Anti-aging and anti-yellowing acrylic plate and preparation method thereof
By combining silica and tetrabutyl titanate with polyurethane base coating, an anti-aging acrylic board is formed, which solves the problems of aging and poor heat and humidity resistance of acrylic materials, achieves high toughness and weather resistance of the material, and delays the aging process. .
Patent Information
- Application Number
- CN202410977719.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
Acrylic materials are prone to aging when exposed to the atmospheric environment for a long time, which is manifested by reduced light transmittance, increased yellow index, decreased tensile strength and impact strength. Especially when subjected to external impact or surface scratches, aging is accelerated, resulting in aging resistance, moisture and heat resistance. Poor performance and toughness.
The preparation method is used to mix ethyl orthosilicate, glacial acetic acid, ethanol and deionized water to generate silica sol, and combine tetrabutyl titanate and γ-glycidyl oxypropyltrimethoxysilane to form titanium dioxide-silica Sol, and combined with polyurethane base coating and polytrimethylene adipate to form a transparent protective coating, which avoids agglomeration through the UV shielding function of nano titanium dioxide and the silicon-oxygen-titanium bond structure, and enhances the toughness and weather resistance of the material.
It significantly improves the toughness and aging resistance of acrylic sheets, maintains the transparency and heat resistance of the material, enhances resistance to ultraviolet light, delays the aging process, and improves the applicability of the material.
Smart Images

Figure BDA0004955072660000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of acrylic plates, in particular to an anti-aging and yellowing acrylic plate and a preparation method thereof. Background Art
[0002] Acrylic is a plastic polymerized from methyl methacrylate, also known as organic glass. It has excellent optical properties, chemical corrosion resistance, electrical insulation and biocompatibility, is easy to process and shape, has a low relative density, and has greater mechanical strength than inorganic glass. It is widely used in aviation, navigation, construction, and daily life. However, acrylic materials exposed to the atmosphere for a long time will gradually deteriorate in performance due to the influence of various factors such as ultraviolet rays, temperature, and humidity in the environment. The main manifestations are lower transmittance, higher yellow index, decreased tensile strength and impact strength, and more obvious brittle characteristics. Especially when it is impacted by external forces or the surface is scratched, cracks or defects are generated, its aging process will be significantly accelerated. Therefore, it is necessary to develop acrylic with good aging resistance, good moisture and heat resistance, and good toughness to improve the applicability of acrylic materials. Summary of the invention
[0003] The object of the present invention is to provide an anti-aging and yellowing acrylic plate and a preparation method thereof, so as to solve the problems of poor aging resistance, poor moisture and heat resistance and poor toughness of acrylic materials.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A method for preparing an anti-aging and yellowing acrylic sheet, the preparation method comprising:
[0006] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed to obtain silica sol after reaction; tetrabutyl titanate, acetylacetone, and ethanol are mixed to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed, tetrabutyl titanate solution is added after reaction, and the reaction is continued to obtain titanium dioxide-silica sol;
[0007] Step 2: Mix polytetrahydrofuran and hexamethylene diisocyanate, protect with nitrogen, and obtain a prepolymer after reaction; mix the prepolymer, trimethyl phosphate, dibutyltin dilaurate, silicone defoamer, and silicone surfactant, and obtain a polyurethane base coating after reaction;
[0008] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8-9 with triethanolamine, mixing the polyurethane base coating and the titanium dioxide-silica sol, reacting at 2300-2700 rpm for 14-16 minutes, and standing for 14-16 minutes to obtain a transparent protective coating;
[0009] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed, protected with nitrogen, the vacuum degree is adjusted after the reaction, the reaction is continued, and polypropylene adipate is obtained after cooling. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed, the vacuum degree is adjusted after the reaction, the reaction is continued, and the mixture is poured into a mold for curing after cooling. After curing, the mixture is cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0010] Step 5: Clean the polymethyl methacrylate substrate with anhydrous ethanol, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate, dry at 38-42° C. for 10-14 hours, and cure at room temperature for 2-4 days to obtain an anti-aging yellowing acrylic plate.
