A kind of anti-cracking waterproof mortar and preparation method thereof

Active powder is prepared through high-temperature calcination of magnesium slag, alkali slag, and high ferrosilicon tailings, and combined with materials such as silica fume, calcium carbide slag, desulfurization gypsum, etc., which solves the crack problem during mortar hardening and the low utilization rate of industrial solid waste in the mortar hardening process. , achieving efficient cracking, impermeability and waterproofing effects and environmentally friendly utilization of industrial solid waste.

CN118754528BActive Publication Date: 2024-12-03SHANDONG HUAHAN NEW BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410917565.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-12-03
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

In the prior art, mortar is prone to cracks during hardening, affecting its anti-seepage and waterproofing effect, and industrial solid waste cannot be fully reused, resulting in environmental pollution.

Method used

Use magnesium slag, alkali slag, and high ferrosilicon tailings to prepare active powders, combined with silicon fume, calcium carbide slag, and desulfurization gypsum as gelling materials, and add water reducing agent, retarder, polyethylene glycol and polyvinyl alcohol mortar with good cracking, waterproofing and waterproofing effects are prepared.

Benefits of technology

It achieves good construction performance of the mortar and anti-cracking and waterproofing effect, while improving the utilization rate of industrial solid waste, reducing production costs, and simple process and green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and in particular to a crack-resistant and waterproof mortar and a preparation method thereof. Active powder is prepared by high-temperature calcination of magnesium slag, alkali slag and high-silicon iron tailings, silica fume, carbide slag and desulfurized gypsum are used as cementitious materials, and admixtures are compounded to adjust the mortar performance. The prepared mortar has good construction performance and good crack-resistant, seepage-resistant and waterproof effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a crack-resistant and waterproof mortar and a preparation method thereof. Background Art

[0002] Mortar is a commonly used construction material in construction, water conservancy and other projects. It is generally made of cement, cementitious materials composed of admixtures, fine aggregate, admixtures and water. Due to the evaporation of water and hydration of cementitious materials, the hardened mortar often contains tiny pores, and cement hydration is a process of volume shrinkage, which often produces tiny cracks, affecting the mortar's anti-seepage and waterproofing effects.

[0003] The main methods for improving the crack resistance and waterproofness of mortar in the prior art are: 1. Adding anti-cracking fibers to use the tensile force of the fibers to resist the cracking stress of the mortar and prevent the expansion of microcracks, such as CN102190467A, CN102898102A, CN105669149A, CN117735922A, and CN112142417A. However, it is difficult to evenly disperse the fibers in the mortar and the compressive strength of the mortar will be affected. 2. Adding waterproofing agents to prevent water molecules from penetrating, such as CN103819127A, CN105271978A, and CN10667348 5A, CN115838262A, CN117285294A, however, waterproofing agents are generally organic products, which will affect the mechanical properties of mortar, 3. Adding organic polymers, nano-inorganic fillers, etc. as film-forming materials or hydration fillers to block the mortar micropores and improve the density, such as CN101811850A, CN102491709A, CN103332901A, CN112661461A, CN105236884A, CN111807795A, however, organic polymers and nano-inorganic fillers are relatively expensive, which increases the cost of mortar.

[0004] Industrial production is often accompanied by the generation of industrial solid waste. Fly ash and mineral powder commonly used in the market are often used as active mineral admixtures in cement-based building materials. However, there are still a large number of industrial solid wastes that have not been fully reused. A large amount of magnesium slag is produced during the Pijiang process of magnesium smelting. Its main chemical composition is CaO, SiO2, etc. It is rich in a certain amount of C2S minerals and has a certain hydration activity. It is often used to partially replace raw materials to prepare cement clinker or is ground and used as an admixture. Due to its low hydration activity, it is not as effective as fly ash, mineral powder, etc., so it has not been consumed in large quantities by the construction market. Alkali slag is a solid waste generated when soda ash is produced using the ammonia-soda process. Iron tailings are waste generated by mineral processing and have almost no hydration activity. They have also not been widely recycled. The storage of large amounts of industrial solid waste has a negative impact on the environment. Summary of the invention

[0005] In order to solve the problems existing in the prior art, the present invention provides a crack-resistant and waterproof mortar. Specifically, the present invention adopts magnesium slag, alkali slag, and high-silicon iron tailings to prepare active powder by high-temperature calcination, and combines silica fume, carbide slag, and desulfurized gypsum as cementitious materials, and compound admixtures to adjust the mortar performance. The prepared mortar has good construction performance and good crack-resistant, seepage-resistant and waterproof effects.

