Rigid waterproof agent as well as preparation method and application thereof
Composite polymer concrete waterproofing agents prepared by using materials such as potassium hydroxide solve the problems of easy aging and poor waterproofing effect of existing building waterproofing materials, achieve efficient and long-lasting waterproofing effects, and reduce construction costs and construction periods.
Patent Information
- Application Number
- CN202410920946.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2019-08-21
- Publication Date
- 2024-10-11
AI Technical Summary
Existing building waterproofing materials are prone to aging, have short lifespans, are high in cost and have poor waterproofing effects, making it difficult to completely solve the problem of water seepage and leakage.
A rigid waterproofing agent composed of potassium hydroxide, sodium carbonate, sodium fluoride, polyvinyl alcohol, stearic acid and triethanolamine is used to form a composite polymer concrete waterproofing agent through a specific preparation method for mixing with cement or concrete. , forming a water-increasing adsorption layer and insoluble substances to block pores and achieve impermeability and waterproofing.
It provides efficient and long-lasting waterproof performance, reduces construction costs and construction period, is suitable for basements and other places, has a 100% waterproof effect, has the same durability as cement, and is non-polluting, non-toxic and non-flammable.
Abstract
Description
[0001] This application is a divisional application with an application date of August 21, 2019, application number CN201910776080.2, and invention name “A rigid waterproofing agent and its preparation method”. Technical Field
[0002] The invention belongs to the technical field of building waterproofing and household waterproofing, and particularly relates to a rigid waterproofing agent and a preparation method and application thereof. Background Art
[0003] In the construction industry, all regions have a common problem, that is, water seepage, leakage, and moisture return in basements, roofs, and walls. At present, most of the waterproof materials on the market are flexible waterproof, that is, mainly using roll materials for waterproofing. The raw material of the roll material is asphalt. The disadvantages of this waterproof material are: high operating technology requirements, high construction costs, easy aging of the roll material, and short service life. At the same time, most of the underground waterproof materials used in the construction industry are impermeable agents, which can only play an impermeable role, but not a waterproof role in the strict sense. Due to the poor durability and easy decay of the above-mentioned flexible waterproof, and the impermeability level of the impermeable agent not meeting the standard, it is difficult for the current waterproof materials to completely overcome the problem of water seepage and leakage. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of easy aging, short life, high cost and poor waterproof effect of existing waterproof materials, and to provide a rigid waterproof agent and its preparation method and application. The rigid waterproof agent provided by the present invention has low cost, good durability, simple construction process and convenient maintenance.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A rigid waterproofing agent comprises, by weight, 15-20 kg of potassium hydroxide, 4-5 kg of sodium carbonate, 0.08-0.1 kg of sodium fluoride, 8-12 kg of polyvinyl alcohol, 80-100 kg of stearic acid and 25-35 kg of triethanolamine.
[0007] A method for preparing the above-mentioned rigid waterproofing agent, the specific steps of the method are as follows:
[0008] (1) First, pour potassium hydroxide, sodium fluoride and sodium carbonate into a high temperature resistant container, add 80-100 kg of water, stir while adding until it is evenly mixed, and set aside;
[0009] (2) Start the boiler to heat the reactor and inject 400-500 kg of water into the reactor;
[0010] (3) When the water temperature in the reactor reaches 70°C to 80°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol is dissolved and becomes transparent;
[0011] (4) Then, water is injected into the interlayer of the reactor to cool the reactor. When the water temperature in the reactor drops to 70-80°C, stearic acid is added while stirring until the stearic acid is dissolved. At this time, the water temperature should not exceed 80°C.
[0012] (5) adding the mixture obtained in step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction;
[0013] (6) The boiler stops supplying heat, the hot water in the reactor is released, water is refilled, and the temperature is circulated and cooled. At the same time, 400 kg of water is added to the reactor, and the stirring paddle continues to stir;
[0014] (7) When the temperature in the reactor drops to 30-40°C, add triethanolamine while stirring. After all the raw materials are added, saponify in the reactor for at least 12 hours to prepare the finished product.
[0015] Compared with the prior art, the present invention has the following beneficial effects: strong waterproof performance, waterproof durability is the same as cement, the operation is simple, the waterproofing operation can be completed in one time, the construction period can be shortened, and manpower, material resources and other energy can be saved. It has both anti-seepage and waterproof functions, and meets and exceeds the national testing standards in this regard. Compared with the existing waterproof materials, the present invention has the advantages of saving construction costs, speeding up the construction progress, stable and firm waterproof performance, easy to check and repair in case of special circumstances, no pollution, long service life, and the same life as cement.
