Macromolecular silane coupling agent for polyether-ether-ketone composite material as well as preparation method and application of macromolecular silane coupling agent

By designing the polymer skeleton and flexible winding characteristics of the macromolecular silane coupling agent and the polyether ether ketone resin, the problem of weak interaction of the small molecule coupling agent is solved, and the mechanical properties and thermal stability of the composite material are improved. Suitable for high temperature processing.

CN118755079APending Publication Date: 2024-10-11UNIV OF JINAN +1

Patent Information

Application Number
CN202411241169.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing small molecule silane coupling agents have weak interactions with polyether ether ketone resins, resulting in unsatisfactory reinforcement effects of composite materials, and traditional coupling agents fail at high processing temperatures.

Method used

Design and synthesize a macromolecular silane coupling agent with polyether ether ketone polymer skeleton and flexible winding characteristics. By controlling its structure, the physical and mechanical properties and processing performance can be improved, and specific raw materials and catalysts can be used for reaction preparation under anhydrous conditions.

Benefits of technology

The macromolecular silane coupling agent has excellent thermal stability and solubility properties. The 5% thermal weight loss temperature is higher than 400°C. It performs well at the processing temperature of polyetheretherketone composite materials and significantly improves the mechanical properties of the composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755079A_ABST
    Figure CN118755079A_ABST
Patent Text Reader

Abstract

The invention discloses a macromolecular silane coupling agent for a polyether-ether-ketone composite material and a preparation method and application of the macromolecular silane coupling agent, and belongs to the technical field of high polymer materials.The preparation method comprises the steps that a bisphenol hydroxyl group-containing compound and a difluoro-containing ketone compound are mixed and react under the anhydrous and anaerobic conditions, a reaction product is added into methyl alcohol, precipitates are separated out, and the macromolecular silane coupling agent for the polyether-ether-ketone composite material is obtained; washing and drying the separated precipitate, mixing the precipitate with a silane coupling agent with an isocyanate group as a terminal group, and adding the mixture into tetrahydrofuran for reaction and end capping to prepare the macromolecular silane coupling agent. The organic chain segment of the macromolecular silane coupling agent is relatively long and can be mutually diffused and entangled with the macromolecular chain of a matrix polymer to form effective interface bonding, and a flexible interface layer can be introduced between two phases, so that the interface bonding force between the two phases is enhanced, and the deformation capacity of the interface under the stress effect is also improved; therefore, the strength, modulus and toughness of the composite material can be simultaneously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a macromolecular silane coupling agent for polyetheretherketone composite materials and a preparation method and application thereof. Background Art

[0002] It is well known that polymer composites can be made by introducing inorganic fillers into the polymer matrix. Usually, the fillers are treated with coupling agents to improve the adhesion and dispersion of the interface. The effect of the coupling agent treatment on the properties of the synthesized composites is often significant, and the composites prepared with coupling agents show better performance in many aspects such as mechanical properties, thermal conductivity, and crystallization properties. However, the main disadvantage of traditional coupling agents is that their application temperature cannot meet the high melting processing temperature of polyetheretherketone (PEEK) polymers. In this case, grafting polymer oligomers similar to the high processing temperature polymer matrix onto the surface of inorganic particles may be a feasible method to improve the interfacial adhesion between fillers and polymer matrices, such as PEEK through chain entanglement or through chemical bonding. From the perspective of interface enhancement mechanism, improving the compatibility of reinforcement materials and matrix is ​​the key to solving the interface problems of composites.

[0003] At present, the coupling agents used in polyetheretherketone composite materials are mainly small molecule silane coupling agents. Although a certain reinforcement effect can be achieved after modifying the surface of the reinforcement material, due to compatibility issues, the interaction efficiency between the fiber and the matrix resin is low, so the reinforcement effect is also very limited. Compared with small molecule coupling agents, macromolecular coupling agents have relatively long molecular chains. When used to modify polyetheretherketone-based composite materials, they can produce stronger physical entanglement with the polymer matrix to achieve effective reinforcement; and the structure and composition of the synthesized macromolecular coupling agents can be changed by design to control and improve the performance of the material.

