Preparation method of nano silicon dioxide sol
By using ammonia/ammonium chloride buffer solution and alcohol-water reaction system in the preparation of silica sol, the particle size and separation efficiency of nano-silica are controlled, and the problems of insufficient purity and stability of silica sol in the existing technology are solved, and the application is realized. Preparation of nanosilica sol for high-end fields.
Patent Information
- Application Number
- CN202411151969.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-11
AI Technical Summary
When preparing silica sol, the existing technology has problems such as low product purity, poor stability, low separation efficiency, and large particle size of nanosilica, making it difficult to meet the application needs of high-end fields.
Ammonia/ammonium chloride buffer solution and alcoholic water are used as the reaction system. By controlling the pH value and catalytic microenvironment of the reaction system, orthosilicate is used as the silicon source, and the solution is slowly added to prepare nano-silica. The particle size is controlled and Improve separation efficiency.
Preparation of small particle size (15-50nm), high-purity nano-silica sol is suitable for high-end fields such as electronics and optics, and has good stability. It can be stored for six months in a natural environment without settling, gelling, or separation. High efficiency.
Smart Images

Figure BDA0005003890260000061 
Figure HDA0005003890280000011 
Figure HDA0005003890280000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silica sol preparation, and in particular to a method for preparing nano silica sol. Background Art
[0002] Silica sol, also known as silicon dioxide hydrosol or silicic acid sol, is a milky white colloidal solution and a special nanomaterial. It has physical and chemical properties such as large specific surface area, high dispersibility, high adsorption, high fire resistance and thermal insulation. It is widely used in the fields of chemistry and mechanical polishing.
[0003] At present, the methods for producing silica sol mainly include microemulsion method, template method and sol-gel method. Among them, the microemulsion method often uses sodium silicate as raw material for preparation. There is an organic solvent in the reaction system, which is difficult to completely remove. The purity of the obtained product is low, the reaction time is long, and the separation efficiency is low; the organic template method has a complex reaction system, and the surfactant as a template will introduce a large amount of metal ions, which is not conducive to separation and purification, and the purity of the obtained product is low. The sol-gel method mainly uses silicate as raw material to prepare silica sol. The preparation technology is relatively mature, but in the absence of a stabilizer, gelation is easy to occur, which is difficult to preserve for a long time and is not conducive to storage and transportation. CN101602508A discloses a method for preparing a monodisperse nano-silica spherical particle hydrosol. The sol-gel method is adopted, ammonia is used as a catalyst for the hydrolysis reaction of ethyl orthosilicate, and ethanol is used as a solvent to prepare nano-SiO 2 Particles were obtained by dispersing SiO 2 The particle suspension is heated and blown to volatilize most of the alcohol in the suspension to obtain a nano-silicon dioxide particle slurry, and then an aqueous solution of amino alcohol is added to the slurry to finally prepare a nano-SiO 2 Hydrosol. This method improves the storage stability of silica sol to a certain extent, but the nano-silicon dioxide produced has a large particle size and is not suitable for higher-end scenarios, such as electronic or optical applications. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for preparing nano-silica sol, so as to solve the problems that the silica sol products prepared by the existing methods have low purity, poor stability, low separation efficiency and large nano-silica particle size, and are not suitable for high-end scenarios.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing nano silica sol comprises the following steps:
[0007] S1: dissolving orthosilicate in alcohol, stirring and mixing evenly to obtain solution A;
[0008] S2: adding a buffer solvent, deionized water and alcohol into a reaction vessel, stirring and mixing them uniformly to obtain a solution B;
[0009] S3: Solution A is added evenly and slowly into solution B, and the mixture is stirred to react to obtain silica sol.
[0010] Furthermore, the buffer solvent is an ammonia / ammonium chloride buffer solution with a pH of 9.5 to 10.5.
[0011] Furthermore, in the S1, the mass ratio of orthosilicate to alcohol is 10-40:60-90.