[0006] Specifically, the anti-cracking and waterproof mortar of the present invention is composed of the following raw materials in parts by weight: 320-360 parts of active powder, 80-110 parts of silica fume, 70-80 parts of carbide slag, 20-30 parts of desulfurized gypsum, 1330-1380 parts of fine aggregate, 3-6 parts of water reducer, 1-3 parts of retarder, 2-3 parts of polyethylene glycol, 1-2 parts of polyvinyl alcohol, 0.5-1 parts of defoaming agent, and 160-170 parts of water.

[0007] Preferably, the active powder preparation process is: magnesium slag, alkaline slag, and high-silicon iron tailings are uniformly mixed in a mass ratio of 1: (0.6-0.8): (0.3-0.5), ground, calcined at a high temperature of 1200-1400° C., rapidly cooled, and ball milled to obtain the active powder.

[0008] The process of producing magnesium by the Pijiang process produces a large amount of magnesium slag, the main components of which are γ-C2S, β-C2S and a small amount of MgO. Since the structure of γ-C2S is relatively stable, its hydration activity is low, and the presence of MgO makes it have the risk of poor stability, thus limiting its use as an auxiliary cementitious material. The present invention conducts a large number of experiments on the composition of industrial solid waste, and finally obtains an active powder prepared by high-temperature calcination activation using magnesium slag, alkali slag, and high-silicon iron tailings, and rapid cooling. The present invention finds that the magnesium slag, alkali slag, and high-silicon iron tailings produce mineral phase reorganization during the activation process, the active powder contains a large amount of high-activity β-C2S, the low-activity γ-C2S is reduced, and C6A4MS minerals are generated, thereby greatly improving the hydration activity of the active powder in the early and late stages. During the experiment, it was found that the active powder of the present invention has a certain micro-expansion effect, and therefore has a good anti-seepage and waterproofing effect, and does not need to add expansion agents, fibers and other additives. The reason may be that the active powder contains a small amount of active MgO.

[0009] Preferably, the chemical composition of the magnesium slag includes: CaO 60-65%, SiO2 20-25%, MgO 8-10%, Fe2O3 3-5%, Al2O3 0.5-2%, and TiO2 0.1-0.5%.

[0010] Preferably, the chemical composition of the alkali slag includes: CaO 52-60%, SiO2 13-18%, MgO 6-9%, and Al2O3 3-6%.

[0011] Preferably, the chemical composition of the high-silicon iron tailings includes: SiO2 62-72%, CaO 6-9%, MgO 7-10%, Al2O3 5-9%, and TFe 10-12%.

[0012] In the process of preparing the active powder of the present invention, magnesium slag, alkali slag and high silicon iron tailings all contain MgO, and the high silicon iron tailings can supplement a large amount of SiO2, which is beneficial to the formation of the C6A4MS mineral phase, the alkali slag provides CaO, and the magnesium slag contains some CaF2, which can play a certain fluxing effect. The Fe2O3 contained in the high silicon iron tailings can be dissolved in the activation process to change the crystal structure of calcium silicate, and can also play a certain mineralization and stabilization role, thereby reducing the content of free MgO.

[0013] Preferably, the powder is ground to a particle size of ≤90 μm, and ball-milled to a particle size of ≤20 μm.

[0014] Preferably, the high temperature calcination time is 1-2 hours.

[0015] Preferably, the extreme cooling adopts at least one of air cooling and water cooling.

[0016] The active powder prepared by the present invention has high activity. In order to meet the needs of mechanical properties, the present invention has been subjected to a large number of experimental studies, and the active powder is blended with silica fume to increase the content of hydrated calcium silicate, and calcium carbide slag and desulfurized gypsum are used for excitation to increase the amount of calcium sulfonate generated, which can completely replace cement as a cementitious material. In order to improve the anti-seepage effect and construction performance, the present invention adds a water reducer to reduce the amount of water used, and adds a retarder to increase the open time, and adds a defoamer to eliminate harmful large bubbles generated during the mortar mixing process. In order to cooperate with the use of the active powder, the present invention adds polyethylene glycol and polyvinyl alcohol for compounding, which can overcome the problem of reduced construction performance caused by the active powder and improve the workability of the mortar. In addition, experiments show that the addition of polyethylene glycol and polyvinyl alcohol can increase the density of the mortar, increase the density of the active powder and silica fume hydration products, block water seepage micropores, and improve the anti-seepage and waterproof effects.