[0004] Therefore, providing a macromolecular silane coupling agent and a preparation method thereof that can improve the physical and mechanical properties and processing properties by controlling the structure of the macromolecular coupling agent is a technical problem that those skilled in the art need to solve urgently. Summary of the invention

[0005] In view of this, the present invention is based on the actual needs and future development of polyetheretherketone composite materials to solve the problem that the existing small molecule silane coupling agent has weak interaction with PEEK resin and the reinforcement effect of the composite material is not ideal. Based on molecular design, a macromolecular silane coupling agent with a polyetheretherketone polymer skeleton and flexible winding characteristics is synthesized and used to modify fibers to prepare polyetheretherketone-based composite materials. The present invention achieves the improvement of its physical and mechanical properties and processing performance by controlling the structure of the macromolecular coupling agent.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A macromolecular silane coupling agent for a polyetheretherketone composite material, wherein the macromolecular silane coupling agent is any one of the following general formulas (I) to (III):

[0008]

[0009] (I);

[0010]

[0011] (II);

[0012]

[0013] (III);

[0014] In general formula (I) to general formula (III), 3≤n≤20, X is a C1-C18 linear or branched saturated alkyl group, or a branched or branched alkane with a heteroatom; Y is a C1-C18 linear or branched saturated alkyl group.

[0015] The present invention also provides a method for preparing the above-mentioned macromolecular silane coupling agent, comprising the following steps:

[0016] Adding raw material A and raw material B to an organic solvent under anhydrous and oxygen-free conditions for mixed reaction, adding the reaction product to methanol to precipitate a precipitate, washing and drying the precipitate, mixing it with raw material C, adding it to tetrahydrofuran for reaction and end-capping to prepare a macromolecular silane coupling agent;

[0017] The raw material A is a compound containing bisphenol hydroxyl group, the raw material B is a ketone compound containing difluoride, and C is a silane coupling agent with an isocyanate terminal group.

[0018] Furthermore, the compound containing bisphenol hydroxyl groups is any one of resorcinol, 2-methylhydroquinone and 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl.

[0019] Furthermore, the difluoro-containing ketone compound is 4,4'-difluorobenzophenone.

[0020] Preferably, the molar ratio of the compound containing bisphenol hydroxyl group to the difluoro ketone compound is 1:1.1-1.5.

[0021] Furthermore, the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.

[0022] Furthermore, the reaction temperature of the raw material A and the raw material B is 60-220° C., and the reaction time is 5-8 hours.

[0023] Furthermore, the reaction temperature of the precipitated precipitate and the raw material C is 60-220° C., and the reaction time is 2-5 h.

[0024] Furthermore, the reaction of raw material A and raw material B also includes removing water and adding a catalyst;

[0025] The dehydration is azeotropic dehydration with toluene, and the catalyst is potassium carbonate.

[0026] Furthermore, the reaction of the precipitated precipitate with the raw material C further comprises adding a catalyst;

[0027] The catalyst is dibutyltin dilaurate.

[0028] Preferably, the preparation steps of the macromolecular silane coupling agent are:

[0029] (1) Under room temperature, a compound containing bisphenol hydroxyl groups was added into a four-necked flask equipped with a Dean-Stark apparatus, a condenser, and a nitrogen inlet and outlet, with N-methylpyrrolidone as solvent and anhydrous potassium carbonate as catalyst; the reaction mixture was refluxed at high temperature for 4 h with toluene as an azeotropic agent to dehydrate the system;

[0030] (2) After dehydration and removal of toluene, the temperature was lowered and a difluoroketone compound was added to the flask to increase the reaction temperature. The reaction was heated for 6 h. The reaction product was cooled to room temperature and then poured into anhydrous methanol to form a precipitate. The solid was collected by centrifugation and dried in a vacuum oven at 120 °C for 24 h to obtain a hydroxyl-terminated polyetheretherketone oligomer.

[0031] (3) Add the hydroxyl-terminated polyetheretherketone oligomer into a four-necked flask, add dry tetrahydrofuran as a solvent, add the catalyst dibutyltin dilaurate (DBTDL), and add the silane coupling agent with an isocyanate terminal group dropwise through a separatory funnel under a nitrogen atmosphere. After the addition is completed, continue heating and reacting for 4 hours with continuous stirring. After the reaction is completed, cool to room temperature, precipitate with anhydrous ethanol, centrifuge the precipitate, wash with anhydrous ethanol, and dry in a vacuum drying oven to obtain a macromolecular silane coupling agent.