[0012] Furthermore, in S2, the mass ratio of the buffer solvent, deionized water and alcohol is 1-10:50-70:20-35.
[0013] Furthermore, in S3, the speed of slowly adding is 2 to 8 seconds per drop.
[0014] Furthermore, in S3, the stirring reaction is carried out at 50-80° C. for 4-24 hours.
[0015] Furthermore, the orthosilicate includes methyl orthosilicate or ethyl orthosilicate.
[0016] Furthermore, the alcohol includes methanol or ethanol.
[0017] The present invention improves the traditional sol-gel method, uses ammonia-ammonium chloride buffer solution and alcohol-water mixed solvent as the reaction system, and orthosilicate as the silicon source to prepare silica sol. By stably regulating the pH value of the reaction system and regulating the catalytic microenvironment of the orthosilicate sol-gel, the particle size of nano-silicon dioxide is regulated to obtain low-particle-size nano-silicon dioxide, which is suitable for high-end fields such as optics and electronics.
[0018] In step S1, using alcohol as a diluent to dilute orthosilicate can prevent the orthosilicate concentration from being too high and being directly added to the catalytic system, resulting in the problem of excessive local concentration of orthosilicate and excessive particle size of silica particles. Therefore, the mass ratio of orthosilicate to alcohol is controlled to be 10-40:60-90. On the one hand, it can avoid excessive local concentration of orthosilicate in the catalytic system, resulting in excessive particle size of silica particles, and at the same time avoid excessive addition of alcohol, which increases costs. Preferably, the mass ratio of orthosilicate to alcohol is 10:90.
[0019] As the catalyst is consumed in the solvent environment, the pH value in the solvent will change, thereby causing the uncontrollable growth of silica particles, agglomeration, and making it impossible to control the size of silica particles. Therefore, in step S2, a buffer solvent is selected as a pH stabilizer to prevent the pH value from changing due to changes in catalyst concentration, thereby controlling the growth of silica. At the same time, the salt component in the buffer solvent can form ion clusters in the solvent, and the chloride ions are completely ionized, wrapping the silicon oxygen polymer, thereby forming silica particles with high roundness and small particle size during the process of nano-scale gel; using ammonia water as an alkaline catalyst, it is also possible to avoid using an organic base as a catalyst, further improving the product separation efficiency. At the same time, the concentration of the buffer solvent should not be too large, because the excessive concentration of the buffer solvent will cause the catalyst (i.e., ammonia water) concentration to be too high, and the excessive concentration of the catalyst will cause the silica particle size to be too large.
[0020] In order to further ensure the low-concentration catalytic environment of the silicate reaction, in step S3, solution A is evenly and slowly added to solution B in which the catalyst is evenly dispersed, which can ensure the stability and controllability of the catalytic hydrolysis reaction. In addition, the alcohol in the solvent can promote the contact between water and silicate on the one hand, and form a reaction interface with water on the other hand, creating a microenvironment for the silicate reaction, so that the silicate can undergo nano-scale gelation in the region to generate small-sized silica particles; and using alcohol as a solvent can avoid the use of organic solvents that are difficult to separate, thereby improving the product separation efficiency.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The silica sol preparation method of the present invention uses orthosilicate as silicon source, ammonia / ammonium chloride buffer solution as buffer solvent, and alcohol water as reaction environment to prepare silica sol. The prepared silica sol has high roundness and small particle size (15-50nm), and can be applied to high-end fields such as electronics and optics. In addition, no metal ions are introduced during the reaction process, and the prepared silica sol has high purity. It does not settle and has no gelation phenomenon after being stored in a natural environment for six months, and has good stability; and no organic base is used as a catalyst, and the product separation efficiency is high.
[0023] 2. The present invention uses high-purity silicone instead of traditional silicates, which can better control the nucleation time and growth rate in the sol-gel process, produce more uniform and smaller-sized nanoparticles, and increase the upper limit of product purity, which can be applied to higher-end scenarios, such as electronic or optical applications.
