Method for preparing aluminum fluoride by directional conversion of surplus electrolyte of electrolytic aluminum

Through the high-temperature synthesis and leaching drying process of electrolytic aluminum surplus electrolyte and acid, the problem of excess electrolyte in the aluminum electrolysis process is solved, efficient aluminum fluoride recovery and resource recycling are achieved, and the resource utilization rate and economy of the electrolytic aluminum industry are improved. benefit.

CN118754182APending Publication Date: 2024-10-11CHINALCO ENVIRONMENTAL PROTECTION & ENERGY CONSERVATION GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411051543.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The excess electrolyte produced during the aluminum electrolysis process cannot be effectively recycled, resulting in environmental pollution risks and low resource utilization.

Method used

By performing a high-temperature synthesis reaction between the electrolytic aluminum surplus electrolyte and acid, a mixed material is generated, and then a solvent is added for leaching and drying to obtain anhydrous aluminum fluoride, thereby achieving directional conversion and recovery of the electrolyte.

Benefits of technology

This method has a short reaction process, simple operation, low cost, high product purity, reaching 90-99.5%, and high economic benefits. The filtrate can be further processed to obtain lithium carbonate and other products, which improves resource recycling in the electrolytic aluminum industry. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of electrolytic aluminum solid waste resource utilization, and discloses a method for preparing aluminum fluoride by directional conversion of an electrolytic aluminum surplus electrolyte, which comprises the following steps: mixing the electrolytic aluminum surplus electrolyte with acid, and carrying out high-temperature synthesis reaction to obtain a mixed material; adding a solvent into the mixed material for leaching, and separating after leaching to obtain filtrate and filter residues; and drying the filter residues to obtain the anhydrous aluminum fluoride. The method has the advantages of short reaction process, simple operation, low cost, high purity of the obtained reaction product, high economic benefit and potential application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource utilization of solid waste from aluminum electrolysis, and in particular to a method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis. Background Art

[0002] In the aluminum electrolysis process, the electrolyte molecular ratio gradually increases due to the long-term enrichment of lithium, sodium and potassium in the alumina raw materials in the electrolytic cell and the volatilization of sodium tetrafluoroaluminate (NaAlF4) contained in the high-temperature melt of the electrolyte. Therefore, as the electrolysis process proceeds, AlF3 raw materials need to be continuously added to the aluminum electrolytic cell. With the continuous addition of AlF3, new cryolite is continuously produced during the aluminum electrolysis process, resulting in excessive electrolyte in the cell or even overflow, so the excess electrolyte has to be discharged.

[0003] At present, the aluminum electrolysis industry's ability to absorb excess electrolyte has greatly decreased, and the ability to reuse electrolyte in aluminum electrolysis cells is extremely limited, so the problem of excess electrolyte has gradually become prominent. Every ton of primary aluminum produces about 20-25kg of excess electrolyte, the main components of which are Na3AlF6, CaF2, etc. These materials contain a large amount of fluorine, and if they are not properly handled, they will bring environmental pollution risks.

[0004] Therefore, how to cleanly and efficiently recycle and utilize the fluorine and aluminum resources in the surplus electrolyte of aluminum electrolysis, convert them into aluminum fluoride products and reuse them in the aluminum electrolysis industry to achieve high-value recycling of electrolyte resources is an urgent problem that technicians in this field need to solve. Summary of the invention

[0005] In view of this, the present invention provides a method for preparing aluminum fluoride by directional conversion of surplus electrolyte in aluminum electrolysis, so as to solve the problem that the existing excess electrolyte cannot be effectively recycled.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for preparing aluminum fluoride by directional conversion of surplus electrolyte of aluminum electrolysis comprises the following steps:

[0008] (1) mixing surplus electrolyte of aluminum electrolysis with acid and performing a high temperature synthesis reaction to obtain a mixed material;

[0009] (2) adding a solvent to the mixed material for leaching, and separating to obtain a filtrate and a filter residue after leaching;

[0010] (3) Drying the filter residue to obtain anhydrous aluminum fluoride.

[0011] Preferably, the mass ratio of the electrolytic aluminum surplus electrolyte to the acid in step (1) is 1:1.0-2.2.

[0012] Preferably, the acid is a strong acid, including at least one of concentrated sulfuric acid, concentrated nitric acid and concentrated hydrochloric acid.

[0013] Preferably, the high temperature synthesis reaction in step (1) is carried out in a closed reactor, the temperature of the high temperature synthesis reaction is 150-300° C., and the high temperature synthesis reaction time is 1-5 h.

[0014] Preferably, the ratio of the mixture to the solvent in step (2) is 1 g:(5-50) mL.