[0011] As a limitation of the present invention, the preparation of titanium dioxide-silicon dioxide sol is specifically as follows:
[0012] Tethyl orthosilicate, glacial acetic acid, ethanol and deionized water are mixed in a mass ratio of (41-43):(0.17-0.19):(108-112):(14-16), and reacted at 45-55° C. for 8-10 hours to obtain silica sol. Tetrabutyl titanate, acetylacetone and ethanol are mixed in a mass ratio of (16-18):(5-6):(8-12) to obtain tetrabutyl titanate solution. Silica sol and γ-glycidyloxypropyltrimethoxysilane are mixed in a mass ratio of (38-42):(10-12), and reacted at 25-30° C. and 50-70 rpm for 0.5-1.5 hours. Tetrabutyl titanate solution in a mass ratio of 1:(0.5-0.7) to silica sol is added, and reacted at 45-55° C. for 3-5 hours to obtain titanium dioxide-silica sol.
[0013] As a limitation of the present invention, the preparation of the polyurethane base coating is specifically as follows:
[0014] Polytetrahydrofuran and hexamethylene diisocyanate are mixed in a mass ratio of (164-166):(186-188), and nitrogen is used as a protective gas. The mixture is reacted at 80-90°C for 4-6 hours to obtain a prepolymer. The prepolymer, trimethyl phosphate, dibutyltin dilaurate, an organosilicon defoamer, and an organosilicon surfactant are mixed in a mass ratio of (350-354):(32-34):(0.2-0.4):(1.9-2.1):(0.3-0.5), and the mixture is reacted at 60-70°C and 2300-2700rpm for 20-40 minutes to obtain a polyurethane base coating.
[0015] As a limitation of the present invention, the mass ratio of the polyurethane base coating to the titanium dioxide-silicon dioxide sol is (91-93):(7-9).
[0016] As a limitation of the present invention, the preparation of the polymethyl methacrylate substrate is specifically as follows:
[0017] Adipic acid, 1,2-propylene glycol and tetrabutyl titanate are mixed in a mass ratio of (165-168):(75-77):(0.06-0.08), nitrogen is used as a protective gas, the mixture is reacted at 200-220°C for 5-7h, the vacuum degree is adjusted to 0.096-0.098MPa, the reaction is continued for 1-3h, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate and benzoyl peroxide are mixed, the mixture is reacted at 94-98°C for 4-6h, the vacuum degree is adjusted to 0.097-0.099MPa, the reaction is continued for 1-3h, the mixture is cooled to 46-50°C, the mixture is poured into a mold, and the mixture is cured at 46-50°C for 10-14h, the mixture is cooled to room temperature, and the mold is demolded to obtain a polymethyl methacrylate substrate.
[0018] As a limitation of the present invention, the mass ratio of polypropylene adipate, methyl methacrylate and benzoyl peroxide is (10.0-10.4):(99-101):(2.3-2.5).
[0019] As a limitation of the present invention, the method of cleaning the polymethyl methacrylate substrate with anhydrous ethanol specifically comprises: immersing the polymethyl methacrylate in anhydrous ethanol, ultrasonically cleaning the polymethyl methacrylate substrate at 45-55° C. and 40-60 kHz for 10-20 minutes, taking out the polymethyl methacrylate substrate, and drying it at 70-80° C. for 5-10 minutes.
[0020] As a limitation of the present invention, when the spraying method is used, the spraying pressure is 0.3-0.5 MPa, the spraying distance is 18-22 cm, and the coating thickness is 400-600 μm.