[0017] Preferably, the fine aggregate is selected from at least one of river sand and machine-made sand, and has a fineness modulus of 2.2-2.4.

[0018] Preferably, the water reducing agent is a polycarboxylic acid water reducing agent, and the water reducing rate is ≥25%.

[0019] Preferably, the retarder is selected from at least one of sodium gluconate, borax and sucrose.

[0020] Preferably, the defoamer is a silicone defoamer.

[0021] The present invention also relates to a method for preparing the above-mentioned anti-cracking and waterproof mortar, which specifically comprises the following steps:

[0022] 1) Weigh each raw material by mass.

[0023] 2) Add active powder, silica fume, carbide slag and desulfurized gypsum into the mixer and mix well.

[0024] 3) Add fine aggregate to the mixer and mix well.

[0025] 4) Add water reducing agent, retarder, polyethylene glycol, polyvinyl alcohol and defoamer into water to obtain liquid material.

[0026] 5) Add the liquid into the blender and mix well.

[0027] The present invention has the following technical advantages:

[0028] 1. The active powder is highly active and has a micro-expansion effect. It can be used as a cementitious material with silica fume, carbide slag and desulfurized gypsum, which can completely replace cement and improve the utilization rate of industrial solid waste.

[0029] 2. The compound admixture of the present invention has good adaptability, can improve the activity and density of mortar, improve the mechanical properties of mortar and the anti-seepage and waterproof effect.

[0030] 3. The present invention adopts all-solid waste-based cementitious materials, which are green and environmentally friendly, have a simple preparation process, and have good anti-cracking and waterproof effects. DETAILED DESCRIPTION

[0031] In order to characterize the technical effect of the present invention, mortar was prepared and its performance was tested. The waterproof effect was tested using the water penetration resistance grade test method in GB / T50082. The free expansion rate "+" represents micro-expansion, and "-" represents contraction.

[0032] During the test, standard curing was used for the specimens.

[0033] Example 1

[0034] The mortar is composed of the following raw materials in parts by weight: 330 parts of active powder, 110 parts of silica fume, 80 parts of carbide slag, 20 parts of desulfurized gypsum, 1350 parts of river sand, 5 parts of polycarboxylic acid water reducer, 2 parts of sodium gluconate, 3 parts of polyethylene glycol, 1 part of polyvinyl alcohol, 0.8 parts of organosilicon defoamer, and 165 parts of water.

[0035] The active powder preparation process is as follows: magnesium slag, alkaline slag and high silicon iron tailings are uniformly mixed in a mass ratio of 1:0.7:0.3, ground to a particle size of ≤90 μm, calcined at 1300° C. for 2 h, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0036] After testing, the initial fluidity of the mortar is 260mm, the 1h fluidity is 220mm, the workability is good, the 3d compressive strength is 17.3MPa, the 3d flexural strength is 2.4MPa, the 28d compressive strength is 46.5MPa, the 28d flexural strength is 5.2MPa, the 3d free expansion rate is +0.02%, the 7d free expansion rate is +0.05%, the 28d free expansion rate is +0.06%, and the specimen water-resistance grade is P10.

[0037] Example 2

[0038] The mortar is composed of the following raw materials in parts by weight: 350 parts of active powder, 90 parts of silica fume, 70 parts of carbide slag, 30 parts of desulfurized gypsum, 1350 parts of river sand, 6 parts of polycarboxylic acid water reducer, 2 parts of borax, 2 parts of polyethylene glycol, 2 parts of polyvinyl alcohol, 0.7 parts of organosilicon defoamer, and 165 parts of water.

