Low-alkali geopolymer concrete composite reinforced emulsion and preparation process thereof

Through the low-alkali geopolymer concrete composite reinforced emulsion, sulfate and other components are used to form a weak alkaline liquid, which solves the problems of reduced compressive strength of geopolymer concrete and danger of alkaline excitation liquid, and achieves high strength and stability. Suitable for infrastructure construction.

CN118754497APending Publication Date: 2024-10-11SHANDONG JIAOTONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410979867.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The compressive strength of existing geopolymer concrete decreases under high replacement amounts, and the high alkali content makes it corrosive to the human body and dangerous to operate. The high pH value of the alkaline excitation solution causes burns and breathing problems for operators, hindering its widespread use. application.

Method used

Develop low-alkali geopolymer concrete composite reinforced emulsion containing sulfate, ferric chloride, polyvinyl alcohol, sodium thiosulfate, tertiary complex amine, alkali metal hydroxide, magnesium fluorosilicate, and fine silica gas Gel, carboxymethyl starch ether and graphene nanosheets, with a pH value of around 8.5, form a weakly alkaline liquid to improve the mechanical properties and durability of concrete.

Benefits of technology

It reduces the dosage of strong alkali, improves the strength and stability of concrete at all ages, and solves the problems of low compressive strength and alkali return. It is suitable for different cements, water-reducing agents and admixtures, and is suitable for infrastructure construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754497A_ABST
    Figure CN118754497A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of concrete additives, and relates to a low-alkali geopolymer concrete composite reinforced emulsion and a preparation process thereof. The enhanced emulsion is prepared from the following components in parts by weight: 8 to 15 parts of sulfate, 5 to 8 parts of ferric chloride, 30 to 40 parts of polyvinyl alcohol, 5 to 12 parts of sodium thiosulfate, 1 to 5 parts of tertiary compound amine, 5 to 10 parts of alkali metal hydroxide, 3 to 8 parts of magnesium fluosilicate, 5 to 10 parts of fine silicon dioxide aerogel, 0.1 to 0.5 part of carboxymethyl starch ether, 1 to 3 parts of sodium tripolyphosphate, 1 to 5 parts of graphene nanosheet solution and 10 to 20 parts of water. The enhanced emulsion belongs to a weak base liquid additive, is green and environment-friendly, reduces the use amount of strong base, and improves the strength of the concrete in each age; the method has the advantages of good stability, low mixing amount and the like, and solves the alkali efflorescence problem; and the concrete has good adaptability with different cement, water reducing agents and admixtures, and has a wide application prospect in infrastructure construction engineering in China.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete additives and relates to a low-alkali geopolymer concrete composite reinforcing emulsion and a preparation process thereof. Background Art

[0002] In the annual industrial production, a large amount of solid waste is discharged, such as fly ash from thermal power plants, slag powder from the steel industry, and tailings from the mining industry. Therefore, how to use reasonable technical means to deal with these solid wastes and find alternatives to the "three highs" cement building materials with high pollution, high emissions and high energy consumption is a major challenge.

[0003] Geopolymer concrete has the advantages of high early strength, high temperature resistance, sulfate corrosion resistance and small drying shrinkage. It has broad application prospects in many fields such as the production of ultra-high strength materials, thermal insulation materials, fireproof materials and engineering repair materials. In order to reduce the amount of cement used, researchers at home and abroad use mineral admixtures or solid waste to partially replace cement, such as slag powder, steel slag powder, fly ash and rice husk ash. The use of geopolymer concrete can not only reduce the use of cement, or even avoid the use of cement, but also promote the resource utilization of industrial solid waste.

