained reprocessed lithium iron phosphate has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 is a schematic flow chart of the method for remaking waste lithium iron phosphate in Example 1;
[0062] Figure 2 This is the XRD test diagram of the remanufactured lithium iron phosphate obtained in Example 1. DETAILED DESCRIPTION
[0063] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0064] It should be clear to those skilled in the art that the embodiments are only intended to help understand the present invention and should not be considered as specific limitations of the present invention.
[0065] Example 1
[0066] This embodiment provides a method for remaking waste lithium iron phosphate, such as Figure 1 As shown, including:
[0067] (1) Prepare 1000g of waste lithium iron phosphate A (its components are shown in Table 1); place waste lithium iron phosphate A in a beaker, add 500g of sodium sulfate (0.5 times the mass of grinding aid), 500g of hydrogen peroxide (mass percentage concentration is 20%), and pure water, and stir at room temperature for 0.5h to prepare a slurry with a solid content of 30%; add the mixed slurry into the feed bin of the overflow wet grinder with a slurry peristaltic pump, control the feed flow rate to 10% / min of the total mass of the slurry, and wet grind at 60°C. The wet grinder discharge pipe is connected to the beaker containing the mixed slurry, and the wet grinding is circulated. During the wet grinding, the condensation water pipe is connected and water is passed to the wet grinder for cooling. After wet grinding at 2000rpm for 5h, all the wet-ground slurry is discharged, and solid-liquid separation is performed to obtain lithium extraction liquid and iron-phosphorus-carbon slag;
[0068] (2) The lithium extraction solution is heated to 90° C., a saturated solution of sodium phosphate as a phosphate source is added, the pH value is controlled to be 12.6, and a lithium precipitation reaction is carried out for 0.5 h. The solid-liquid separation is performed to obtain lithium phosphate and mother liquor A (containing sodium sulfate); the obtained lithium phosphate is rinsed twice with pure water, dried and crushed to obtain battery-grade lithium phosphate, and the obtained mother liquor A is appropriately concentrated and repeatedly used as a grinding aid in step (1). 1000g of iron-phosphorus-carbon slag is accumulated and placed in a beaker. 500g of phosphoric acid and pure water are added according to the ratio of the molar amount of phosphate in the phosphoric acid to the molar amount of the iron element in the iron-phosphorus-carbon slag of 3.5:1. The mixture is stirred for 0.5h to prepare a slurry with a solid content of 30%. The mixed slurry is added into the feed bin of the overflow wet mill with a slurry peristaltic pump for wet grinding. The discharge pipe of the wet mill is connected to the beaker containing the mixed slurry. Circular wet grinding is performed during wet grinding. The condensation water pipe is connected during wet grinding, and water is passed to the wet mill for cooling. After wet grinding at 2000rpm for 5h, all the wet-ground slurry is discharged for solid-liquid separation to obtain a dihydrogen ferrous phosphate solution and carbon powder slag.
[0069] (3) adding reduced iron powder to the ferric dihydrogen phosphate solution, and performing a reduction reaction for 4 hours, controlling the pH value at the end point of the reaction to be 2.5, so as to reduce all the ferric iron to ferrous iron and remove copper, and filtering to obtain a crude ferrous dihydrogen phosphate solution; the excess reduced iron powder is washed and reused;
[0070] (4) adding sodium fluoride to the crude ferrous phosphate solution, controlling the amount of the fluoride salt to be 1.3 times the theoretical amount of the reaction with the aluminum element in the crude ferrous phosphate solution, performing aluminum precipitation reaction for 2 hours, and performing solid-liquid separation to obtain aluminum product crude cryolite and ferrous phosphate purified solution; refining the crude cryolite to obtain refined cryolite;
[0071] (5) adding a saturated solution of sodium carbonate as a carbonate source to the purified ferrous dihydrogen phosphate solution to a pH value of 6, and performing an iron precipitation reaction for 2 hours to obtain a mother solution B and ferrous phosphate octahydrate, and rinsing the obtained ferrous phosphate octahydrate with deionized water twice;
[0072] (6) The battery-grade lithium phosphate obtained in step (2) and the washed ferrous phosphate octahydrate obtained in step (5) are mixed in equimolar amounts to form a slurry, placed in a high-pressure reactor, heated to 180° C., and subjected to a hydrothermal aging reaction for 20 h. After solid-liquid separation, the mixture is rinsed twice with deionized water, and dried in a nitrogen atmosphere furnace at 100° C. for 6 h to obtain reconstituted lithium iron phosphate.
[0073] Example 2
[0074] This embodiment provides a method for remaking waste lithium iron phosphate, which expands the production scale. In step (1), 5 kg of waste lithium iron phosphate A is used, and in step (2), 5 kg of iron-phosphorus-carbon slag is used. The amounts of other raw materials are adjusted accordingly. Except for the above, other conditions are exactly the same as those in Example 1.