[0015] Preferably, the solvent in step (2) is water.

[0016] Preferably, the leaching temperature in step (2) is 40-100° C., and the leaching time is 0.2-2 h.

[0017] Preferably, in step (3), the drying temperature is 60-150° C., and the drying time is 8-20 h.

[0018] The present invention provides a method for preparing aluminum fluoride by directional conversion of surplus electrolyte of aluminum electrolysis. Compared with the prior art, the method has the following beneficial effects:

[0019] The method of the present invention has a short reaction process, simple operation, low cost, and a high purity of the obtained reaction product, which can reach 90-99.5%, and has high economic benefits and potential application value. In addition, if the lithium content in the surplus electrolyte of electrolytic aluminum is high, the filtrate can be further processed to obtain products such as lithium carbonate. DETAILED DESCRIPTION

[0020] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the reagents and equipment used are all commercially available. If in the following examples, specific treatment conditions and treatment methods are not clearly described, then conditions and methods known in the art can be used to process.

[0021] The present invention provides a method for preparing aluminum fluoride by directional conversion of surplus electrolyte of aluminum electrolysis, comprising the following steps:

[0022] Step S100: Mix the surplus electrolyte of aluminum electrolysis with acid, and perform a high-temperature synthesis reaction to obtain a mixed material.

[0023] In this step, the mass ratio of the electrolytic aluminum surplus electrolyte to the acid is 1:1.0-2.2, preferably 1:1.4-2.1, and further preferably 1.6-2.0; the acid is a strong acid, including at least one of concentrated sulfuric acid, concentrated nitric acid and concentrated hydrochloric acid, preferably concentrated sulfuric acid.

[0024] Optionally, the high temperature synthesis reaction is carried out in a closed reactor, the high temperature synthesis reaction temperature is 150-300°C, preferably 170-250°C, and more preferably 180-230°C; the high temperature synthesis reaction time is 1-5h, preferably 1-4h, and more preferably 1.5-3h.

[0025] It should be noted that, taking concentrated sulfuric acid as an example, during the high-temperature synthesis reaction of the excess electrolyte of electrolytic aluminum and sulfuric acid, part of the aluminum contained in the electrolyte is converted into Al2(SO4)3 and leached into the solution, and the other part of the aluminum remains in the solid phase, and its structure is converted from the original Na3AlF6 to Na5Al3F 14 With the change of reaction temperature and raw material concentration, the content of Al in Na5Al3F 14 , Na3AlF6 and Al2(SO4)3, and their phase proportions are constantly changing.

[0026] When the acid concentration is increased, the HF gas generated by the reaction reacts with Na5Al3F 14 Further reaction generates AlF3. When the amount of acid added is too much, more aluminum will be leached into the liquid phase, and the mass of the slag phase will decrease, that is, the solid phase reaction product obtained will be reduced accordingly; when the amount of acid added is too little, the structure of the reaction product is mainly Na5Al3F 14 Therefore, in the high-temperature synthesis reaction process, it is necessary to control the appropriate amount of acid and temperature conditions to convert the electrolyte into aluminum fluoride in a directional manner.

[0027] Step S200: adding a solvent to the mixed material for leaching, and separating the filtrate and the filter residue after leaching.

[0028] In this step, the ratio of the mixture to the solvent is 1 g:(5-50) mL, preferably 1 g:(10-40) mL, and more preferably 1 g:(20-30) mL; the solvent is preferably water.

[0029] Since the electrolyte will be converted into soluble substances such as Al2(SO4)3, Na2SO4 and K2SO4 during the high-temperature synthesis reaction, the role of adding water is to dissolve the above soluble substances into the medium before proceeding to the next step. If too much water is added, the amount of circulating water in the process will increase, the labor intensity will increase, and the production efficiency will be reduced; if too little water is added, the above feasible substances will not be fully dissolved in the medium, resulting in the loss of valuable metal ions.

[0030] Among them, the purpose of mixing is to make the soluble reaction product leached into the medium as much as possible, so the mixing can be as uniform as possible. Preferably, the mixing method is stirring, the leaching temperature is 40-100°C, preferably 50-100°C, and more preferably 60-80°C; the leaching time is 0.2-2h, the stirring speed is 200-500rpm, preferably 250-450rpm, and more preferably 300-450rpm; the mixing and stirring time is 0.2-2h, preferably 0.5-1.5h, and more preferably 0.6-1.2h.

[0031] Step S300: Dry the filter residue to obtain anhydrous aluminum fluoride.

[0032] In this step, the drying temperature is 60-150°C, preferably 80-120°C, and more preferably 90-110°C; the drying time is 8-20h, preferably 10-15h, and more preferably 10-12h.