[0039] The active powder preparation process is as follows: magnesium slag, alkaline slag and high silicon iron tailings are uniformly mixed in a mass ratio of 1:0.6:0.5, ground to a particle size of ≤90 μm, calcined at 1350° C. for 1.5 h, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0040] After testing, the initial fluidity of the mortar is 250mm, the 1h fluidity is 230mm, the workability is good, the 3d compressive strength is 19.6MPa, the 3d flexural strength is 2.7MPa, the 28d compressive strength is 48.2MPa, the 28d flexural strength is 5.6MPa, the 3d free expansion rate is +0.01%, the 7d free expansion rate is +0.04%, the 28d free expansion rate is +0.05%, and the specimen water-resistance grade is P10.

[0041] Comparative Example 1

[0042] The mortar is composed of the following raw materials in parts by weight: 330 parts of fly ash, 110 parts of mineral powder, 80 parts of carbide slag, 20 parts of desulfurized gypsum, 1350 parts of river sand, 5 parts of polycarboxylic acid water reducer, 2 parts of sodium gluconate, 3 parts of polyethylene glycol, 1 part of polyvinyl alcohol, 0.8 parts of silicone defoamer and 165 parts of water.

[0043] After testing, the initial fluidity of the mortar is 220mm, the 1h fluidity is 180mm, the workability is good, the 3d compressive strength is 9.3MPa, the 3d flexural strength is 1.1MPa, the 28d compressive strength is 32.5MPa, the 28d flexural strength is 3.2MPa, the 3d free expansion rate is -0.03%, the 7d free expansion rate is -0.06%, the 28d free expansion rate is -0.08%, and the specimen water resistance grade is P4.

[0044] Comparative Example 2

[0045] The mortar is composed of the following raw materials in parts by weight: 330 parts of active powder, 110 parts of fly ash, 80 parts of calcium carbide slag, 20 parts of desulfurized gypsum, 1350 parts of river sand, 5 parts of polycarboxylic acid water reducer, 2 parts of sodium gluconate, 3 parts of polyethylene glycol, 1 part of polyvinyl alcohol, 0.8 parts of organosilicon defoamer, and 165 parts of water.

[0046] The active powder preparation process is as follows: coal gangue, alkali slag and high-silicon iron tailings are uniformly mixed in a mass ratio of 1:0.7:0.3, ground to a particle size of ≤90 μm, calcined at 1300° C. for 2 hours, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0047] After testing, the initial fluidity of the mortar is 240mm, the 1h fluidity is 190mm, the workability is good, the 3d compressive strength is 12.9MPa, the 3d flexural strength is 1.7MPa, the 28d compressive strength is 36.3MPa, the 28d flexural strength is 3.5MPa, the 3d free expansion rate is -0.03%, the 7d free expansion rate is -0.05%, the 28d free expansion rate is -0.07%, and the specimen water resistance grade is P4.

[0048] Comparative Example 3

[0049] The mortar is composed of the following raw materials in parts by weight: 330 parts of active powder, 110 parts of silica fume, 100 parts of carbide slag, 1350 parts of river sand, 5 parts of polycarboxylic acid water reducer, 2 parts of sodium gluconate, 3 parts of polyethylene glycol, 1 part of polyvinyl alcohol, 0.8 parts of organosilicon defoamer, and 165 parts of water.

[0050] The active powder preparation process is as follows: magnesium slag, fly ash and iron tailings are uniformly mixed in a mass ratio of 1:0.7:0.3, ground to a particle size of ≤90 μm, calcined at 1300° C. for 2 h, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0051] After testing, the initial fluidity of the mortar was 230mm, with slight bleeding, no fluidity after 1h, 3d compressive strength was 14.7MPa, 3d flexural strength was 1.6MPa, 28d compressive strength was 33.0MPa, 28d flexural strength was 2.9MPa, 3d free expansion rate was +0.01%, 7d free expansion rate was -0.03%, 28d free expansion rate was -0.08%, and the specimen water-resistance grade was P6.

[0052] Comparative Example 4

[0053] The mortar is composed of the following raw materials in parts by weight: 330 parts of active powder, 110 parts of mineral powder, 80 parts of carbide slag, 20 parts of desulfurized gypsum, 1350 parts of river sand, 6 parts of polycarboxylate water reducer, 2 parts of sodium gluconate, 0.8 parts of organosilicon defoamer, and 165 parts of water.