[0004] Although geopolymer concrete has so many advantages and broad prospects, it is still in the small-scale trial production stage and has not yet been widely used in actual projects. At present, there are serious problems that restrict the development and application of geopolymer concrete. First, too high a substitution amount will lead to a decrease in the compressive strength of concrete, which is not conducive to achieving the target requirements that geopolymer concrete should achieve. Second, most oligomers are activated by alkali, which has a high alkali content and is extremely corrosive to the human body. In addition, they have large shrinkage for concrete engineering, and the rapid hydration in the early stage leads to a large loss of strength in the later stage, and at the same time leads to a decrease in durability such as impermeability. Third, high-performance concrete or even ultra-high-performance concrete that meets the strength requirements is prepared by mixing geopolymer with alkaline activating liquid, but the alkaline activating liquid has a high pH value and high cost, which can easily cause burns or respiratory problems to operators. For example, Chinese patent CN113773028B discloses a geopolymer concrete and a preparation method thereof, which uses mineral powder, fly ash, silica fume, fine aggregate, alkali activator and composite shrinkage reducer to prepare geopolymer concrete with a compressive strength of ultra-high 150MPa, wherein the alkali activator contains too much strong alkali, which is a common defect of most current geopolymer concretes and seriously hinders the promotion and widespread use of geopolymer concrete.

[0005] Therefore, it is of great significance to develop a low-alkali geopolymer concrete composite reinforcing emulsion. Summary of the invention

[0006] In view of the deficiencies of the above-mentioned prior art, the present invention provides a low-alkali geopolymer concrete composite reinforcing emulsion and a preparation process thereof. The specific technical scheme is as follows:

[0007] The first object of the present invention is to provide a low-alkali geopolymer concrete composite reinforcement emulsion, comprising the following components in parts by weight:

[0008] 8-15 parts of sulfate, 5-8 parts of ferric chloride, 30-40 parts of polyvinyl alcohol (PVA-polyvinyl alcohol), 5-12 parts of sodium thiosulfate, 1-5 parts of tertiary complex amine, 5-10 parts of alkali metal hydroxide, 3-8 parts of magnesium fluorosilicate, 5-10 parts of fine silica aerogel, 0.1-0.5 parts of carboxymethyl starch ether, 1-3 parts of sodium tripolyphosphate, 1-5 parts of graphene nanosheet solution, and 10-20 parts of water; the mass fraction of graphene nanosheets in the graphene nanosheet solution is 2-5%.

[0009] The pH value of the low-alkali geopolymer concrete composite reinforcing emulsion of the present invention is about 8.5, and it is a weak alkaline liquid additive. The processing is relatively simple and easy to operate. In addition, no harmful substances are generated during the processing, and no harm is caused to the construction workers. It is an environmentally friendly emulsion. The reinforcing emulsion has good adaptability to different cements, water reducing agents and admixtures, and has good application prospects.

[0010] In the low-alkali geopolymer concrete composite reinforcing emulsion of the present invention, polyvinyl alcohol molecular chains combine with cement hydration products (such as calcium aluminate) to form an interface layer, and finally form a composite structure in which the polymer and the cement hydration products are cross-linked, densely filled, and mutually penetrated, so that the system is hard and dense and has a certain toughness, thereby greatly improving the mechanical properties of the binder. Alkali metal hydroxides can promote the dissolution and activation of active ingredients in geopolymers such as active silicon oxide and aluminum oxide, and react with them to generate more stable hydration products, such as hydrated calcium aluminate, hydrated calcium silicate, etc. Sulfate and sodium thiosulfate can accelerate the cement hydration and volcanic ash reaction process. Polyvinyl alcohol, sulfate, etc. also have a coupled superposition effect, which can significantly reduce the early self-shrinkage of concrete and significantly improve the strength of concrete at all ages.

[0011] The addition of tertiary complex amine can react with the hydroxyl (-OH) on the surface of cement particles to form a protective film or adsorption layer, reduce the interaction between cement particles, reduce the cohesion between particles, thereby promoting the dispersion and dissolution of cement particles, accelerating the hydration and hardening of cement, and then driving the volcanic ash reaction of geopolymer, which can not only promote coagulation, but also increase the compressive strength of geopolymer concrete, improve early strength, have a significant promoting effect, and improve mechanical strength. Carboxymethyl starch ether molecules have a network structure and are negatively charged. They will adsorb positively charged cement particles and can connect cement as a transition bridge, thereby giving the slurry a larger yield value and improving workability.