[0024] 3. The method of the present invention controls the conditions of the hydrolysis and condensation reactions (such as pH value, temperature, reaction time and reactant concentration) more accurately, so that the particle size distribution and morphology of the prepared silica particles are significantly improved, and the uniformity and roundness of the dispersion of the silica particles are significantly improved.
[0025] 4. The solvent and reaction raw materials used in the present invention are environmentally friendly materials, which are more energy-saving and environmentally friendly. The raw materials are easily available and the preparation method is simple, which is more conducive to the industrialized continuous production of silica sol and has a higher output. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the microstructure of the silica sol prepared in Example 1 of the present invention;
[0027] Figure 2 This is a schematic diagram of the microstructure of the silica sol prepared in Example 2 of the present invention;
[0028] Figure 3 Schematic diagram of the microstructure of the silica sol prepared in Comparative Example 1;
[0029] Figure 4 Schematic diagram of the microstructure of the silica sol prepared in Comparative Example 2. DETAILED DESCRIPTION
[0030] The specific implementation modes of the present invention are further described in detail below in conjunction with specific examples.
[0031] The numerical ranges in the present invention are understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any intermediate value in the stated value or stated range and any other stated value or intermediate value in the stated range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0032] Unless otherwise stated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of conflict with any incorporated document, the content of this specification shall prevail. Regarding "comprising", "including", "having", "containing", etc. used herein, they are all open terms, which means including but not limited to.
[0033] Unless otherwise specified, the experimental methods used in the present invention are all conventional methods.
[0034] Unless otherwise specified, the materials, reagents, etc. used in the present invention can be purchased or synthesized by known methods.
[0035] The quantitative tests in the present invention were repeated three times and the results were averaged.
[0036] Example 1
[0037] This embodiment provides a method for preparing nano-silica sol, comprising the following steps:
[0038] S1: Prepare solution A: add 40g of methyl orthosilicate into 60g of methanol and stir at room temperature for 10min to mix the two evenly;
[0039] S2: Prepare solution B: add 5 g of ammonia / ammonium chloride buffer solution with a pH value of 9.5, 60 g of deionized water, and 35 g of methanol into a reaction container, and stir at room temperature for 10 min to mix the three evenly;
[0040] S3: Mixing: After stirring evenly, solution A is slowly and evenly added to solution B at a speed of 2 seconds per drop, and then stirred at 60° C. for 4 hours to obtain silica sol.
[0041] Stability test: The prepared silica sol is left to stand for a period of time to observe whether the silica sol will quickly settle or gel, so as to determine its stability. Experiments have shown that the silica sol prepared in this embodiment can be stored in a natural environment for six months without settling or gelling, and has good stability.
[0042] The microstructure of the silica sol prepared in this embodiment is as follows: Figure 1 As shown by Figure 1 It can be seen that the silicon dioxide particles prepared by the present invention are evenly distributed, have high roundness, and have a particle size of 15-20 nm, and can be used in high-end fields such as electronics and optics.
[0043] Example 2
[0044] This embodiment provides a method for preparing nano-silica sol, comprising the following steps:
[0045] S1: Prepare solution A: add 40g of tetraethyl orthosilicate into 60g of ethanol and stir at room temperature for 10min to mix the two evenly;
[0046] S2: Prepare solution B: add 5 g of ammonia / ammonium chloride buffer solution with a pH value of 9.5, 60 g of deionized water, and 35 g of ethanol into a reaction vessel, and stir at room temperature for 10 min to mix the three evenly;
[0047] S3: Mixing: After stirring evenly, solution A is slowly and evenly added to solution B at a speed of 2 seconds per drop, and then stirred at 60° C. for 4 hours to obtain silica sol.
[0048] Stability test: The prepared silica sol is left to stand for a period of time to observe whether the silica sol will quickly settle or gel, so as to determine its stability. Experiments have shown that the silica sol prepared in this embodiment can be stored in a natural environment for six months without settling or gelling, and has good stability.