[0054] The active powder preparation process is as follows: magnesium slag, alkaline slag and high silicon iron tailings are uniformly mixed in a mass ratio of 1:0.7:0.3, ground to a particle size of ≤90 μm, calcined at 1300° C. for 2 h, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0055] After testing, the initial fluidity of the mortar was 190mm, it was compacted, had no fluidity after 1h, the compressive strength at 3d was 15.1MPa, the flexural strength at 3d was 1.3MPa, the compressive strength at 28d was 39.8MPa, the flexural strength at 28d was 4.2MPa, the free expansion rate at 3d was -0.02%, the free expansion rate at 7d was +0.01%, the free expansion rate at 28d was +0.03%, and the specimen’s water resistance grade was P4.

[0056] Comparative Example 5

[0057] The mortar is composed of the following raw materials in parts by weight: 330 parts of active powder, 110 parts of silica fume, 80 parts of carbide slag, 20 parts of desulfurized gypsum, 1350 parts of river sand, 5 parts of polycarboxylate water reducer, 2 parts of sodium gluconate, 4 parts of polyvinyl alcohol, and 165 parts of water.

[0058] The active powder preparation process is as follows: magnesium slag, alkaline slag and high silicon iron tailings are uniformly mixed in a mass ratio of 1:0.7:0.3, ground to a particle size of ≤90 μm, calcined at 1300° C. for 2 h, rapidly cooled, and ball-milled to a particle size of ≤20 μm.

[0059] After testing, the initial fluidity of the mortar was 240mm, with slight bleeding, the fluidity after 1h was 170mm, the compressive strength at 3d was 15.9MPa, the flexural strength at 3d was 1.8MPa, the compressive strength at 28d was 40.4MPa, the flexural strength at 28d was 4.5MPa, the free expansion rate at 3d was +0.01%, the free expansion rate at 7d was +0.03%, the free expansion rate at 28d was +0.04%, and the water resistance grade of the specimen was P8.

[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A crack-resistant waterproof mortar, characterized in that: The invention is composed of the following raw materials in parts by weight: 320-360 parts of active powder, 80-110 parts of silica fume, 70-80 parts of carbide slag, 20-30 parts of desulfurized gypsum, 1330-1380 parts of fine aggregate, 3-6 parts of water reducer, 1-3 parts of retarder, 2-3 parts of polyethylene glycol, 1-2 parts of polyvinyl alcohol, 0.5-1 parts of defoamer, and 160-170 parts of water. The active powder preparation process is as follows: magnesium slag, alkaline slag and high silicon iron tailings are mixed uniformly in a mass ratio of 1: (0.6-0.8): (0.3-0.5), ground, calcined at a high temperature of 1200-1400° C., rapidly cooled, and ball milled to obtain the active powder.

2. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The chemical composition of the magnesium slag includes: CaO 60-65%, SiO2 20-25%, MgO 8-10%, Fe2O3 3-5%, Al2O3 0.5-2%, and TiO2 0.1-0.5%.

3. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The chemical composition of the alkali slag includes: CaO 52-60%, SiO2 13-18%, MgO 6-9%, and Al2O3 3-6%.

4. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The chemical composition of the high-silicon iron tailings includes: SiO2 62-72%, CaO 6-9%, MgO 7-10%, Al2O3 5-9%, and TFe 10-12%.

5. The anti-cracking and waterproof mortar according to claim 1, characterized in that: Grind to particle size ≤90μm, ball mill to particle size ≤20μm.

6. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The fine aggregate is selected from at least one of river sand and machine-made sand, and has a fineness modulus of 2.2-2.

4.

7. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent, and the water reducing rate is ≥25%.

8. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The retarder is selected from at least one of sodium gluconate, borax and sucrose.

9. The anti-cracking and waterproof mortar according to claim 1, characterized in that: The defoamer is an organosilicon defoamer.

10. The method for preparing the crack-resistant and waterproof mortar according to any one of claims 1 to 9, characterized in that: The steps include: 1) Weigh each raw material by mass. 2) Add active powder, silica fume, carbide slag and desulfurized gypsum into the mixer and mix evenly. 3) Add fine aggregate to the mixer and mix well. 4) Add water reducing agent, retarder, polyethylene glycol, polyvinyl alcohol and defoamer into water to obtain liquid material. 5) Add the liquid into the blender and mix well.