[0012] The addition of graphene nanosheets can effectively enhance the compressive and bending mechanical properties of concrete, thereby increasing the durability of concrete. Ferric chloride is mainly involved in the formation of ferroaluminate, which makes the concrete have higher density and impermeability. Fine silica aerogel has a large specific surface area and high porosity, and has good dispersibility and suspension in both water-based and solvent-based adhesives, as well as thickening, thixotropy and reinforcement effects. Sodium tripolyphosphate can promote the absorption of water in cement, improve the fluidity and ductility of cement, thereby enhancing the strength and toughness of concrete, especially increasing the flexural strength of cement and reducing the decrease rate of compressive strength. In addition, sodium tripolyphosphate can also reduce the shrinkage and crack resistance of cement concrete, thereby improving the durability of cement concrete. Magnesium fluorosilicate is mainly used as a supplementary reinforcing agent. Fluorosilicate ions react rapidly with calcium silicate, magnesium silicate and other substances existing on the surface of concrete to generate complex fluorosilicates, which can promote the reaction of silicates with calcium hydroxide, a product of cement hydration, and ultimately generate water and calcium silicate that do not expand or shrink and have stable properties, thereby improving the stability of the composite material.

[0013] Furthermore, the method for preparing the graphene nanosheet solution comprises the following steps: dissolving the graphene nanosheet in water, stirring for 4-5 minutes, and then performing ultrasonic treatment for 20-30 minutes to obtain the graphene nanosheet solution.

[0014] Furthermore, the sulfate is a complex of polyaluminum sulfate and magnesium sulfate, and the mass ratio of the polyaluminum sulfate to magnesium sulfate is 1:1; the polyaluminum sulfate is produced by Gongyi Longtai Water Purification Filler Factory, wherein aluminum oxide (Al2O3) ≥ 15.8 and iron oxide (Fe2O3) ≤ 0.2.

[0015] Polyaluminium sulfate can make the hydration product calcium sulfoaluminate generate faster, thereby accelerating the hydration and hardening of cement; magnesium sulfate can build bridges for various crystal structures of cement after hydration, thereby enhancing the strength of concrete.

[0016] Furthermore, the polyvinyl alcohol, specification PVA1788, 120 powder, Shanghai Chemical Reagent Factory.

[0017] Furthermore, the alkali metal hydroxide is any one of sodium hydroxide and potassium hydroxide.

[0018] Furthermore, the tertiary complex amine is any one or two or more of trimethylamine, tripropylamine, triisopropylamine, tri-n-butylamine, triethanolamine, tetramethylethylenediamine, and isopropyldiethylamine.

[0019] The second object of the present invention is to provide a preparation process of the low-alkali geopolymer concrete composite reinforcing emulsion, comprising the following steps:

[0020] S1: Dissolve the sulfate in water, raise the temperature to 70-80°C, add ferric chloride and sodium thiosulfate, and continue stirring for 1-2 hours to obtain solution A;

[0021] S2: Cool solution A to 60-65°C, add magnesium fluorosilicate and alkali metal oxide, and continue stirring for 0.5-1h to obtain solution B;

[0022] S3: adding carboxymethyl starch ether, sodium tripolyphosphate, tertiary complex amine, and fine silica aerogel to the solution B after returning to room temperature, and stirring for 0.5-1h to obtain solution C;

[0023] S4: Add polyvinyl alcohol and graphene nanosheet solution to solution C, control the rotation speed at 1500-2500 rpm, perform high-speed shear stirring, raise the temperature to 90-100° C. while stirring, and continue stirring for 0.5-1h until completely dissolved and dispersed to obtain a uniformly mixed solution D; the solution D is restored to room temperature to obtain a low-alkali geopolymer concrete composite reinforcing emulsion.

[0024] The low-alkali geopolymer concrete composite reinforcing emulsion of the present invention is used for preparing geopolymer concrete.