[0032] The beneficial effects of the present invention are:

[0033] The macromolecular silane coupling agent prepared by the present invention has excellent thermal stability, and the test results show that the 5% thermal weight loss temperature of the macromolecular silane coupling agent of the present invention is higher than 400° C. Since the processing temperature of the PEEK composite material generally does not exceed 380° C., the macromolecular silane coupling agent of the present invention has good thermal stability at the processing temperature of the PEEK composite material.

[0034] The macromolecular silane coupling agent of the present invention has excellent solubility, and is easily soluble in the polar solvent N-methylpyrrolidone, and also has good solubility in the organic solvents dimethyl sulfoxide, toluene and tetrahydrofuran, and secondly has certain solubility in the organic solvents N,N-dimethylformamide and chloroform. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Infrared spectra of R-DFBP-KH901, MeHQ-DFBP-KH901 and TMDHB-DFBP-KH901 prepared in the examples of the present invention;

[0036] Figure 2 H NMR spectra of R-DFBP-KH901, MeHQ-DFBP-KH901 and TMDHB-DFBP-KH901 prepared in the examples of the present invention;

[0037] Figure 3 XPS structural characterization diagrams of R-DFBP-KH901, MeHQ-DFBP-KH901, and TMDHB-DFBP-KH901 prepared in the embodiments of the present invention; wherein (a) is R-DFBP-KH901, (b) is MeHQ-DFBP-KH901, and (c) is TMDHB-DFBP-KH901;

[0038] Figure 4 TG and DTG graphs of R-DFBP-KH901, MeHQ-DFBP-KH901, and TMDHB-DFBP-KH901 prepared in the examples of the present invention; wherein (a) is R-DFBP-KH901, (b) is MeHQ-DFBP-KH901, and (c) is TMDHB-DFBP-KH901;

[0039] Figure 5 The mechanical properties of 3mm carbon fiber reinforced polyetheretherketone composite materials treated with different coupling agents prepared in the embodiments of the present invention. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] A macromolecular silane coupling agent (R-DFBP-KH901) for polyetheretherketone composite materials has the following structural formula:

[0043] , where n=10.

[0044] The specific preparation steps are:

[0045] 12.10 g (0.11 mol) of resorcinol and 16.56 g (0.11 mol) of anhydrous potassium carbonate were added to a four-necked flask equipped with a Dean-Stark apparatus, a condenser, and a nitrogen inlet. 30 ml of NMP was used as a solvent and 25 ml of toluene was used as an azeotropic agent. The mixture was refluxed at 140°C for 4 h, then the temperature was reduced to 100°C, 21.82 g (0.10 mol) of 4,4'-difluorobenzophenone was added to the flask to raise the reaction temperature to 170°C, and maintained at this temperature for another 6 h. The reaction mixture was cooled to room temperature. The resulting mixture was then poured into anhydrous methanol to form a precipitate, and the solid was collected by centrifugal filtration and dried in a vacuum oven at 120°C for 24 h to obtain a reddish-brown solid, which was recorded as R-DFBP.

[0046] R-DFBP (0.485 mmol) was added to a four-necked flask, and then 30 ml of dry tetrahydrofuran was added as a solvent, and a catalyst dibutyltin dilaurate (DBTDL) (0.5% of the reactant mass) was added. Under a nitrogen atmosphere, 3-isocyanate propyltrimethoxysilane (KH901) (0.3 g, 1.456 mmol) was added dropwise through a separatory funnel at a ratio of 1 / 1.5 to the functional group. After the addition was completed, the reaction was continued at 70°C for 4 hours with continuous stirring. After the reaction was completed, it was cooled to room temperature, precipitated with anhydrous ethanol, centrifuged, washed with anhydrous ethanol, dried in a vacuum drying oven, sealed and stored, and the product was labeled R-DFBP-KH901.

[0047] Example 2

[0048] A macromolecular silane coupling agent (MeHQ-DFBP-KH901) for polyetheretherketone composite materials has the following structural formula:

[0049] , where n=10.