[0075] Example 3
[0076] This embodiment provides a method for reprocessing waste lithium iron phosphate. The method uses another waste lithium iron phosphate B (its composition is shown in Table 1) in step (1). Except for the above, other conditions are exactly the same as those in Example 1.
[0077] Example 4
[0078] This embodiment provides a method for reprocessing waste lithium iron phosphate. In step (1) of the reprocessing method, the oxidant is replaced by sodium nitrate instead of hydrogen peroxide. Except for the above, other conditions are exactly the same as those in Example 1.
[0079] Example 5
[0080] This embodiment provides a method for reprocessing waste lithium iron phosphate. In step (1) of the reprocessing method, the oxidant is replaced by sodium hypochlorite instead of hydrogen peroxide. Except for the above, other conditions are exactly the same as those in Example 1.
[0081] Characterization and Testing:
[0082] Figure 2This is the XRD diagram of the remanufactured lithium iron phosphate obtained in Example 1. It can be seen from the figure that the remanufactured lithium iron phosphate obtained conforms to the lithium iron phosphate phase of the PDF card.
[0083] The elemental composition of the raw materials, intermediate products and final products involved in the method for remaking waste lithium iron phosphate in Example 1 was tested, and the results are shown in Tables 1 and 2.
[0084] Table 1
[0085] Sample of Example 1 Li Fe P Cu Al Ni Co Mn Waste lithium iron phosphate A (wt%) 4.17 34.11 18.61 0.0006 0.0846 0.1383 0.0185 0.1278 Lithium extraction solution (g / L) 20.23 0.001 0.001 0.0003 0.0001 0.0001 0.0001 0.0001 Iron phosphorus carbon slag (wt%) 0.072 34.23 18.68 0.0007 0.085 0.140 0.019 0.13 Mother liquor A(g / L) 1.45 0.001 0.001 0.0003 0.0001 0.0001 0.0001 0.0001 Ferrous dihydrogen phosphate solution (g / L) 0.11 45.23 40.1 0.23 0.45 0.01 0.003 0.01 Ferrous dihydrogen phosphate crude solution (g / L) 0.11 72.368 40.135 0.001 0.43 0.01 0.003 0.01 Ferrous dihydrogen phosphate purification solution (g / L) 0.1 71.21 39.87 0.001 0.01 0.01 0.003 0.01 Mother liquor B (g / L) 0.06 2.34 1.34 0.0001 0.0001 0.0001 0.0001 0.0001
[0086] Table 2
[0087]
[0088]
[0089] The elemental composition of the raw materials, intermediate products and final products involved in the method for remaking waste lithium iron phosphate in Example 3 was tested, and the results are shown in Tables 3 and 4.
[0090] Table 3
[0091] Sample of Example 3 Li Fe P Cu Al Ni Co Mn Waste lithium iron phosphate B (wt%) 2.8 22.4 12.4 0.8 1.1 0.15 0.04 0.23 Lithium extraction solution (g / L) 14.2 0.01 0.01 0.001 0.005 0.001 0.001 0.001 Iron phosphorus carbon slag (wt%) 0.09 22.38 12.38 0.08 1.09 0.15 0.04 0.23 Mother liquor A(g / L) 1.56 0.001 0.001 0.001 0.001 0.001 0.001 0.001 Ferrous dihydrogen phosphate solution (g / L) 0.01 41.32 37.21 1.45 1.87 0.23 0.06 0.35 Ferrous dihydrogen phosphate crude solution (g / L) 0.01 63.34 37.21 0.001 1.85 0.22 0.06 0.35 Ferrous dihydrogen phosphate purification solution (g / L) 0.01 61.23 37.01 0.001 0.034 0.21 0.06 0.34 Mother liquor B (g / L) 0.01 2.34 1.36 0.001 0.001 0.001 0.001 0.15
[0092] Table 4
[0093] Sample of Example 3 Li P <![CDATA[PO4 3- ]]> Fe Cu Al <![CDATA[H2O]]> Li / P Fe / P Lithium phosphate (wt%) 12.33 18.25 37.6 0.01 0.001 0.001 32.3 2.99 - Ferrous phosphate octahydrate (wt%) 0.001 4.31 12.35 11.89 0.001 0.001 72.43 - 1.52 Reprocessed lithium iron phosphate (wt%) 4.40 19.56 40.32 35.12 0.001 0.001 0.11 0.99 0.99 National standard lithium iron phosphate (wt%) 4.4±1 20±1 / 35±2 / / / / /
[0094] The elemental composition of the remanufactured lithium iron phosphate obtained in Example 2-5 was tested, and the results are shown in Table 5.
