Preparation method of wet oxidation copper-clad ceramic substrate

The wet oxidation method uses potassium permanganate oxidation solution to process copper sheets, which solves the problems of uneven oxide layer and high cost in the existing oxidation technology, improves the sintering yield and surface quality of copper-clad ceramic substrates, and meets the requirements Meets the needs of a variety of grains and roughness.

CN118754699AActive Publication Date: 2024-10-11NINGBO JIANGFENG TONGXIN SEMICON MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411030930.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing thermal oxidation and electrolytic oxidation technologies result in uneven oxide layers of copper-clad ceramic substrates, high costs and low sintering yields, making it difficult to meet the needs of different grains and roughness.

Method used

The wet oxidation method is used to anneal, clean, pre-bend and oxidize the copper sheets using potassium permanganate oxidizing solution (concentration: 3-5%), and then co-sintered with the ceramic sheets to optimize the surface of the copper substrate and improve the sintering quality. efficiency and reduce production costs.

Benefits of technology

Through the wet oxidation method, the surface quality of the copper-clad ceramic substrate is improved, the sintering yield is improved, the requirements for different grains and roughness are met, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a preparation method of a wet oxidation copper-clad ceramic substrate, and the preparation method comprises the steps: sequentially carrying out annealing treatment, cleaning treatment and pre-bending treatment on a copper sheet to obtain a pre-bent copper sheet, placing the pre-bent copper sheet in a carrier, adding an oxidation liquid into the carrier for oxidation treatment to obtain a copper oxide sheet, and carrying out wet oxidation treatment on the copper oxide sheet to obtain the wet oxidation copper-clad ceramic substrate. Placing the copper oxide sheet on the surface of a ceramic sheet for sintering to obtain a copper-clad ceramic substrate; wherein the oxidation liquid is potassium permanganate oxidation liquid, and the concentration of the potassium permanganate oxidation liquid is 3-5%. Through specific design of the preparation method of the copper-clad ceramic substrate, a wet copper oxide sheet mode is adopted, a foundation is laid for subsequent preparation of the copper-clad ceramic substrate, the surface of the copper substrate is integrally improved, the product sintering yield is improved, the production cost is reduced, and the requirements of different crystal grains and roughness can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper-clad ceramic substrate preparation, and relates to a method for preparing a wet-oxidized copper-clad ceramic substrate. Background Art

[0002] With the development of power semiconductors, the demand for copper-clad ceramic substrates is increasing. Currently, the pre-oxidation of copper sheets of copper-clad ceramic substrates is carried out by thermal oxidation.

[0003] The prior art solution discloses a new process for removing oxide scale from the surface of copper alloy wire. The cleaning system used in the process includes copper alloy wire, a winder, an unwinder, a base plate and a cleaning module, wherein a cleaning module is provided in the middle of the base plate; the cleaning module includes an extrusion connecting rod, a sleeve, a bracket, a weight and a support wheel; the brackets are symmetrically fixedly installed on the base plate; a through groove is provided in the middle of the brackets, and a horizontal plate is fixedly connected to the top of the two brackets; the support wheels are hinged in the through grooves; a sleeve is connected to the outer ring of the copper alloy wire; an extrusion connecting rod is provided on the outer ring of the sleeve; the top of the extrusion connecting rod is connected to the horizontal plate by a spring, and the bottom of the extrusion connecting rod is connected to the weight block by a spring; a support plate is provided on both sides of the extrusion connecting rod; a group of protrusions are provided on the side of the support plate close to the extrusion connecting rod.

[0004] The prior art solution discloses a method for improving the oxidation of the copper surface of a copper-clad ceramic substrate after welding, and uses processes such as pickling, water washing, alkali washing, water washing, and drying to remove the anti-oxidation film, thereby achieving the effect of preventing the copper-clad ceramic substrate from being oxidized after welding on the client side. At the same time, modified silicon dioxide is added during the pickling process to prevent concentrated sulfuric acid from corroding the copper plate and affecting its performance. However, a copper-clad ceramic substrate without an anti-oxidation layer will cause color difference on the copper surface. Under long-term transportation and moisture contact, the copper-clad ceramic substrate will oxidize and other problems. This invention solves this problem through a nitrogen baking process.