[0033] The technical solutions provided by the present invention are described in detail below in conjunction with specific embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0034] The main components of the lithium-rich aluminum electrolyte in the following embodiments of the present invention include the following main components by mass percentage: F 38.35%, Al 24.11%, Na 28.5%, K 3.10%, Ca 5.31%, Mg 0.27%, and the remainder is C, O and SiO2.

[0035] Example 1

[0036] (1) 50 g of excess electrolyte from aluminum electrolysis was taken, mixed with 50 g of 98% concentrated sulfuric acid, stirred for 30 min, and then transferred to a sealed reaction container, and then reacted at 300° C. for 1 h. After the reaction was completed, a mixed material was obtained.

[0037] (2) The obtained mixture was mixed with water in a ratio of 1 g:5 mL, and then stirred at 40° C. and 500 rpm for 0.2 h. After the stirring, the mixture was filtered and separated to obtain a filtrate and a filter residue. The filter residue was dried at 150° C. for 8 h to obtain an anhydrous AlF3 product.

[0038] Example 2

[0039] (1) 50 g of excess electrolyte from aluminum electrolysis was taken, mixed with 90 g of 98% concentrated sulfuric acid and stirred for 30 min, and then transferred to a sealed reaction container, and then reacted at 200° C. for 5 h. After the reaction was completed, a mixed material was obtained.

[0040] (2) The obtained mixture was mixed with water in a ratio of 1 g:25 mL, and then stirred at 80° C. and 200 rpm for 2 h. After the stirring, the mixture was filtered and separated to obtain a filtrate and a filter residue. The filter residue was dried at 60° C. for 20 h to obtain an anhydrous AlF3 product.

[0041] Example 3

[0042] (1) 50 g of excess electrolyte from aluminum electrolysis was mixed with 110 g of 98% concentrated sulfuric acid and stirred for 30 min, then transferred to a sealed reaction vessel, and then reacted at 150° C. for 2 h. After the reaction was completed, a mixed material was obtained.

[0043] (2) The obtained mixture was mixed with water in a ratio of 1 g:50 mL, and then stirred at 100° C. and 300 rpm for 60 min. After the stirring, the mixture was filtered and separated to obtain a filtrate and a filter residue. The filter residue was dried at 100° C. for 10 h to obtain an anhydrous AlF3 product. The element contents of the obtained product are shown in Table 1.

[0044] Table 1

[0045] element Al F S Na Si Ca Fe Ni Zn Impurities content(%) 52.061 43.778 2.614 0.714 0.656 0.051 0.05 0.025 0.016 margin

[0046] The total recovery rate and recovery purity of aluminum and fluorine from electrolyte raw materials to products in Examples 1-3 were calculated. The results are shown in Table 2.

[0047] Table 2

[0048] Aluminum recovery rate / % Fluorine recovery rate / % Example 1 75.33 35.5 Example 2 70 32 Example 3 65 28

[0049] Comparative Example 1

[0050] Comparative Example 1 is substantially the same as Example 1, except that the amount of 98% concentrated sulfuric acid added in step (1) is 30 g.

[0051] Comparative Example 2

[0052] Comparative Example 2 is substantially the same as Example 1, except that the amount of 98% concentrated sulfuric acid added in step (1) is 40 g.

[0053] Comparative Example 3

[0054] Comparative Example 3 is substantially the same as Example 1, except that the amount of 98% concentrated sulfuric acid added in step (1) is 115 g.

[0055] Comparative Example 4

[0056] Comparative Example 4 is substantially the same as Example 1, except that step (1) is reacted at 130° C. for 1 h.

[0057] Comparative Example 5

[0058] Comparative Example 5 is substantially the same as Example 1, except that step (1) is reacted at 130° C. for 5 h.

[0059] Comparative Example 6

[0060] Comparative Example 6 is substantially the same as Example 1, except that step (1) is reacted at 300° C. for 0.5 h.

[0061] Comparative Example 7

[0062] Comparative Example 7 is substantially the same as Example 1, except that step (1) is reacted at 310° C. for 1 h.

[0063] Comparative Example 8

[0064] Comparative Example 8 is substantially the same as Example 1, except that the ratio of the mixed material to water in step (2) is 1 g:55 mL.

[0065] Comparative Example 9

[0066] Comparative Example 9 is substantially the same as Example 1, except that the ratio of the mixed material to water in step (2) is 1 g:3 mL.

[0067] The total recovery rates of aluminum and fluorine from electrolyte raw materials to products in Comparative Examples 1-9 were calculated, and the results are shown in Table 3.