[0095] Table 5
[0096] Reprocessed lithium iron phosphate (wt%) Li P <![CDATA[PO4 3- ]]> Fe Cu Al <![CDATA[H2O]]> Li / P Fe / P Example 2 4.38 19.51 40.34 35.08 0.001 0.02 0.1 0.99 0.99 Example 4 4.23 18.50 40.28 35.07 0.001 0.03 0.1 1.01 1.04 Example 5 4.34 18.50 40.31 35.02 0.001 0.02 0.1 1.03 1.04 National standard lithium iron phosphate 4.4±1 20±1 / 35±2 / / / / /
[0097] Note: In Table 1-5, “-” means the value is too small and is ignored; “ / ” means no need to calculate. The molar ratio Li / P and the molar ratio Fe / P are calculated based on the relative molecular mass of Li being 7, Fe being 56, and P being 31.
[0098] The remanufactured lithium iron phosphate obtained in Example 1-5 was used as the positive electrode material to prepare a battery for testing:
[0099] Weigh the positive electrode material, acetylene black and polytetrafluoroethylene in a mass ratio of 80:10:10 respectively, mix and grind the positive electrode material and acetylene black thoroughly, and then add polytetrafluoroethylene. Then press the positive electrode film with a certain thickness on a roller mill, and place the obtained positive electrode film in a vacuum drying oven at 120°C for 12 hours. Press the dried positive electrode film tightly with aluminum foil to obtain a positive electrode sheet.
[0100] Battery assembly: Place the prepared weighed positive electrode sheet into a glove box filled with argon, use a metal lithium sheet as the negative electrode of the battery, the electrolyte is 1 mol / L LiPF6 (EC+DEC, volume ratio is 1:1), and the separator is Celgard2400 type, and assemble into a CR2032 button cell. After assembly, take out the battery and seal it, and let it stand for 12 hours before testing.
[0101] The first charge specific capacity and the first discharge specific capacity at 0.1C were tested with a charge cut-off voltage of 4V and a discharge cut-off voltage of 2V; the discharge specific capacity at 1C was tested with a charge cut-off voltage of 3.75V and a discharge cut-off voltage of 2V. The results are recorded in Table 6.
[0102] Table 6
[0103]
[0104] Combining Table 1, Table 2, Table 3, Table 4, Table 5, and Table 6 for analysis, in the process of remaking lithium iron phosphate, iron powder is added to remove copper and sodium fluoride is added to remove aluminum. Therefore, the content of impurities copper and aluminum in lithium phosphate, iron phosphate and lithium iron phosphate is low, and the electrochemical properties of the remade lithium iron phosphate material are less affected. For impurities such as nickel, cobalt and manganese, although there is no targeted removal method in the remaking method described in the present invention, which will result in a certain amount of nickel, cobalt and manganese in ferrous phosphate and remade lithium iron phosphate, the nickel, cobalt and manganese present in the remade lithium iron phosphate have no obvious effect on the first charge specific capacity and first discharge specific capacity of 0.1C, as well as the 1C discharge specific capacity.
[0105] From the above, it can be seen that the reprocessing method of the present invention can achieve efficient and complete recovery of valuable elements in lithium iron phosphate battery waste. Compared with the existing acid leaching technology, it can greatly reduce the amount of acid and alkali used, and the reaction process is mild and controllable, the production cost is low, and the harm to the environment and human body is reduced. The obtained reprocessed lithium iron phosphate has excellent performance.
[0106] The present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0107] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0108] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0109] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for remaking waste lithium iron phosphate, It is characterized in that include: (1) mixing waste lithium iron phosphate, a grinding aid and an oxidant, and performing a first pulping wet grinding to obtain a lithium extraction liquid and iron-phosphorus-carbon slag; (2) subjecting the lithium extraction solution to lithium precipitation reaction to obtain lithium phosphate and mother liquor; mixing the iron-phosphorus-carbon slag with phosphoric acid and subjecting the mixture to a second pulping wet grinding to obtain a ferrous dihydrogen phosphate solution and carbon powder slag; (3) mixing the ferrous dihydrogen phosphate solution with iron powder and performing a reduction reaction to obtain a crude ferrous dihydrogen phosphate solution; (4) subjecting the crude ferrous dihydrogen phosphate solution to an aluminum precipitation reaction to obtain an aluminum product and a purified ferrous dihydrogen phosphate solution; (5) subjecting the purified ferrous dihydrogen phosphate solution to an iron precipitation reaction to obtain ferrous phosphate; (6) The ferrous phosphate obtained in step (5) is mixed with the lithium phosphate obtained in step (2), slurried and subjected to hydrothermal aging reaction to obtain remade lithium iron phosphate.