[0025] The beneficial effects of the present invention are:

[0026] The low-alkali geopolymer concrete composite reinforcing emulsion of the present invention belongs to a weak-alkali liquid additive, is green and environmentally friendly, not only reduces the amount of strong alkali used, utilizes geopolymer to partially or completely replace cement, but also can solve the problem of low strength or even strength shrinkage of geopolymer, and greatly improves the strength of concrete at all ages; at the same time, it has many advantages such as good stability, low dosage, good adaptability, etc., solves the problem of alkali reversion easily caused by alkali stimulation; and has good adaptability to different cements, water reducers and admixtures, and will have broad application prospects in the construction of my country's infrastructure such as high-speed railways, highways, water conservancy, oil wells, subways, underground passages, tunnels, mines, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1The state diagram of the low-alkali geopolymer concrete composite reinforcing emulsion prepared in the embodiment of the present invention;

[0028] Figure 2 The state diagram of the geopolymer concrete test block before freezing and thawing prepared in the embodiment of the present invention;

[0029] Figure 3 This is a diagram of the state of a test block of geopolymer concrete after freeze-thaw prepared in an embodiment of the present invention. DETAILED DESCRIPTION

[0030] The instruments, reagents, materials, etc. involved in the following embodiments, unless otherwise specified, are all conventional instruments, reagents, materials, etc. in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following embodiments, unless otherwise specified, are all conventional experimental methods, detection methods, etc. in the prior art.

[0031] Polyvinyl alcohol: molecular weight 1788, Shanghai Chemical Reagent Factory;

[0032] Sulfate: A composite of polyaluminium sulfate and magnesium sulfate in a mass ratio of 1:1. Polyaluminium sulfate is produced by the Longtai Water Purification Filler Factory in Gongyi City, wherein aluminium oxide (Al2O3) is ≥15.8 and iron oxide (Fe2O3) is ≤0.2;

[0033] Tertiary complex amine: triethanolamine;

[0034] The alkali metal hydroxide is sodium hydroxide;

[0035] Preparation of graphene nanosheet solution:

[0036] 10 g of graphene nanosheets were dissolved in 440 ml of water and stirred in the water with a stirrer for 4-5 min, and then the solution was ultrasonically treated with an ultrasonic probe for 25 min to obtain a graphene nanosheet solution.

[0037] The above substances are used in the preparation of the geopolymer concrete composite reinforcing emulsions in the following examples or comparative examples.

[0038] Example:

[0039] A low-alkali geopolymer concrete composite reinforcing emulsion, composed of the following components in parts by weight:

[0040] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 15 parts of water;

[0041] The method for preparing the low-alkali geopolymer concrete composite reinforcing emulsion comprises the following steps:

[0042] S1: Dissolve the sulfate in water, heat to 75°C, add ferric chloride and sodium thiosulfate, and stir for 2 hours to obtain solution A;

[0043] S2: Cool solution A to 65°C, add magnesium fluorosilicate and alkali metal oxide, and continue stirring for 1 hour to obtain solution B;

[0044] S3: adding carboxymethyl starch ether, sodium tripolyphosphate, tertiary complex amine, and fine silica aerogel to the solution B after returning to room temperature, and stirring for 1 hour to obtain solution C;

[0045] S4: Add polyvinyl alcohol and graphene nanosheet solution to solution C, control the rotation speed at 2500 rpm, perform high-speed shear stirring, raise the temperature to 95°C while stirring, and continue stirring for 1 hour until it is completely dissolved and dispersed to obtain a uniformly mixed solution D; the solution D is restored to room temperature to obtain a low-alkali geopolymer concrete composite reinforcement emulsion. The emulsion state is detailed in Figure 1 .