[0050] The specific preparation steps are:

[0051] 13.64 g (0.11 mol) of MeHQ and 16.56 g (0.11 mol) of anhydrous potassium carbonate were added to a four-necked flask equipped with a Dean-Stark apparatus, a condenser, and a nitrogen inlet and outlet. 30 ml of NMP was used as a solvent and 25 ml of toluene was used as an azeotropic agent. The mixture was refluxed at 160°C for 4 h to dehydrate the system. After dehydration and removal of toluene, the temperature was lowered to 100°C, and 21.82 g (0.10 mol) of DFBP was added to the flask to raise the reaction temperature to 200°C and maintained for 3 h. The reaction mixture was cooled to room temperature. The resulting mixture was then poured into anhydrous methanol to form a precipitate, which was collected by filtration. The product was a tan solid and was recorded as MeHQ-DFBP.

[0052] The synthesized MeHQ-DFBP (0.485 mmol) was added to a four-necked flask, 30 ml of dry tetrahydrofuran was added as a solvent, and the catalyst dibutyltin dilaurate (DBTDL) (0.5% of the reactant mass) was added. Under a nitrogen atmosphere, 3-isocyanate propyltrimethoxysilane (KH901) (0.3 g, 1.456 mmol) was added dropwise through a separatory funnel at a ratio of 1 / 1.5 to the functional group. After the addition was completed, the reaction was continued at 70°C for 4 hours with continuous stirring. After the reaction was completed, it was cooled to room temperature, precipitated with anhydrous ethanol, centrifuged, washed with anhydrous ethanol, dried in a vacuum drying oven, and sealed for storage. The product was recorded as MeHQ-DFBP-KH901.

[0053] Example 3

[0054] A macromolecular silane coupling agent (TMDHB-DFBP-KH901) for polyetheretherketone composite materials has the following structural formula:

[0055] Where n=10.

[0056] The specific preparation steps are:

[0057] 26.62 g (0.11 mol) of 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl (excess) and 16.56 g (0.12 mol) of anhydrous potassium carbonate were added to a four-necked flask equipped with a Dean-Stark apparatus, a condenser, and a nitrogen inlet and outlet. 30 ml of NMP was used as a solvent and 25 ml of toluene was used as an azeotropic agent. The mixture was refluxed at 160°C for 4 h to dehydrate the system. After dehydration and removal of toluene, the temperature was reduced to 100°C, and 21.82 g (0.10 mol) of DFBP was added to the flask to increase the reaction temperature to 220°C and maintained for 6 h. The reaction mixture was cooled to room temperature. The resulting mixture was then poured into anhydrous methanol to form a precipitate, which was collected by filtration. The product was an amorphous brown solid, recorded as TMDHB-DFBP.

[0058] The synthesized TMDHB-DFBP (0.485 mmol) was added to a four-necked flask, 30 ml of dry tetrahydrofuran was added as a solvent, and the catalyst dibutyltin dilaurate (DBTDL) (0.5% of the reactant mass) was added. Under a nitrogen atmosphere, 3-isocyanate propyltrimethoxysilane (KH901) (0.3 g, 1.456 mmol) was added dropwise through a separatory funnel at a ratio of 1 / 1.5 to the functional group. After the addition was completed, the reaction was carried out at a temperature of 70°C for 4 hours with continuous stirring. After the reaction was completed, it was cooled to room temperature, precipitated with anhydrous ethanol, centrifuged, washed with anhydrous ethanol, dried in a vacuum drying oven, sealed and stored, and the products were marked as TMDHB-DFBP-KH901.

[0059] Test Example 1

[0060] The products of Examples 1-3: R-DFBP-KH901, MeHQ-DFBP-KH901 and TMDHB-DFBP-KH901 were subjected to infrared comparative characterization:

[0061] like Figure 1 As shown, the spectrum shows the stretching vibration peak of O-H, the symmetric stretching vibration peak of the ether bond, the stretching vibration peak and bending vibration peak of the C-CO bond. There are peaks of the carbonyl group in the newly generated carbamate and the peaks of the newly added Si-O bond.

[0062] The nuclear magnetic resonance characterization:

[0063] like Figure 2 As shown, the characteristic peak of methyl hydrogen appears at (near 3.6 ppm) a, and the characteristic peaks of three methylene hydrogen appear at (near 0.7 ppm) b, (near 1.7 ppm) c, and (near 3.8 ppm) d.

[0064] XPS characterization:

[0065] like Figure 3 As shown, the results show four typical peaks near 284 eV (C 1s), 532 eV (O 1s), 399 eV (N 1s), and 101 eV (Si2p).