[0016] The present invention can play the role of waterproofing and moisture-proofing, fills the gap of rigid waterproof products on the market, can replace traditional flexible waterproofing and anti-seepage agents, and the anti-seepage and waterproofing level reaches and exceeds the national standard. The national testing standard is that the water permeability pressure reaches 0.6-0.8Mpa, and the present invention can reach 1.8-2.5Mpa, which is in a leading position both at home and abroad. The present invention fundamentally solves the waterproofing problem, can carry water for operation, is particularly suitable for underground waterproofing and moisture-proofing, and the waterproofing effect can reach 100%.
[0017] This product is cheap, stable in performance, strong in crack resistance, has micro-expansion, and is extremely effective in controlling the plastic shrinkage, dry shrinkage, and micro-cracks caused by temperature and humidity changes in concrete, preventing and inhibiting the formation and development of cracks, and is resistant to freezing and thawing, heat-resistant and durable, wear-resistant, non-toxic and odorless, non-flammable, and non-corrosive to steel bars. The rigid waterproofing agent made from this product is easy to construct, pollution-free, and low in cost. It does not require any other waterproofing products, and can complete the waterproofing operation in one go, which shortens the construction period and saves energy. The waterproofing and anti-seepage effect of the project is reliable, and the service life is long, eliminating many worries. It is suitable for internal and external waterproofing of new and old projects of concrete structures, such as: subways, tunnels, roads, dams, water towers, vegetable cellars, etc. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is further described below in conjunction with the embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0019] The principle of waterproofing of the present invention is: a composite polymer concrete rigid waterproofing agent composed of a polymer as the main body and auxiliary agents. It can form a water-increasing adsorption layer between cement particles and slurry and generate insoluble substances, fill the tiny pores in the mortar and block the capillary channels, cut off the water seepage channels, increase the density of the mortar, and thus achieve the purpose of anti-seepage and waterproofing.
[0020] The method of using the waterproofing agent of the present invention is as follows: (1) Mixing with cement, mixing according to 1.8-2% of the cement dosage, wherein the requirements for cement are mortar waterproofing 425#; concrete waterproofing 325#; ordinary silicate or slag silicate international cement, the factory date is no more than three months, and different brands cannot be mixed. (2) Mixing with concrete, mixing according to 0.9% of the concrete dosage, the requirements for concrete raw materials: the requirements for cement are mortar waterproofing 425#; concrete waterproofing 325#; ordinary silicate or slag silicate international cement, the factory date is no more than three months, and different brands cannot be mixed; sand: medium sand, mud content <3wt.%, no debris; stone: maximum diameter <40mm, mud content <1.0%. In the specific waterproofing process, if the quality of cement or concrete meets the above requirements, the waterproofing effect is best.
[0021] The invention provides a rigid waterproofing agent, which consists of 15-20 kg of potassium hydroxide, 4-5 kg of sodium carbonate, 0.08-0.1 kg of sodium fluoride, 8-12 kg of polyvinyl alcohol, 80-100 kg of stearic acid and 25-35 kg of triethanolamine in parts by mass.
[0022] In the present invention, the rigid waterproofing agent is preferably composed of 15-20 parts of potassium hydroxide, 4-5 parts of sodium carbonate, 0.08-0.1 parts of sodium fluoride, 10 parts of polyvinyl alcohol, 80-100 parts of stearic acid, and 30 parts of triethanolamine in terms of mass fractions.
[0023] The present invention also provides a method for preparing the rigid waterproofing agent described in the above technical solution, and the specific steps of the method are as follows:
[0024] (1) First, pour potassium hydroxide, sodium fluoride and sodium carbonate into a high temperature resistant container, add 80-100 kg of water, stir while adding until the mixture is evenly mixed, and set aside; the high temperature resistant container refers to a container that can withstand a high temperature of 120°C, for example, a stainless steel tank or an enamel product;
[0025] (2) Start the boiler to heat the reactor and inject 400-500 kg of water into the reactor;
[0026] (3) When the water temperature in the reactor reaches 70°C to 80°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol melts and becomes transparent. When the polyvinyl alcohol melts and becomes transparent, it should be heated to a maximum of 100°C;
[0027] (4) Then, water (normal temperature tap water can be used) is injected into the reactor interlayer to cool the reactor. When the water temperature in the reactor drops to 70-80°C, stearic acid is added while stirring until the stearic acid is dissolved. At this time, the water temperature should not exceed 80°C.