[0046] The low-alkali geopolymer concrete composite reinforcing emulsion prepared in the example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The geopolymer concrete specimen was prepared according to the "Testing Procedure for Cement and Cement Concrete for Highway Engineering" (JTG3420-2020). The specific preparation method is as follows:

[0047] G1: The mix ratio of geopolymer concrete is cement P.O42.5: mineral powder: fly ash: desulfurized gypsum: natural crushed stone (10-20mm): natural crushed stone (5-10mm): river sand: diluted reinforcing emulsion: water reducing agent = 100: 220: 100: 20: 790: 450: 500: 180: 2.5. Weigh the above materials in 8 groups of 100mm*100mm*100mm and 3 groups of 100mm*100mm*400mm for later use;

[0048] G2: First, put all materials except the diluted reinforcing emulsion and water reducing agent into the forced mixer, dry mix for 30 seconds, then add the diluted reinforcing emulsion and water reducing agent, and continue to stir for 2 minutes;

[0049] G3: Pour the concrete into the mold and vibrate it on the compaction table for at least 30 seconds, and then finish it after initial setting;

[0050] G4: Place in a standard curing room for curing at ages of 7d, 28d, 56d, and 90d, and then conduct performance tests.

[0051] The concrete performance test is carried out in accordance with the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GB / T50082-2009); the result judgment is carried out in accordance with the "Technical Specifications for Highway Bridge and Culvert Construction" (JTG / T3650-2020).

[0052] Test results:

[0053] The slump of the concrete prepared by the low-alkali geopolymer concrete composite reinforcing emulsion prepared in this example is 135 mm; after demolding, see Figure 2 The test block was well formed, with no obvious bubbles, holes, cracks, or appearance defects such as alkali reversion. The 28d compressive strength was 45.5MPa and the flexural strength was 3.9MPa. The quick freezing method (freezing for 2h and thawing for 1h) was used. When the mass loss was 5%, the number of repeated freeze-thaw cycles was 210, the compressive strength was 42.7MPa, and the strength loss rate was 6.2%. There was a pockmarked surface phenomenon. For details, see Figure 3 It can be seen that all the above indicators meet the corresponding grade requirements of C30 concrete in the "Technical Specifications for Highway Bridge and Culvert Construction" (JTG / T3650-2020).

[0054] Comparative Example 1:

[0055] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0056] 28 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 21 parts of water.

[0057] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0058] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0059] Test results:

[0060] Compared with the embodiment, the amount of polyvinyl alcohol added in this comparative example is reduced, and the water in the emulsion is relatively increased, but the overall water-cement ratio remains basically unchanged. The test block is well formed, with no obvious bubbles, holes, cracks, or obvious appearance defects such as alkali return. The 28d compressive strength is 37.5MPa, and the flexural strength is 3.2MPa. It can be seen that the compressive strength does not meet the requirement of the configuration strength of 38.8MPa. Therefore, when the amount of polyvinyl alcohol added is small, the composite structure of the polymer and the gelled hydrate cross-linked, densely filled, and interpenetrating is not sufficient.

[0061] Comparative Example 2:

[0062] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0063] 41 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 14 parts of water.

[0064] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0065] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0066] Test results:

[0067] Compared with the embodiment, the amount of polyvinyl alcohol added in this comparative example is increased, and the water in the emulsion is relatively reduced, but the overall water-cement ratio remains basically unchanged. The test block is well formed, with no obvious bubbles, holes, cracks, or obvious appearance defects such as alkali return. The 28d compressive strength is 39.5MPa, and the flexural strength is 3.5MPa. Although the compressive strength meets the requirement of the configuration strength of 38.8MPa, it is still less than when the amount is 2%-3%. Therefore, the amount of polyvinyl alcohol does not show a completely linear relationship. When the polymer content is too large, its compressive strength decreases accordingly.

[0068] Comparative Example 3:

[0069] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0070] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, and 18 parts of water.

[0071] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0072] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0073] Test results:

[0074] Compared with the embodiment, the comparative example does not add the graphene nanosheet solution, and the corresponding water increases, but does not affect the basic water-cement ratio. The test block is well formed, without obvious bubbles, holes, cracks, and appearance defects such as alkali return. The 28d compressive strength is 40.9MPa and the flexural strength is 3.6MPa. It can be seen that the graphene nanosheet solution affects the mechanical properties of geopolymer concrete to a certain extent.