[0049] The microstructure of the silica sol prepared in this embodiment is as follows: Figure 2 As shown by Figure 2 It can be seen that the silicon dioxide particles prepared by the present invention are evenly distributed, have high roundness, and have a particle size of 15-25 nm, and can be used in high-end fields such as electronics and optics.
[0050] Example 3
[0051] This embodiment provides a method for preparing nano-silica sol, comprising the following steps:
[0052] S1: Prepare solution A: add 10g of tetraethyl orthosilicate to 90g of ethanol and stir at room temperature for 10min to mix the two evenly;
[0053] S2: Prepare solution B: add 1g of ammonia / ammonium chloride buffer solution with a pH value of 9.5, 50g of deionized water, and 20g of ethanol into a reaction vessel, and stir at room temperature for 10min to mix the three evenly;
[0054] S3: Mixing: After stirring evenly, solution A is slowly and evenly added to solution B at a speed of 2 seconds per drop, and then stirred at 50° C. for 24 hours to obtain silica sol.
[0055] Stability test: The prepared silica sol is left to stand for a period of time to observe whether the silica sol will quickly settle or gel, so as to determine its stability. Experiments have shown that the silica sol prepared in this embodiment can be stored in a natural environment for six months without settling or gelling, and has good stability.
[0056] Example 4
[0057] This embodiment provides a method for preparing nano-silica sol, comprising the following steps:
[0058] S1: Prepare solution A: add 30g of ethyl orthosilicate into 70g of ethanol and stir at room temperature for 10min to mix the two evenly;
[0059] S2: Prepare solution B: add 10g of ammonia / ammonium chloride buffer solution with a pH value of 10.5, 70g of deionized water, and 35g of ethanol into a reaction vessel, and stir at room temperature for 10min to mix the three evenly;
[0060] S3: Mixing: After stirring evenly, solution A is slowly and evenly added to solution B at a speed of 8 seconds per drop, and then stirred at 80° C. for 4 hours to obtain silica sol.
[0061] Stability test: The prepared silica sol is left to stand for a period of time to observe whether the silica sol will quickly settle or gel, so as to determine its stability. Experiments have shown that the silica sol prepared in this embodiment can be stored in a natural environment for six months without settling or gelling, and has good stability.
[0062] Comparative Example 1
[0063] Comparative Example 1 provides a method for preparing a silica sol, comprising the following steps:
[0064] (1) diluting liquid sodium silicate with deionized water and passing it through an ion resin exchange bed (732 type strong acid styrene-based cation exchange resin) to obtain active silicate;
[0065] (2) placing active silicic acid in a beaker, adjusting the pH of the active silicic acid solution to alkaline with a 5% NaOH solution (stabilizer), heating and boiling under stirring, aging to obtain a mother liquor, and then measuring the concentration and particle size of the mother liquor for later use;
[0066] (3) Place the mother liquor in a three-necked flask, heat to boil, turn on the stirrer, and use a separatory funnel to uniformly drip active silicic acid into the flask at a certain speed. Use 5% NaOH solution to adjust the pH value of the solution to alkaline until the active silicic acid is added. After aging, obtain silica sol.
[0067] This comparative example uses sodium silicate as a raw material to prepare silica sol, which not only has complicated reaction steps and a long reaction cycle, but also Figure 3 As shown, the interface between the generated silica sol particles is unclear, the particle morphology is mostly non-spherical, the morphology cannot be controlled, and it is unstable and is prone to gelation after being placed for one month.
[0068] Comparative Example 2
[0069] Comparative Example 2 provides a method for preparing a silica sol, comprising the following steps:
[0070] S1: After 300 g of ultrapure water and 10 g of hexadecyltrimethylammonium bromide are mixed evenly, 5 g of ammonia / ammonium chloride buffer solvent with a pH value of 10.5 is added dropwise thereto, and stirred at room temperature for 10 min to mix evenly;
[0071] S2: 30 g of methyl orthosilicate was added to the above solution in three batches, 30 min / batch, and stirred at 80° C. for 4 h to obtain silica sol.