[0066] The thermal stability performance was characterized:

[0067] like Figure 4 As shown, from Figure 4 It can be seen that the 5% thermal weight loss of the three products is higher than 400°C, indicating that the macromolecular coupling agent synthesized by the present invention will not decompose and fail when used at the processing temperature.

[0068] Therefore, the different macromolecular silane coupling agents synthesized by the present invention all have good thermal stability at the processing temperature of the PEEK composite material.

[0069] Test Example 2 Dissolution Performance:

[0070] The products prepared in Examples 1-3 were dissolved in different solvents, and the remaining solid content and solution color were observed after 5 minutes. The results are shown in Table 1 below.

[0071] Table 1 Solubility of macromolecular silane coupling agents in different solvents

[0072] name NMP DMF DMSO <![CDATA[CDCl3]]> Toluene THF Methanol Ethanol R-DFBP-KH901 ++ + ++ + ++ ++ — — MeHQ-DFBP-KH901 ++ + ++ + ++ ++ — — TMDHB-DFBP-KH901 ++ + ++ ++ ++ ++ — —

[0073] Note: ++: easily soluble (soluble at room temperature); +: soluble (needs heating to dissolve); -: insoluble

[0074] The solubility of the macromolecular silane coupling agent prepared by the present invention is that it is easily soluble in the polar solvent NMP, and it also has good solubility in the organic solvents DMSO, toluene and tetrahydrofuran. Secondly, it is soluble in the organic solvents DMF and chloroform, but the dissolution rate is slow and needs to be heated to dissolve, but it is not soluble in reagents such as methanol and ethanol.

[0075] Test Example 3

[0076] Commercially available coupling agents KH901 (3-isocyanatepropyltrimethoxysilane), R-DFBP-KH901, MeHQ-DFBP-KH901, and TMDHB-DFBP-KH901 were prepared into 2% coupling agent hydrolyzate. Carbon fibers were treated with the silane coupling agent hydrolyzate. The treated carbon fibers were prepared into polyetheretherketone composites by extrusion granulation and high-temperature compression molding, and the performance of the composites was tested.

[0077] The specific operation method is:

[0078] (1) Weigh the reinforcing materials carbon fiber 10%, macromolecular silane coupling agent 2%, and polyetheretherketone 88% by mass.

[0079] (2) Clean the surface of the carbon fiber, soak the carbon fiber in anhydrous ethanol solution for 24 hours, ultrasonically treat it for 30 minutes, and vacuum dry it. Then treat the dried carbon fiber with nitric acid in a 60°C water bath; after treatment, wash it with distilled water until it is neutral, and dry it in a vacuum drying oven at 60°C.

[0080] (3) Add the treated carbon fiber to the NMP solution of the macromolecular silane coupling agent, then slowly add 2% water, heat the mixture to 80°C with stirring, and react for 12 hours. Collect the fibers by filtration, wash with cold NMP, and dry in a vacuum oven at 120°C for 48 hours.

[0081] (4) Turn on the power of the extruder and connect the cooling water. First, add the dried polyetheretherketone matrix into the barrel and run the machine. Then, add the corresponding treated carbon fiber from the side forced feeding port at the fourth section of the extruder. After the polyetheretherketone is melted in the first two sections of the extruder, it is evenly mixed with the fibers added from the side when it reaches the fourth section under the action of the twin screw. The fibers are distributed in the molten polyetheretherketone and are driven to the end of the extrusion by the screw. The temperature of each section of the twin-screw extruder was controlled at 360°C, 380°C, 380°C, 380°C, 370°C, 365°C, 360°C, and 360°C, and the extrusion temperature was 360°C to obtain fiber-reinforced PEEK composite filament strips. After extrusion, the strips were transported by a conveyor belt and entered into a water-cooled, and after cooling, they were pulled into a roller cutter pelletizer to obtain cylindrical particles with a diameter of 2-4 mm and a length of 4-6 mm, i.e., carbon fiber reinforced polyetheretherketone composite pellets with a fiber mass percentage of 10% were obtained.