[0021] The beneficial effects achieved by the present invention are as follows: polypropylene adipate is a flexible polyester. After forming an interpenetrating network group with polymethyl methacrylate, the linear polypropylene adipate enters between the polymethyl methacrylate macromolecular chains, interacts with the polar groups on the chains, destroys the physical crosslinking points between the polymethyl methacrylate macromolecular chains, and improves the toughness of the material. In addition, the synthesized polypropylene adipate is a transparent, liquid polymer that can be evenly dispersed in the methyl methacrylate monomer, has good compatibility, and will not significantly reduce the transparency of the material. The selected polyurethane coating is a transparent product obtained by addition polymerization of hexamethylene diisocyanate and polytetrahydrofuran, which not only has the characteristics of high strength, good wear resistance, good weather resistance, etc. of the isocyanate group, but also has the characteristics of good heat resistance, good water resistance, good toughness, etc. of the polyol, and because the isocyanate group is highly active, it is very easy to react with the hydroxyl-containing substance on the surface of the substrate, so when used as a coating material, it generally has good adhesion. Nano titanium dioxide is an excellent ultraviolet shielding agent, but it has strong polarity and large specific surface area. When directly added to polymers, agglomeration will occur, which will lose expected performance. In addition, under the influence of ultraviolet light, nano titanium dioxide will produce photocatalytic phenomenon and degrade polymer substrates. Therefore, the present invention prepares titanium dioxide-silicon dioxide composite sol, which, while retaining the ultraviolet shielding function of nano titanium dioxide, introduces silicon-oxygen-titanium bonds and silicon-oxygen network structures to avoid the agglomeration of nano titanium dioxide, and also avoids the polymer substrate from being catalytically degraded by nano titanium dioxide. DETAILED DESCRIPTION
[0022] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0023] γ-Glycidyloxypropyltrimethoxysilane (G810441) was provided by Shanghai McLean, polytetrahydrofuran (Mn~1000) was provided by Sinopharm Group, and silicone defoamer: BYK141 and silicone surfactant: BYK347 (1.02g / ml) were provided by Shanghai Buding.
[0024] Example 1: A method for preparing an anti-aging yellowing acrylic sheet, which is prepared by the following steps:
[0025] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed in a mass ratio of 42:0.18:110:15, and reacted at 50°C for 9 hours to obtain silica sol; tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 17:5.5:10 to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed in a mass ratio of 40:11, and reacted at 27°C and 60rpm for 1 hour; tetrabutyl titanate solution is added in a mass ratio of 1:0.6 to silica sol, and reacted at 50°C for 4 hours to obtain titanium dioxide-silica sol;
[0026] Step 2: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 165:187, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 352:33:0.3:2:0.4, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0027] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8 with triethanolamine, mixing the polyurethane coating and the titanium dioxide-silica sol at a mass ratio of 92:8, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0028] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 166.5:76:0.07, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10.2:100:2.4, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0029] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0030] Embodiment 2: A method for preparing an anti-aging yellowing acrylic sheet, which is prepared by the following steps:
[0031] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed in a mass ratio of 41:0.17:108:14, and reacted at 50°C for 9 hours to obtain silica sol; tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 16:5:8 to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed in a mass ratio of 38:10, and reacted at 27°C and 60rpm for 1 hour; tetrabutyl titanate solution is added in a mass ratio of 1:0.5 to silica sol, and reacted at 50°C for 4 hours to obtain titanium dioxide-silica sol;
[0032] Step 2: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 164:186, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 350:32:0.2:1.9:0.3, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0033] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8 with triethanolamine, mixing the polyurethane coating and the titanium dioxide-silica sol at a mass ratio of 91:7, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0034] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 165:75:0.06, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10:99:2.3, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0035] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0036] Embodiment 3: A method for preparing an anti-aging and yellowing acrylic sheet, which is prepared by the following steps:
[0037] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed in a mass ratio of 43:0.19:112:16, and reacted at 50°C for 9 hours to obtain silica sol; tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 18:6:12 to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed in a mass ratio of 42:12, and reacted at 27°C and 60rpm for 1 hour; tetrabutyl titanate solution is added in a mass ratio of 1:0.7 to silica sol, and reacted at 50°C for 4 hours to obtain titanium dioxide-silica sol;
[0038] Step 2: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 166:188, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 354:34:0.4:2.1:0.5, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0039] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8 with triethanolamine, mixing the polyurethane coating and the titanium dioxide-silica sol at a mass ratio of 93:9, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0040] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 168:77:0.08, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10.4:101:2.5, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0041] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0042] Based on Example 1, a control experiment was carried out, specifically Comparative Example 1 and Comparative Example 2, as described below:
[0043] Comparative Example 1: Titanium dioxide-silicon dioxide sol was not used, and other conditions were the same as those in Example 1.