[0005] The prior art solution discloses the preparation and application of a partially oxidized silver-plated copper-clad substrate, wherein chemical silver deposition is performed on a copper-clad ceramic substrate to obtain a chemical silver deposition layer with a thickness of 5 to 10 μm; after the copper-clad ceramic substrate is subjected to a film lamination operation, a silver-plated substrate is obtained by electroplating silver or welding a silver solder sheet; an electrolytic oxidation solution is used to electrically oxidize the surface of the exposed silver layer, and after cleaning and drying, the partially oxidized silver-plated copper-clad substrate is obtained by thermal sintering.

[0006] However, the current thermal oxidation and electrolytic oxidation will result in uneven oxidation layer due to the influence of equipment temperature, oxidation atmosphere, electrolysis parameters, etc., which will easily lead to bubbles during sintering, and the cost of oxidation is high. Therefore, it is urgent to design a preparation method for wet oxidation copper-clad ceramic substrates to overcome the defects of the existing technology and meet the needs of practical applications. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a wet-oxidized copper-clad ceramic substrate. In the present invention, through the specific design of the preparation method of the copper-clad ceramic substrate, the wet-oxidized copper sheet is used to lay the foundation for the subsequent preparation of the copper-clad ceramic substrate, improve the surface of the copper substrate as a whole, improve the product sintering yield, reduce the production cost, and meet the requirements of different grains and roughness.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing a wet-oxidized copper-clad ceramic substrate, the preparation method comprising:

[0010] The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet;

[0011] Placing the pre-bent copper sheet in a carrier, adding an oxidizing liquid into the carrier for oxidation treatment, and obtaining an oxidized copper sheet;

[0012] Placing the copper oxide sheet on the surface of the ceramic sheet for sintering to obtain a copper-clad ceramic substrate;

[0013] Among them, the oxidizing liquid is potassium permanganate oxidizing liquid, and the concentration of potassium permanganate oxidizing liquid is 3-5%, for example, it can be 3%, 3.5%, 4%, 4.5%, 5%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] In the present invention, through the specific design of the preparation method of the copper-clad ceramic substrate, the wet oxidation copper sheet method is adopted to lay the foundation for the subsequent preparation of the copper-clad ceramic substrate, improve the surface of the copper substrate as a whole, improve the product sintering yield, reduce the production cost, and meet the requirements of different grains and roughness.

[0015] It should be noted that, in traditional dry oxidation, the oxide layer is uneven, the oxidation cost is high, the oxidation production efficiency is low, the surface roughness and grain size do not meet customer requirements, and the yield rate of the sintered substrate is low; the present invention uses a potassium permanganate oxidation solution with a concentration of 3-5% to oxidize the copper sheet, which can improve the surface of the copper-clad substrate, increase the product yield, and reduce production costs compared to dry oxidation.

[0016] It should be noted that the shape, size, material, etc. of the carrier in the present invention are not particularly limited. The carrier is mainly used to place copper sheets, and its shape and size can be consistent with the copper sheets. Those skilled in the art can make adaptive adjustments according to actual conditions.

[0017] As a preferred technical solution of the present invention, the annealing treatment is carried out under vacuum or protective atmosphere.

[0018] Preferably, the protective atmosphere is any one of nitrogen, helium or argon, or a combination of at least two of them.

[0019] It should be noted that the protective atmosphere in the present invention may also be other inert gas atmospheres, such as neon gas.

[0020] As a preferred technical solution of the present invention, the temperature of the annealing treatment is 400-500°C, for example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] The annealing temperature in the present invention is 400-500° C. because within this range, the oxidation effect of the copper sheet is optimal. If it is not within this range, the temperature is too low and the copper sheet cannot be softened. If the temperature is too high, the copper sheet will stick.

[0022] Preferably, the annealing time is 60 to 120 min, for example, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] The annealing time in the present invention is 60 to 120 minutes because within this range, the copper sheet cleaning effect is not good. If it is not within this range, the time is too short and the copper sheet is not fully softened; if the time is too long, the efficiency is too low.

[0024] As a preferred technical solution of the present invention, the cleaning process is carried out in the following manner:

[0025] The annealed copper sheet is rinsed and ultrasonically cleaned in sequence.

[0026] As a preferred technical solution of the present invention, the flushing liquid used in the flushing treatment is a mixture of acidic degreasing agent, sulfuric acid and hydrogen peroxide.