[0028] (5) adding the mixture obtained in step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction;
[0029] (6) The boiler stops supplying heat, the hot water in the reactor is released, and water (normal temperature tap water can be used) is refilled to circulate and cool down. At the same time, 400 kg of water (normal temperature tap water can be used) is added to the reactor. At this time, the stirring paddle continues to stir;
[0030] (7) When the temperature in the reactor drops to 30-40°C, add triethanolamine while stirring. After all the raw materials are added, saponify in the reactor for at least 12 hours to prepare the finished product.
[0031] Note: Do not stir too fast, just one or one and a half turns per second, otherwise a lot of bubbles will be generated.
[0032] Example 1
[0033] A rigid waterproofing agent comprises, in parts by mass, 20 kg of potassium hydroxide, 4 kg of sodium carbonate, 0.1 kg of sodium fluoride, 10 kg of polyvinyl alcohol, 100 kg of stearic acid and 30 kg of triethanolamine.
[0034] (1) First, pour potassium hydroxide, sodium fluoride, and sodium carbonate into a high temperature resistant container, add 100 kg of water, and stir while adding until the mixture is evenly mixed, and set aside; the high temperature resistant container is a stainless steel tank;
[0035] (2) Start the boiler to heat the reactor and inject 400 kg of water into the reactor;
[0036] (3) When the water temperature in the reactor reaches 70°C to 80°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol melts and becomes transparent. When the polyvinyl alcohol melts and becomes transparent, it should be heated to a maximum of 100°C;
[0037] (4) Then, water (normal temperature tap water can be used) is injected into the reactor interlayer to cool the reactor. When the water temperature in the reactor drops to 70-80°C, stearic acid is added while stirring until the stearic acid is dissolved. At this time, the water temperature does not exceed 80°C.
[0038] (5) adding the mixture obtained in step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction;
[0039] (6) The boiler stops supplying heat, the hot water in the reactor is released, and water (normal temperature tap water can be used) is refilled to circulate and cool down. At the same time, 400 kg of water (normal temperature tap water can be used) is added to the reactor. At this time, the stirring paddle continues to stir;
[0040] (7) When the temperature in the reactor drops to 30°C, add triethanolamine while stirring. After all the raw materials are added, saponify in the reactor for at least 12 hours to prepare the finished product.
[0041] Note: Do not stir too fast, just one or one and a half turns per second, otherwise a lot of bubbles will be generated.
[0042] The rigid waterproofing agent prepared in this embodiment was used in the waterproofing project of the underground substation in Wanzhou Economic Development Zone, Chongqing, which completely solved the leakage problem.
[0043] Example 2
[0044] A rigid waterproofing agent comprises, by weight, 15 parts of potassium hydroxide, 5 parts of sodium carbonate, 0.08 parts of sodium fluoride, 10 parts of polyvinyl alcohol, 80 parts of stearic acid and 30 parts of triethanolamine.
[0045] (1) First, potassium hydroxide, sodium fluoride and sodium carbonate are poured into a high temperature resistant container, and 90 kg of water is added, stirring while adding until the mixture is uniform, and the mixture is set aside; the high temperature resistant container is made of enamel;
[0046] (2) Start the boiler to heat the reactor and inject 450 kg of water into the reactor;
[0047] (3) When the water temperature in the reactor reaches 75°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol melts and becomes transparent. When the polyvinyl alcohol melts and becomes transparent, it should be heated to a maximum of 100°C;
[0048] (4) Then, water (normal temperature tap water can be used) is injected into the reactor interlayer to cool the reactor. When the water temperature in the reactor drops to 70-80°C, stearic acid is added while stirring until the stearic acid is dissolved. At this time, the water temperature does not exceed 80°C.
[0049] (5) adding the mixture obtained in step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction;
[0050] (6) The boiler stops supplying heat, the hot water in the reactor is released, and water (normal temperature tap water can be used) is refilled to circulate and cool down. At the same time, 400 kg of water (normal temperature tap water can be used) is added to the reactor. At this time, the stirring paddle continues to stir;
[0051] (7) When the temperature in the reactor drops to 30-40°C, add triethanolamine while stirring. After all the raw materials are added, saponify in the reactor for at least 12 hours to prepare the finished product.