[0068] Table 3

[0069] Aluminum recovery rate / % Fluorine recovery rate / % Comparative Example 1 <![CDATA[Without AlF3]]> / Comparative Example 2 <![CDATA[Without AlF3]]> / Comparative Example 3 60.5 20 Comparative Example 4 58.6 26.3 Comparative Example 5 62.2 28.4 Comparative Example 6 60.8 26.6 Comparative Example 7 72.5 32.5 Comparative Example 8 75.5 35.6 Comparative Example 9 72.6 33.8

[0070] It can be seen from Example 1 and Comparative Examples 1-3 that when the acid concentration is increased, the HF gas generated by the reaction reacts with Na5Al3F 14 Further reaction generates AlF3; when the amount of acid added is too much, more aluminum will be leached into the liquid phase, the mass of the slag phase will decrease, that is, the solid phase reaction product obtained will be reduced accordingly, and the fluorine recovery rate will decrease. When the amount of acid added is too little, the main structure of aluminum and fluorine elements is Na5Al3F 14 The reaction product is difficult to obtain aluminum fluoride product. In Comparative Examples 1 and 2, the sulfuric acid concentration is low, and the product obtained after the reaction is Na5Al3F 14Solid phase, no AlF3 in the product.

[0071] It can be seen from Example 1 and Comparative Examples 4-7 that during the high-temperature synthesis reaction, part of the aluminum contained in the electrolyte is converted into Al2(SO4)3 and leached into the solution, and the other part of the aluminum remains in the solid phase. When the reaction temperature is low, the structure of the solid phase product is converted from the original Na3AlF6 to Na5Al3F 14 Only under certain reaction temperature and time conditions can AlF3 products be generated. Comparative Examples 4-7 show that the lower the reaction temperature, the lower the recovery rate of aluminum and fluorine. As the reaction temperature increases, it is easier to generate AlF3 products and the recovery rate of aluminum and fluorine is higher.

[0072] It can be seen from Example 1 and Comparative Examples 8-9 that since the electrolyte will be converted into soluble substances such as Al2(SO4)3, Na2SO4 and K2SO4 during the high-temperature synthesis reaction, the purpose of adding water is to dissolve the above-mentioned soluble substances into the medium before proceeding to the next step of operation; if the amount of water added is too much, the amount of circulating water in the process will increase, the labor intensity will increase, and the production efficiency will be reduced; if the amount of water added is too little, the above-mentioned feasible substances are not fully dissolved in the medium, resulting in the loss of valuable metal ions and a decrease in the recovery rate of aluminum and fluorine.

[0073] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", "yet another embodiment", "some embodiments", "some specific embodiments", "some other specific embodiments" and the like means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0074] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis, characterized in that: The following steps are involved: (1) mixing surplus electrolyte of aluminum electrolysis with acid and performing a high temperature synthesis reaction to obtain a mixed material; (2) adding a solvent to the mixed material for leaching, and separating to obtain a filtrate and a filter residue after leaching; (3) Drying the filter residue to obtain anhydrous aluminum fluoride.

2. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1, characterized in that: The mass ratio of the surplus electrolyte of aluminum electrolysis to the acid in step (1) is 1:1.0-2.

2.

3. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1 or 2, characterized in that: The acid is a strong acid, including at least one of concentrated sulfuric acid, concentrated nitric acid and concentrated hydrochloric acid.

4. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1, characterized in that: The high temperature synthesis reaction in step (1) is carried out in a closed reactor, the temperature of the high temperature synthesis reaction is 150-300° C., and the high temperature synthesis reaction time is 1-5 hours.

5. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1, characterized in that: The usage ratio of the mixture and the solvent in step (2) is 1 g:(5-50) mL.

6. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1 or 5, characterized in that: The solvent in step (2) is water.

7. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1, characterized in that: The leaching temperature in step (2) is 40-100° C., and the leaching time is 0.2-2 h.

8. The method for preparing aluminum fluoride by directional conversion of surplus electrolyte from aluminum electrolysis according to claim 1, characterized in that: The drying temperature in step (3) is 60-150° C., and the drying time is 8-20 hours.

Citation Information

Patent Citations

  • Methods for producing aluminum trifluoride

    CN102781836A

  • Separation recycling method for aluminum electrolysis refractory electrolyte

    CN109972175A

  • Method for treating fluorine-containing waste electrolyte

    CN113149052A

  • Method for efficiently extracting lithium from lithium-rich aluminum electrolyte waste residues and preparing anhydrous aluminum fluoride

    CN113718107A

  • Method for comprehensively recycling aluminum electrolysis waste cathodes through water leaching-pressurization purification

    CN115974071A