[0027] Preferably, in the mixed liquid, the mass ratio of the acidic degreaser, the sulfuric acid and the hydrogen peroxide is (5-6):(10-12):(80-85), for example, it can be 5:10:85, 5:10:12, 5.5:11:82, 5.5:12:81, 6:10:83, 6:11:84, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] It should be noted that the rinse liquid in the present invention is a mixture of an acidic degreasing agent, sulfuric acid and hydrogen peroxide, and the mass ratio is limited to (5-6):(10-12):(80-85) because the oxidation effect of the copper sheet is optimal within this range. If it is not within this range, the cleaning effect of the copper sheet will be poor, affecting the oxidation results.

[0029] It should be noted that the acidic degreasing agent in the present invention is well known to those skilled in the art. It is prepared from a variety of surfactants and is a non-toxic, odorless, non-flammable neutral liquid. When added to the pickling solution, it can not only remove oil but also promote the dissolution of rust and slow down the corrosion of the acid on the base metal.

[0030] As a preferred technical solution of the present invention, pure water is used for the ultrasonic cleaning.

[0031] It should be noted that the pure water in the present invention can be purified water, which is made from water that meets the sanitary standards for drinking water as raw water, through electrodialysis, ion exchange, reverse osmosis, distillation and other appropriate processing methods, and is sealed in a container and does not contain any additives. It is colorless and transparent and can be drunk directly.

[0032] Preferably, the ultrasonic cleaning time is 5 to 10 minutes, for example, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] As a preferred technical solution of the present invention, the pre-bending process is performed in the following manner:

[0034] The cleaned copper sheet is placed in a pre-bending mold for press bending.

[0035] It should be noted that the shape, size, material, etc. of the pre-bending mold in the present invention are not particularly limited. The pre-bending mold is mainly used to place the copper sheet and press the copper sheet according to its curvature. Its shape, size and copper sheet can be consistent. Technical personnel in this field can make adaptive adjustments according to actual conditions.

[0036] Preferably, the curvature of the pre-bent copper sheet is R100-R300mm, for example, it can be R100mm, R130mm, R150mm, R180mm, R200mm, R220mm, R260mm, R300mm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] The curvature of the pre-bent copper sheet in the present invention is R100-R300 mm because within this range, the oxidation effect of the copper sheet is optimal. If it is not within this range, bubbles will be generated when the copper sheet is sintered.

[0038] As a preferred technical solution of the present invention, the temperature of the oxidation treatment is 30-50°C, for example, it can be 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] The oxidation treatment temperature in the present invention is 30-50° C. because within this range, the oxidation effect of the copper sheet is optimal. If it is not within this range, the oxidation effect of the copper sheet is poor due to the high temperature, and the oxidation effect of the copper sheet cannot be achieved due to the low temperature.

[0040] Preferably, the oxidation treatment time is 20 to 60 s, for example, 20 s, 25 s, 30 s, 35 s, 40 s, 45 s, 50 s, 55 s, 60 s, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, after the oxidation treatment, the copper oxide sheet needs to be dried.

[0042] Preferably, the drying treatment time is 5 to 10 minutes, for example, it can be 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the temperature of the drying treatment is 70-80°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] As a preferred technical solution of the present invention, the surface area of ​​the copper oxide sheet is smaller than the surface area of ​​the ceramic sheet.

[0045] Preferably, the sintering temperature is 1065-1080°C, for example, it can be 1065°C, 1068°C, 1070°C, 1072°C, 1074°C, 1076°C, 1078°C, 1080°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] The sintering temperature in the present invention is 1065-1080°C because within this range, the product yield is the highest. If it is not within this range, the temperature is too low and the eutectic reaction of copper-ceramic cannot be carried out. If the temperature is too high, the product is easily deformed.

[0047] Preferably, the sintering time is 30 to 60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, during sintering, the oxygen content in the sintering furnace is less than 50 ppm, for example, it can be 20 ppm, 25 ppm, 30 ppm, 35 ppm, 40 ppm, 45 ppm, 50 ppm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] The oxygen content in the sintering furnace in the present invention is lower than 50 ppm because within this range, the yield rate of the product is the highest. Since sintering is performed under oxygen-free or micro-oxygen environment conditions, exceeding the range will cause abnormal sintering of the product.