[0052] Note: Do not stir too fast, just one or one and a half turns per second, otherwise a lot of bubbles will be generated.
[0053] The rigid waterproofing agent of this embodiment was applied to a construction project 10,000 meters underground in Zhenbao Garden, Yanghe New District, Suqian City, Jiangsu Province, which also solved the problem of waterproof leakage. Both embodiments were water-carrying operations, which further verified the effect of the invention.
[0054] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A rigid waterproofing agent, It is characterized in that The rigid waterproofing agent is composed of 15-20 kg of potassium hydroxide, 4-5 kg of sodium carbonate, 0.08-0.1 kg of sodium fluoride, 10 kg of polyvinyl alcohol, 80-100 kg of stearic acid and 30 kg of triethanolamine in parts by mass; The specific steps of the preparation method of the rigid waterproofing agent are: (1) Pour potassium hydroxide, sodium fluoride and sodium carbonate into a high temperature resistant container, add 80-100 kg of water, and stir while adding until the mixture is uniform to obtain a mixture; (2) Start the boiler to heat the reactor and inject 400-500 kg of water into the reactor; (3) When the water temperature in the reactor reaches 70°C to 80°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol is dissolved and becomes transparent; (4) injecting water into the interlayer of the reactor to cool the reactor, and when the water temperature in the reactor drops to 70-80° C., adding stearic acid, stirring while adding, until the stearic acid is dissolved, at which time the water temperature is controlled not to exceed 80° C.; (5) adding the mixture of step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction; (6) The boiler stops supplying heat, the hot water in the reactor is released, water is refilled, and the temperature is circulated and cooled. At the same time, 400 kg of water is added to the reactor, and the stirring paddle continues to stir; (7) When the temperature in the reactor drops to 30-40° C., triethanolamine is added while stirring. After all the raw materials are added, saponification is carried out in the reactor for at least 12 hours to obtain the rigid waterproofing agent.
2. A method for preparing the rigid waterproofing agent according to claim 1, It is characterized in that The specific steps are: (1) Pour potassium hydroxide, sodium fluoride and sodium carbonate into a high temperature resistant container, add 80-100 kg of water, and stir while adding until the mixture is uniform to obtain a mixture; (2) Start the boiler to heat the reactor and inject 400-500 kg of water into the reactor; (3) When the water temperature in the reactor reaches 70°C to 80°C, add polyvinyl alcohol into the reactor, stir while adding, and continue heating until the polyvinyl alcohol is dissolved and becomes transparent; (4) injecting water into the interlayer of the reactor to cool the reactor, and when the water temperature in the reactor drops to 70-80° C., adding stearic acid, stirring while adding, until the stearic acid is dissolved, at which time the water temperature is controlled not to exceed 80° C.; (5) adding the mixture of step (1) into a reaction kettle, stirring while adding, and after all the addition is completed, maintaining the temperature at 75-80° C. for 30-40 min to carry out a saponification reaction; (6) The boiler stops supplying heat, the hot water in the reactor is released, water is refilled, and the temperature is circulated and cooled. At the same time, 400 kg of water is added to the reactor, and the stirring paddle continues to stir; (7) When the temperature in the reactor drops to 30-40° C., triethanolamine is added while stirring. After all the raw materials are added, saponification is carried out in the reactor for at least 12 hours to obtain the rigid waterproofing agent.
3. Use of the rigid waterproofing agent according to claim 1 or the rigid waterproofing agent obtained by the preparation method according to claim 2 in concrete structure engineering.
4. The use according to claim 3, It is characterized in that The concrete structure engineering includes subways, tunnels, roads, dams, water towers or vegetable cellars.
5. The use according to claim 3 or 4, It is characterized in that The application method of the rigid waterproofing agent is: mixing the rigid waterproofing agent with cement; the mass of the rigid waterproofing agent is 1.8-2% of the mass of the cement.
6. The use according to claim 3 or 4, It is characterized in that The application method of the rigid waterproof agent is: mixing the rigid waterproof agent with concrete; the mass of the rigid waterproof agent is 0.9% of the mass of the concrete.
Citation Information
Patent Citations
Preparation method of mortar and concrete waterproof agent
CN104072008A
Production method of waterproofing agent
CN104628420A
Novel penetration waterproof agent
CN105218153A