[0075] Comparative Example 4:

[0076] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0077] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 6 parts of graphene nanosheet solution, and 12 parts of water.

[0078] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0079] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0080] Test results:

[0081] Compared with the embodiment, the comparative example increases the graphene nanosheet solution, and the corresponding water is reduced, but the basic water-cement ratio is not affected. The test block is well formed, without obvious bubbles, holes, cracks, and appearance defects such as alkali return. The 28d compressive strength is 45.7MPa, and the flexural strength is 3.9MPa. It can be seen that although the mechanical properties are improved by adding the graphene nanosheet solution, the magnitude is not large, and the current graphene is still expensive, and the cost performance is low under this ratio.

[0082] Comparative Example 5:

[0083] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0084] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 9 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 12 parts of water.

[0085] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0086] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0087] Test results:

[0088] Compared with the embodiment, the comparative example increases the dosage of ferric chloride by 3%, and correspondingly reduces the dosage of water, but basically does not affect the water-cement ratio. The test block is well formed, without obvious bubbles, holes, cracks, and appearance defects such as alkali return. The 28d compressive strength is 47.1MPa and the flexural strength is 3.9MPa. This is because the participation of iron ions increases the number of ferroaluminate crystals and improves the strength, but the strength increase is not obvious, and the cost performance is low.

[0089] Comparative Example 6:

[0090] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0091] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 4 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 18 parts of water.

[0092] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0093] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0094] Test results:

[0095] Compared with the embodiment, the comparative example reduces the dosage of ferric chloride by 3% and increases the dosage of water accordingly, but the water-cement ratio is basically not affected. The test block is well formed, without obvious bubbles, holes, cracks, and appearance defects such as obvious alkali return. The 28d compressive strength is 44.2MPa and the flexural strength is 3.7MPa. This is because the reduction of iron ions leads to a corresponding reduction of ferroaluminate crystals and a decrease in strength.

[0096] Comparative Example 7:

[0097] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0098] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 4 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 18 parts of water.

[0099] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0100] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0101] Test results:

[0102] Compared with the embodiment, this comparative example reduces the amount of alkali metal hydroxide added, and the water content increases accordingly, but the water-cement ratio is basically not affected. The test block is well formed, with no obvious bubbles, holes, cracks, or appearance defects such as alkali return, but the 28d compressive strength is 35.1MPa and the flexural strength is 3.1MPa. All of the above indicators are lower than the corresponding grade requirements of C30 concrete in the Technical Specifications for Highway Bridge and Culvert Construction (JTG / T3650-2020). It can be seen that in geopolymer concrete, the alkali-activated material is reduced, and the geopolymer cannot be fully activated, resulting in reduced strength.

[0103] Comparative Example 8:

[0104] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0105] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 11 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 11 parts of water.

[0106] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0107] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0108] Test results:

[0109] Compared with the embodiment, the alkali metal hydroxide in this comparative example is increased to 11 parts, and the water is reduced accordingly, but the overall water-cement ratio remains basically unchanged. The test block is well formed, without obvious bubbles, holes, cracks, but has slight appearance defects such as alkali return, and the 28d compressive strength is 46.2MPa and the flexural strength is 3.8MPa. Therefore, although the strength has increased, the amplitude is not large, and the amount of alkali metal hydroxide should be reasonably controlled.

[0110] Comparative Example 9:

[0111] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0112] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 5 parts of magnesium fluorosilicate, 4 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 19 parts of water.