[0050] As a preferred technical solution of the present invention, the preparation method specifically comprises:

[0051] The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet;

[0052] Placing the pre-bent copper sheet in a carrier, adding an oxidizing liquid into the carrier for oxidation treatment, and obtaining an oxidized copper sheet;

[0053] Placing the copper oxide sheet on the surface of the ceramic sheet and co-sintering to obtain a copper-clad ceramic substrate;

[0054] Wherein, the oxidizing liquid is potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 3-5%;

[0055] The annealing treatment is carried out in vacuum or in a protective atmosphere, wherein the protective atmosphere is any one of nitrogen, helium or argon or a combination of at least two thereof;

[0056] The annealing temperature is 400-500°C, and the annealing time is 60-120 minutes;

[0057] The cleaning process is carried out in the following manner: the annealed copper sheet is sequentially rinsed and ultrasonically cleaned;

[0058] The rinsing liquid used in the rinsing treatment is a mixture of an acidic degreasing agent, sulfuric acid and hydrogen peroxide. In the mixture, the mass ratio of the acidic degreasing agent, the sulfuric acid and the hydrogen peroxide is (5-6):(10-12):(80-85);

[0059] The ultrasonic cleaning uses pure water, and the ultrasonic cleaning time is 5 to 10 minutes;

[0060] The pre-bending process is performed as follows: the cleaned copper sheet is placed in a pre-bending mold for press bending;

[0061] The curvature of the pre-bent copper sheet is R100-R300mm;

[0062] The temperature of the oxidation treatment is 30 to 50° C., and the time of the oxidation treatment is 20 to 60 seconds;

[0063] After the oxidation treatment, the copper oxide sheet needs to be dried for 5 to 10 minutes at a temperature of 70 to 80° C.

[0064] The surface area of ​​the copper oxide sheet is smaller than that of the ceramic sheet. The sintering temperature is 1065-1080° C., the sintering time is 30-60 minutes, and during sintering, the oxygen content in the sintering furnace is lower than 50 ppm.

[0065] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] In the present invention, through the specific design of the preparation method of the copper-clad ceramic substrate, the wet oxidation copper sheet method is adopted to lay the foundation for the subsequent preparation of the copper-clad ceramic substrate, improve the surface of the copper substrate as a whole, improve the product sintering yield, reduce the production cost, and meet the requirements of different grains and roughness. DETAILED DESCRIPTION

[0068] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0069] Example 1

[0070] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, wherein:

[0071] The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet; the pre-bent copper sheet is placed in a carrier, and an oxidizing liquid is added into the carrier for oxidation treatment to obtain an oxidized copper sheet; the oxidized copper sheet is placed on the surface of a ceramic sheet and co-sintered to obtain a copper-clad ceramic substrate; wherein the oxidizing liquid is a potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 3%.

[0072] The annealing treatment is carried out under vacuum, the annealing temperature is 500° C., and the annealing time is 60 min.

[0073] The cleaning treatment is carried out as follows: the annealed copper sheet is rinsed and ultrasonically cleaned in sequence; the rinsing liquid used in the rinsing treatment is a mixture of an acidic degreaser, sulfuric acid and hydrogen peroxide, in which the mass ratio of the acidic degreaser, sulfuric acid and hydrogen peroxide is 5:10:85; pure water is used for ultrasonic cleaning, and the ultrasonic cleaning time is 5 minutes.

[0074] The pre-bending process is carried out as follows: the cleaned copper sheet is placed in a pre-bending mold for press bending; the curvature of the pre-bent copper sheet is R100mm.

[0075] The oxidation treatment temperature is 30°C, the oxidation treatment time is 60s, and after the oxidation treatment, the oxidized copper sheet needs to be dried. The drying treatment time is 5min and the drying treatment temperature is 80°C.

[0076] The surface area of ​​the copper oxide sheet is smaller than that of the ceramic sheet. The sintering temperature is 1065°C and the sintering time is 60 minutes. During sintering, the oxygen content in the sintering furnace is 20 ppm.

[0077] Example 2

[0078] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, wherein:

[0079] The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet; the pre-bent copper sheet is placed in a carrier, and an oxidizing liquid is added into the carrier for oxidation treatment to obtain an oxidized copper sheet; the oxidized copper sheet is placed on the surface of a ceramic sheet and co-sintered to obtain a copper-clad ceramic substrate; wherein the oxidizing liquid is a potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 4%.