2. The method for remaking waste lithium iron phosphate according to claim 1, It is characterized in that In step (1), the grinding aid comprises at least one sulfate of sodium, potassium and ammonium; Preferably, the oxidant comprises at least one of sodium, potassium, and ammonium nitrates, hypochlorites, or hydrogen peroxide; Preferably, the amount of the grinding aid is 0.2 to 2 times the mass of the waste lithium iron phosphate; Preferably, the amount of the oxidant is 0.2 to 3 times the mass of the waste lithium iron phosphate; Preferably, the pulping time of the first pulping wet grinding is 0.5 to 2 hours; Preferably, the solid content of the slurry in the first pulping wet grinding is 10% to 30%; Preferably, the feed rate of the first pulping wet mill is 5% to 15% / min of the total mass of the pulp; Preferably, the wet grinding speed of the first pulping wet grinding is 1000-3000 rpm, and the wet grinding time is 0.5-5 h.
3. The method for remaking waste lithium iron phosphate according to claim 1 or 2, It is characterized in that In step (2), the lithium extraction solution is mixed with a phosphate source to perform the lithium precipitation reaction; Preferably, the phosphate source comprises at least one of sodium, potassium and ammonium phosphates; Preferably, the amount of the phosphate source is 1.1 to 1.5 times the theoretical amount of the phosphate source reacting with the lithium element in the lithium extraction solution; Preferably, the temperature of the lithium precipitation reaction is 85-95°C and the time is 0.1-2h; Preferably, the pH value of the lithium precipitation reaction is 12 to 13; Preferably, after the lithium precipitation reaction, solid-liquid separation, drying and crushing are sequentially performed to obtain the lithium phosphate; Preferably, the mother liquor is recycled to step (1) as the grinding aid.
4. The method for remaking waste lithium iron phosphate according to any one of claims 1 to 3, It is characterized in that In step (2), the amounts of the phosphoric acid and the iron-phosphorus-carbon slag are controlled according to a ratio of the molar amount of phosphate in the phosphoric acid to the molar amount of the iron element in the iron-phosphorus-carbon slag of (3-4.5):1; Preferably, the pulping time of the second pulping wet grinding is 0.5 to 2 hours; Preferably, the solid content of the slurry in the second pulping wet grinding is 20% to 40%; Preferably, the feed rate of the second pulping wet mill is 5% to 15% / min of the total mass of the pulp; Preferably, the wet grinding speed of the second pulping wet grinding is 1000-3000 rpm, and the wet grinding time is 0.5-5 h.
5. The method for reprocessing waste lithium iron phosphate according to any one of claims 1 to 4, It is characterized in that In step (3), the end point pH value of the reduction reaction is 2 to 3; Preferably, the reduction reaction time is 3 to 5 hours.
6. The method for reprocessing waste lithium iron phosphate according to any one of claims 1 to 5, It is characterized in that In step (4), the crude ferrous dihydrogen phosphate solution is mixed with at least one fluoride salt of sodium, potassium, and ammonium to carry out the aluminum precipitation reaction; Preferably, the amount of the fluoride salt is 0.5 to 2 times the theoretical amount of the reaction with the aluminum element in the crude ferrous dihydrogen phosphate solution; Preferably, the aluminum precipitation reaction time is 1 to 3 hours.
7. The method for remaking waste lithium iron phosphate according to any one of claims 1 to 6, It is characterized in that In step (5), the purified ferrous dihydrogen phosphate solution is mixed with an alkali source to perform the iron precipitation reaction; Preferably, the alkali source comprises carbonate and / or hydroxide of at least one of sodium, potassium and ammonium; Preferably, the pH value of the iron precipitation reaction is 5 to 7; Preferably, the iron precipitation reaction time is 1 to 3 hours.
8. The method for reprocessing waste lithium iron phosphate according to any one of claims 1 to 7, It is characterized in that In step (6), the hydrothermal aging reaction is carried out under an inert atmosphere; Preferably, the temperature of the hydrothermal aging reaction is 90 to 200° C. and the time is 10 to 30 hours; Preferably, after the hydrothermal aging reaction is completed, the obtained product is dried at 80-120° C. for 4-8 hours to obtain the remanufactured lithium iron phosphate.
9. A remanufactured lithium iron phosphate, It is characterized in that Obtained according to the reprocessing method according to any one of claims 1 to 8.
10. A lithium ion battery, It is characterized in that Contains the remanufactured lithium iron phosphate as claimed in claim 9.
Citation Information
Patent Citations
Method for preparing basic lithium iron phosphate and regenerating lithium iron phosphate from waste lithium iron phosphate positive electrode powder
CN117049499A
Method for wet recovery of iron phosphate and lithium carbonate from lithium iron phosphate battery
CN117361467A
Method for regenerating battery-grade iron phosphate from waste lithium iron phosphate
CN117756073A
Method for recovering lithium from lithium iron phosphate waste and application thereof
US20230340635A1
Recovery method for lithium iron phosphate
WO2024021237A1
Cited By
Regeneration, repair and doping method of waste lithium iron phosphate material and regenerated positive electrode material