[0113] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0114] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0115] Test results:

[0116] Compared with the embodiment, the comparative example has a reduced amount of fine silica aerogel to 4 parts, and the test block is well formed, with no obvious bubbles, holes, cracks, and no obvious appearance defects such as alkali reversion. The 28d compressive strength is 43.8MPa, and the flexural strength is 3.7MPa. The quick freezing method (freezing for 2h and thawing for 1h) is used. When the mass loss is 5%, the number of repeated freeze-thaw cycles is 190 times, the compressive strength is 42.7MPa, and the strength loss rate is 2.5%. It can be seen that although the above indicators meet the corresponding grade requirements of C30 concrete in the "Technical Specifications for Highway Bridge and Culvert Construction" (JTG / T3650-2020), they are weaker than the embodiment. Therefore, the filling effect and volcanic ash effect of fine silica aerogel have obviously enhanced the mechanical indicators.

[0117] Comparative Example 10:

[0118] A geopolymer concrete composite reinforcing emulsion, comprising the following components in parts by weight:

[0119] 34 parts of polyvinyl alcohol, 10 parts of sulfate, 6 parts of ferric chloride, 7 parts of sodium thiosulfate, 3 parts of tertiary complex amine, 7 parts of alkali metal hydroxide, 2 parts of magnesium fluorosilicate, 8 parts of fine silica aerogel, 0.5 parts of carboxymethyl starch ether, 1.5 parts of sodium tripolyphosphate, 3 parts of graphene nanosheet solution, and 18 parts of water.

[0120] The preparation method of the geopolymer concrete composite reinforcing emulsion is the same as that in the embodiment, and will not be repeated here.

[0121] The geopolymer concrete composite reinforcing emulsion prepared in this comparative example was diluted with water at a ratio of 2:100 to obtain a diluted reinforcing emulsion, which was used to prepare geopolymer concrete (C30). The preparation method and the detection method were the same as those in the embodiment and will not be repeated here.

[0122] Test results:

[0123] Compared with the embodiment, the magnesium fluorosilicate is reduced to 2 parts in this comparative example, and the water is increased accordingly, but the overall water-cement ratio is basically unchanged. The test block is well formed, without obvious bubbles, holes, cracks, and appearance defects such as alkali return. The 28d compressive strength is 41.2MPa, and the flexural strength is 3.5MPa. The quick freezing method (freezing 2h, melting 1h) is adopted. When the mass loss is 5%, the number of repeated freeze-thaw cycles is 153 times, and the compressive strength is 35.7MPa, and the strength loss rate is 13.3%. It can be seen that although the above indicators meet the corresponding grade requirements of C30 concrete in "Technical Specifications for Highway Bridge and Culvert Construction" (JTG / T3650-2020), the compressive strength and the strength loss after freeze-thaw are relatively fast, which is that the reduction of fluorosilicate ions leads to insufficient reaction of silicate and calcium hydroxide and reduced strength.

[0124] Comparative Example 11:

[0125] In this comparative example, geopolymer concrete (C30) was prepared without adding the geopolymer concrete composite reinforcing emulsion. The geopolymer concrete specimen was prepared according to the "Testing Procedure for Cement and Cement Concrete for Highway Engineering" (JTG3420-2020). The specific preparation method is as follows:

[0126] G1: The mix ratio of geopolymer concrete is cement P.O42.5: mineral powder: fly ash: desulfurized gypsum: natural crushed stone (10-20mm): natural crushed stone (5-10mm): river sand: water reducing agent = 100:220:100:20:790:450:500:2.5. Weigh the above materials in 8 groups of 100mm*100mm*100mm and 3 groups of 100mm*100mm*400mm for later use;

[0127] The other preparation steps are the same as those in the embodiment and will not be described again here.