[0080] The annealing treatment is carried out under a protective atmosphere of nitrogen, the annealing temperature is 450°C, and the annealing time is 80 minutes.

[0081] The cleaning treatment is carried out as follows: the annealed copper sheet is rinsed and ultrasonically cleaned in sequence; the rinsing liquid used in the rinsing treatment is a mixture of acidic degreaser, sulfuric acid and hydrogen peroxide, in which the mass ratio of acidic degreaser, sulfuric acid and hydrogen peroxide is 5.5:11:82; pure water is used for ultrasonic cleaning, and the ultrasonic cleaning time is 7 minutes.

[0082] The pre-bending process is carried out as follows: the cleaned copper sheet is placed in a pre-bending mold for press bending; the curvature of the pre-bent copper sheet is R200mm.

[0083] The oxidation treatment temperature is 40°C, the oxidation treatment time is 40s, and after the oxidation treatment, the oxidized copper sheet needs to be dried. The drying treatment time is 8min and the drying treatment temperature is 75°C.

[0084] The surface area of ​​the copper oxide sheet is smaller than that of the ceramic sheet. The sintering temperature is 1070°C and the sintering time is 45 minutes. During sintering, the oxygen content in the sintering furnace is 35 ppm.

[0085] Example 3

[0086] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, wherein:

[0087] The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet; the pre-bent copper sheet is placed in a carrier, and an oxidizing liquid is added into the carrier for oxidation treatment to obtain an oxidized copper sheet; the oxidized copper sheet is placed on the surface of a ceramic sheet and co-sintered to obtain a copper-clad ceramic substrate; wherein the oxidizing liquid is a potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 5%.

[0088] The annealing treatment is carried out under a protective atmosphere of argon, the annealing temperature is 400° C., and the annealing time is 120 min.

[0089] The cleaning treatment is carried out as follows: the annealed copper sheet is rinsed and ultrasonically cleaned in sequence; the rinsing liquid used in the rinsing treatment is a mixture of acidic degreaser, sulfuric acid and hydrogen peroxide, in which the mass ratio of the acidic degreaser, sulfuric acid and hydrogen peroxide is 6:12:82; pure water is used for ultrasonic cleaning, and the ultrasonic cleaning time is 10 minutes.

[0090] The pre-bending process is carried out as follows: the cleaned copper sheet is placed in a pre-bending mold for press bending; the curvature of the pre-bent copper sheet is R300mm.

[0091] The oxidation treatment temperature is 50°C, the oxidation treatment time is 20s, and after the oxidation treatment, the oxidized copper sheet needs to be dried. The drying treatment time is 10min and the drying treatment temperature is 70°C.

[0092] The surface area of ​​the copper oxide sheet is smaller than that of the ceramic sheet. The sintering temperature is 1080°C and the sintering time is 30 minutes. During sintering, the oxygen content in the sintering furnace is 50 ppm.

[0093] Example 4

[0094] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the annealing temperature is 380° C., and other parameters and test conditions are the same as those in Example 1.

[0095] Example 5

[0096] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Embodiment 1 in that the annealing temperature is 550° C., and other parameters and test conditions are the same as those in Embodiment 1.

[0097] Example 6

[0098] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the annealing time is 55 minutes, and the other parameters and test conditions are the same as those in Example 1.

[0099] Example 7

[0100] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the annealing time is 125 minutes, and the other parameters and test conditions are the same as those in Example 1.

[0101] Example 8

[0102] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the mass ratio of the acidic degreaser, sulfuric acid and hydrogen peroxide is 1:3:80, and the other parameters and experimental conditions are the same as those in Example 1.

[0103] Example 9

[0104] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the mass ratio of the acidic degreaser, sulfuric acid and hydrogen peroxide is 2:1.5:90, and the other parameters and experimental conditions are the same as those in Example 1.

[0105] Example 10

[0106] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the curvature of the pre-bent copper sheet is R95 mm, and other parameters and test conditions are the same as those in Example 1.

[0107] Embodiment 11

[0108] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the curvature of the pre-bent copper sheet is R310 mm, and other parameters and test conditions are the same as those in Example 1.