[0072] like Figure 4As shown, this method can only produce large-size silica particles with severe bonding. In addition, the soft template agent (hexadecyltrimethylammonium bromide) often contains a large amount of metal ion impurities, and the removal of the soft template agent also requires a high calcination temperature and is difficult to completely remove, resulting in the problem of high separation energy consumption.
[0073] Comparative Example 3
[0074] S1: Prepare solution A: add 40g of tetraethyl orthosilicate and 60g of ethanol into a reaction container and stir at room temperature for 10min to mix the two evenly;
[0075] S2: Prepare solution B: add 5g ammonia water, 60g deionized water and 35g ethanol into the reaction container and stir at room temperature for 10min to mix the three evenly;
[0076] S3: Mixing: After stirring evenly, solution A is slowly and evenly added to solution B at a speed of 2 seconds per drop, and then stirred at 60° C. for 4 hours to obtain silica sol.
[0077] This comparative example directly uses ammonia water as a catalyst. As the reaction proceeds, the concentration of the catalyst gradually decreases, and the pH value of the solvent system cannot be guaranteed, resulting in the generated silica sol having different particle sizes, uneven particles, low roundness, and severe adhesion.
[0078] The performance comparison of the embodiments and the comparative examples is shown in Table 1.
[0079] Table 1 Comparison of the properties of silica sols prepared in the embodiments and comparative examples
[0080]
[0081] As can be seen from Table 1, the silica sol prepared by the method of the present invention has a particle size of 15 to 50 nm, which is relatively small and can be applied to high-end fields such as electronics and optics. The prepared silica sol can be stored for 6 months in a natural environment without sedimentation and still maintains a sol state, is stable and does not gel, and has excellent stability.
[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing nano-silica sol, It is characterized in that The following steps are involved: S1: dissolving orthosilicate in alcohol, stirring and mixing evenly to obtain solution A; S2: adding a buffer solvent, deionized water and alcohol into a reaction vessel, stirring and mixing them uniformly to obtain a solution B; S3: Solution A is added evenly and slowly into solution B, and the mixture is stirred to react to obtain silica sol.
2. The method for preparing nano silica sol according to claim 1, It is characterized in that The buffer solvent is an ammonia / ammonium chloride buffer solution with a pH of 9.5 to 10.
5.
3. The method for preparing nano silica sol according to claim 1, It is characterized in that In the S1, the mass ratio of orthosilicate to alcohol is 10-40:60-90.
4. The method for preparing nano silica sol according to claim 1, It is characterized in that In the S2, the mass ratio of the buffer solvent, deionized water and alcohol is 1-10:50-70:20-35.
5. The method for preparing nano silica sol according to claim 1, It is characterized in that In the above S3, the speed of slowly adding is 2 to 8 seconds per drop.
6. The method for preparing nano silica sol according to claim 1, It is characterized in that In S3, the stirring reaction is carried out at 50-80° C. for 4-24 hours.
7. The method for preparing nano silica sol according to claim 1, It is characterized in that The orthosilicate includes methyl orthosilicate or ethyl orthosilicate.
8. The method for preparing nano silica sol according to claim 1, It is characterized in that The alcohol includes methanol or ethanol.
Citation Information
Patent Citations
Silica sol for chemical mechanical polishing as well as preparation method and application thereof
CN115924922A
Cited By
Method and system for preparing silica sol by utilizing photovoltaic wastewater
CN119683631A
A method and system for preparing silica sol using photovoltaic wastewater
CN119683631B
Method for regulating and controlling irregularity and morphology of SiO2 abrasive material through cations
CN119875586A
Nano silicon dioxide sol and preparation method thereof
CN120518085A