[0128] Test results:

[0129] Compared with the embodiment, the water-cement ratio of this comparative example remains basically unchanged, and the workability meets the construction requirements. After 24 hours of demolding, the test block is well formed, with no obvious bubbles, holes, or cracks, but there is an obvious alkali return phenomenon. After testing, the 28d compressive strength of the control example test block is only 28.8MPa, which is only 63.2% of the compressive strength of 45.5MPa of the embodiment; the flexural strength is 2.7MPa, which is only 69.2% of the flexural strength of 3.9MPa of the embodiment. It can be seen that the main indicators of this comparative example have not met the requirements of 38.8MPa for the corresponding configuration strength of C30 concrete in the "Technical Specifications for Highway Bridge and Culvert Construction" (JTG / T3650-2020). The main reason is that the geopolymer is not fully excited, the crystal network structure is not dense enough, and the inorganic salt part is not effectively solidified, resulting in low compressive strength. It can be inferred from this that the low-alkali geopolymer concrete composite reinforcing emulsion of the present invention can effectively couple geopolymer, cement and other aggregates, and the volcanic ash reaction, complex salt reaction and hydration reaction are more complete, which can significantly improve the strength of concrete at all ages, and especially can solve the problem of alkali reversion easily caused by alkali excitation, which will effectively promote the deep resource utilization of solid waste and improve the comprehensive benefits.

[0130] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A low-alkali geopolymer concrete composite reinforcing emulsion, It is characterized in that The composition comprises the following components in parts by weight: 8-15 parts of sulfate, 5-8 parts of ferric chloride, 30-40 parts of polyvinyl alcohol, 5-12 parts of sodium thiosulfate, 1-5 parts of tertiary complex amine, 5-10 parts of alkali metal hydroxide, 3-8 parts of magnesium fluorosilicate, 5-10 parts of fine silica aerogel, 0.1-0.5 parts of carboxymethyl starch ether, 1-3 parts of sodium tripolyphosphate, 1-5 parts of graphene nanosheet solution, and 10-20 parts of water; The mass fraction of the graphene nanosheets in the graphene nanosheet solution is 2-5%.

2. The low-alkali geopolymer concrete composite reinforcement emulsion according to claim 1, It is characterized in that The method for preparing the graphene nanosheet solution comprises the following steps: placing the graphene nanosheet in water, stirring for 4-5 minutes, and then performing ultrasonic treatment for 20-30 minutes to obtain the graphene nanosheet solution.

3. The low-alkali geopolymer concrete composite reinforcing emulsion according to claim 1, It is characterized in that The sulfate is a complex of polyaluminium sulfate and magnesium sulfate in a mass ratio of 1:

1.

4. The low-alkali geopolymer concrete composite reinforcement emulsion according to claim 1, It is characterized in that The alkali metal hydroxide is any one of sodium hydroxide and potassium hydroxide.

5. The low-alkali geopolymer concrete composite reinforcement emulsion according to claim 1, It is characterized in that The tertiary complex amine is any one or two or more of trimethylamine, tripropylamine, triisopropylamine, tri-n-butylamine, triethanolamine, tetramethylethylenediamine, and isopropyldiethylamine.

6. A process for preparing the low-alkali geopolymer concrete composite reinforcing emulsion according to any one of claims 1 to 5, It is characterized in that The steps include: S1: Dissolve the sulfate in water, raise the temperature to 70-80°C, add ferric chloride and sodium thiosulfate, and continue stirring for 1-2 hours to obtain solution A; S2: Cool solution A to 60-65°C, add magnesium fluorosilicate and alkali metal oxide, and continue stirring for 0.5-1h to obtain solution B; S3: adding carboxymethyl starch ether, sodium tripolyphosphate, tertiary complex amine, and fine silica aerogel to the solution B after returning to room temperature, and stirring for 0.5-1h to obtain solution C; S4: Add polyvinyl alcohol and graphene nanosheet solution to solution C, control the rotation speed at 1500-2500 rpm, perform high-speed shear stirring, raise the temperature to 90-100° C. while stirring, and continue stirring for 0.5-1h until completely dissolved and dispersed to obtain a uniformly mixed solution D; the solution D is restored to room temperature to obtain a low-alkali geopolymer concrete composite reinforcing emulsion.

Citation Information

Patent Citations

  • Special anti-sloughing liquid coagulant for foam concrete cast-in-place wall

    CN113173729A

  • Concrete waterproof agent and preparation method thereof

    CN116283018A

  • Cement-free premixed green ultra-high performance concrete and preparation method thereof

    CN117263632A