[0109] Example 12

[0110] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the oxidation treatment temperature is 28° C., and other parameters and test conditions are the same as those in Example 1.

[0111] Example 13

[0112] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the oxidation treatment temperature is 53° C., and other parameters and test conditions are the same as those in Example 1.

[0113] Embodiment 14

[0114] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the sintering temperature is 1050° C., and the other parameters and test conditions are the same as those in Example 1.

[0115] Embodiment 15

[0116] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the sintering temperature is 1090° C., and other parameters and test conditions are the same as those in Example 1.

[0117] Example 16

[0118] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the oxygen content in the sintering furnace is 15 ppm, and other parameters and test conditions are the same as those in Example 1.

[0119] Embodiment 17

[0120] This embodiment provides a method for preparing a wet-oxidized copper-clad ceramic substrate, which is different from Example 1 in that the oxygen content in the sintering furnace is 60 ppm, and other parameters and test conditions are the same as those in Example 1.

[0121] Comparative Example 1

[0122] This comparative example provides a method for preparing a copper-clad ceramic substrate, which is different from Example 1 in that no oxidation liquid is used for oxidation, and other parameters and test conditions are the same as those in Example 1.

[0123] The copper-clad ceramic substrates in the above embodiments and comparative examples were subjected to grain tests, and the results are shown in Table 1 below.

[0124] Table 1 Test results of copper-clad ceramic substrates in the examples and comparative examples

[0125] Grain test results (unit: piece) Example 1 120.3 Example 2 121.4 Example 3 123.1 Example 4 118.6 Example 5 115.3 Example 6 118.3 Example 7 119.4 Example 8 116.2 Example 9 117.9 Example 10 114.2 Embodiment 11 113.8 Example 12 118.5 Example 13 119.6 Embodiment 14 111.5 Embodiment 15 112.4 Example 16 115.2 Embodiment 17 119.8 Comparative Example 1 70.2

[0126] From Table 1 above, we know that:

[0127] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 4 and 5. This is because the present invention limits the annealing temperature to 400-500° C., which makes the grain detection of the copper-clad ceramic substrate optimal.

[0128] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 6 and 7. This is because the present invention limits the annealing time to 60 to 120 minutes, which makes the grain detection of the copper-clad ceramic substrate optimal.

[0129] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 8 and 9. This is because the present invention limits the mass ratio of the acidic degreaser, sulfuric acid and hydrogen peroxide to (5-6):(10-12):(80-85), which makes the grain detection of the copper-clad ceramic substrate optimal.

[0130] The test data of the copper-clad ceramic substrate of Examples 1-3 are different from the test data of the copper-clad ceramic substrate of Examples 10 and 11. This is because the present invention limits the curvature of the pre-bent copper sheet to R100-R300 mm, which makes the grain detection of the copper-clad ceramic substrate optimal.

[0131] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 12 and 13. This is because the temperature of the oxidation treatment is limited to 30-50° C. in the present invention, so that the grain detection of the copper-clad ceramic substrate is optimal.

[0132] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 14 and 15. This is because the present invention limits the sintering temperature to 1065-1080° C., which makes the grain detection of the copper-clad ceramic substrate optimal.

[0133] The test data of the copper-clad ceramic substrates of Examples 1-3 are better than the test data of the copper-clad ceramic substrates of Examples 16 and 17. This is because the present invention limits the oxygen content in the sintering furnace to 20-50 ppm, which makes the grain detection of the copper-clad ceramic substrate optimal.

[0134] The test data of the copper-clad ceramic substrate of Examples 1-3 are better than the test data of the copper-clad ceramic substrate of Comparative Example 1. This is because the present invention uses an oxidizing liquid to oxidize the copper sheet, which can improve the surface of the copper-clad substrate, increase the product yield, and reduce production costs compared to dry oxidation.

[0135] In summary, the present invention, through the specific design of the preparation method of the copper-clad ceramic substrate, adopts the wet oxidation copper sheet method to lay the foundation for the subsequent preparation of the copper-clad ceramic substrate, improve the surface of the copper substrate as a whole, improve the product sintering yield, reduce the production cost, and can meet the requirements of different grains and roughness.