[0082] (5) The carbon fiber reinforced polyetheretherketone composite pellets prepared above were dried at 150 °C for 3 h to remove moisture. A high-temperature release agent was sprayed in the mold, and the release agent was evenly applied to all corners of the mold with a wire brush to facilitate smooth demolding after molding. 10 g and 5 g of the dried pellets were respectively placed in the dumbbell mold and the long strip mold of the high-temperature molding machine, and pre-pressed for 30 s to squeeze out some of the air remaining in the mold before the mold was heated. The mold temperature was set to 380 °C, and then the mold began to heat. When the pellets were melted and plasticized, the following pressurization and depressurization methods were used: the pressure was increased to 25 T and maintained for 1 min, and then the pressure was released; the pressure was increased to 25 T and maintained for 1 min, and then the pressure was released; finally, the pressure was increased to 25 T again and maintained for 30 min. Some splashing occurred during this period, which is normal. After 30 minutes of heat preservation and pressure holding, the molded product will be cooled at a rate of 40℃ / h and continue to maintain pressure. When the system temperature drops below 300℃, the pressure will be reduced until the product temperature is below 150℃ for demolding. After cooling to room temperature, the edges and corners of the spline will be further polished and corrected with a file.

[0083] like Figure 5 As shown in the figure, the tensile and flexural strengths after treatment with KH901 are 114.7MPa and 155.9MPa, the tensile and flexural strengths after treatment with R-DFBP-KH901 macromolecular silane coupling agent are 128.5MPa and 166.3MPa, the tensile and flexural strengths after treatment with MeHQ-DFBP-KH901 macromolecular silane coupling agent are 131.2MPa and 170.1MPa, and the tensile and flexural strengths after treatment with TMDHB-DFBP-KH901 macromolecular silane coupling agent are 128.8MPa and 161.7MPa. Compared with small molecule silane coupling agents, macromolecular silane coupling agents have a greater improvement in the mechanical properties of composite materials.

[0084] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A macromolecular silane coupling agent for polyetheretherketone composite materials, characterized in that: The macromolecular silane coupling agent is any one of the following general formulas (I) to (III): ; (Ⅰ); ; (Ⅱ); ; (Ⅲ); In general formula (I) to general formula (III), 3≤n≤20, X is a C1-C18 linear or branched saturated alkyl group, or a branched or branched alkane with a heteroatom; Y is a C1-C18 linear or branched saturated alkyl group.

2. A method for preparing a macromolecular silane coupling agent for a polyetheretherketone composite material according to claim 1, characterized in that: The following steps are involved: Adding raw material A and raw material B to an organic solvent under anhydrous and oxygen-free conditions for mixed reaction, adding the reaction product to methanol to precipitate a precipitate, washing and drying the precipitate, mixing it with raw material C, adding it to tetrahydrofuran for reaction and end-capping to prepare a macromolecular silane coupling agent; The raw material A is a compound containing bisphenol hydroxyl, the raw material B is a ketone compound containing difluoride, and C is a silane coupling agent with an isocyanate terminal group; the reaction temperature of the raw material A and the raw material B is 60-220° C., and the reaction time is 5-8 hours; the reaction temperature of the precipitated precipitate and the raw material C is 60-220° C., and the reaction time is 2-5 hours; The compound containing bisphenol hydroxyl group is any one of resorcinol, 2-methylhydroquinone and 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl; The difluorinated ketone compound is 4,4'-difluorobenzophenone.

3. The method for preparing a macromolecular silane coupling agent for a polyetheretherketone composite material according to claim 2, characterized in that: The organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.

4. The method for preparing a macromolecular silane coupling agent for a polyetheretherketone composite material according to claim 2 or 3, characterized in that: The reaction of raw material A and raw material B also includes removing water and adding a catalyst; The dehydration is azeotropic dehydration with toluene, and the catalyst is potassium carbonate.

5. The method for preparing a macromolecular silane coupling agent for a polyetheretherketone composite material according to claim 2, characterized in that: The reaction of the precipitated precipitate with the raw material C further comprises adding a catalyst; The catalyst is dibutyltin dilaurate.

6. Use of the macromolecular silane coupling agent for polyetheretherketone composite materials according to claim 1 in polyetheretherketone composite materials.

Citation Information

Patent Citations

  • Cross-linkable polymer compositions

    CN109843975A

Cited By

  • Long-acting toughened polylactic acid composite material and preparation method thereof

    CN122103505A