[0136] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

[0137] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a wet-oxidized copper-clad ceramic substrate, characterized in that: The preparation method comprises: The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet; Placing the pre-bent copper sheet in a carrier, adding an oxidizing liquid into the carrier for oxidation treatment, and obtaining an oxidized copper sheet; Placing the copper oxide sheet on the surface of the ceramic sheet for sintering to obtain a copper-clad ceramic substrate; Wherein, the oxidizing liquid is potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 3-5%.

2. The preparation method according to claim 1, characterized in that: The annealing treatment is carried out under vacuum or protective atmosphere; Preferably, the protective atmosphere is any one of nitrogen, helium or argon, or a combination of at least two of them.

3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the annealing treatment is 400-500°C; Preferably, the annealing treatment time is 60 to 120 minutes.

4. The preparation method according to any one of claims 1 to 3, characterized in that The cleaning process is carried out as follows: The annealed copper sheet is rinsed and ultrasonically cleaned in sequence.

5. The preparation method according to claim 4, characterized in that: The flushing liquid used in the flushing treatment is a mixture of acidic degreasing agent, sulfuric acid and hydrogen peroxide; Preferably, in the mixed liquid, the mass ratio of the acidic degreasing agent, the sulfuric acid and the hydrogen peroxide is (5-6):(10-12):(80-85).

6. The preparation method according to claim 4 or 5, characterized in that: The ultrasonic cleaning adopts pure water; Preferably, the ultrasonic cleaning time is 5 to 10 minutes.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The pre-bending process is performed as follows: The cleaned copper sheet is placed in a pre-bending mold for bending; Preferably, the curvature of the pre-bent copper sheet is R100-R300 mm.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The temperature of the oxidation treatment is 30 to 50°C; Preferably, the oxidation treatment time is 20 to 60 seconds; Preferably, after the oxidation treatment, the copper oxide sheet needs to be dried.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The surface area of ​​the copper oxide sheet is smaller than the surface area of ​​the ceramic sheet; Preferably, the sintering temperature is 1065-1080°C; Preferably, the sintering time is 30 to 60 minutes; Preferably, during sintering, the oxygen content in the sintering furnace is lower than 50 ppm.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method specifically comprises: The copper sheet is subjected to annealing treatment, cleaning treatment and pre-bending treatment in sequence to obtain a pre-bent copper sheet; Placing the pre-bent copper sheet in a carrier, adding an oxidizing liquid into the carrier for oxidation treatment, and obtaining an oxidized copper sheet; Placing the copper oxide sheet on the surface of the ceramic sheet and co-sintering to obtain a copper-clad ceramic substrate; Wherein, the oxidizing liquid is potassium permanganate oxidizing liquid, and the concentration of the potassium permanganate oxidizing liquid is 3-5%; The annealing treatment is carried out in vacuum or in a protective atmosphere, wherein the protective atmosphere is any one of nitrogen, helium or argon or a combination of at least two thereof; The annealing temperature is 400-500°C, and the annealing time is 60-120 minutes; The cleaning process is carried out in the following manner: the annealed copper sheet is sequentially rinsed and ultrasonically cleaned; The rinsing liquid used in the rinsing treatment is a mixture of an acidic degreasing agent, sulfuric acid and hydrogen peroxide. In the mixture, the mass ratio of the acidic degreasing agent, the sulfuric acid and the hydrogen peroxide is (5-6):(10-12):(80-85); The ultrasonic cleaning uses pure water, and the ultrasonic cleaning time is 5 to 10 minutes; The pre-bending process is performed as follows: the cleaned copper sheet is placed in a pre-bending mold for press bending; The curvature of the pre-bent copper sheet is R100-R300mm; The temperature of the oxidation treatment is 30 to 50° C., and the time of the oxidation treatment is 20 to 60 seconds; After the oxidation treatment, the copper oxide sheet needs to be dried for 5 to 10 minutes at a temperature of 70 to 80° C. The surface area of ​​the copper oxide sheet is smaller than that of the ceramic sheet. The sintering temperature is 1065-1080° C., the sintering time is 30-60 minutes, and during sintering, the oxygen content in the sintering furnace is lower than 50 ppm.

Citation Information

Patent Citations

  • Ceramic copper-clad plate and preparation method thereof

    CN112533388A

  • Method for increasing copper thickness of DCB

    CN116001387A

  • Method for solving large bubbles of chemical copper oxide sheet sintered copper-clad ceramic substrate

    CN116037746A