[0044] A method for preparing an anti-aging and yellowing acrylic sheet is prepared by the following steps:
[0045] Step 1: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 165:187, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 352:33:0.3:2:0.4, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0046] Step 2: The polyurethane coating and deionized water were mixed in a mass ratio of 92:8, reacted at 2500 rpm for 15 minutes, and allowed to stand for 15 minutes to obtain a transparent protective coating;
[0047] Step 3: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 166.5:76:0.07, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10.2:100:2.4, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0048] Step 4: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0049] Comparative Example 2: Titanium dioxide sol was used alone, and other conditions were the same as those in Example 1.
[0050] A method for preparing an anti-aging and yellowing acrylic sheet is prepared by the following steps:
[0051] Step 1: Tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 17:5.5:10 to obtain a tetrabutyl titanate solution, deionized water and KH560 are mixed in a mass ratio of 40:11, reacted at 27°C and 60rpm for 1h, and tetrabutyl titanate solution in a mass ratio of 1:0.6 to deionized water is added, and reacted at 50°C for 4h to obtain a titanium dioxide sol;
[0052] Step 2: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 165:187, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 352:33:0.3:2:0.4, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0053] Step 3: adjusting the pH of the titanium dioxide sol to 8 with triethanolamine, mixing the polyurethane coating and the titanium dioxide sol at a mass ratio of 92:8, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0054] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 166.5:76:0.07, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10.2:100:2.4, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0055] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0056] Comparative Example 3: No polyurethane base coating was used, and other conditions were the same as those in Example 1.
[0057] A method for preparing an anti-aging and yellowing acrylic sheet is prepared by the following steps:
[0058] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed in a mass ratio of 42:0.18:110:15, and reacted at 50°C for 9 hours to obtain silica sol; tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 17:5.5:10 to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed in a mass ratio of 40:11, and reacted at 27°C and 60rpm for 1 hour; tetrabutyl titanate solution is added in a mass ratio of 1:0.6 to silica sol, and reacted at 50°C for 4 hours to obtain titanium dioxide-silica sol;
[0059] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8 with triethanolamine, mixing deionized water and the titanium dioxide-silica sol in a mass ratio of 92:8, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0060] Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed in a mass ratio of 166.5:76:0.07, nitrogen is used as a protective gas, the mixture is reacted at 210°C for 6 hours, the vacuum degree is adjusted to 0.097 MPa, the reaction is continued for 2 hours, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed in a mass ratio of 10.2:100:2.4, the mixture is reacted at 96°C for 5 hours, the vacuum degree is adjusted to 0.098 MPa, the reaction is continued for 2 hours, the mixture is cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0061] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0062] Comparative Example 4: No polypropylene adipate was added, and the remaining conditions were the same as those in Example 1.
[0063] A method for preparing an anti-aging and yellowing acrylic sheet is prepared by the following steps:
[0064] Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed in a mass ratio of 42:0.18:110:15, and reacted at 50°C for 9 hours to obtain silica sol; tetrabutyl titanate, acetylacetone, and ethanol are mixed in a mass ratio of 17:5.5:10 to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed in a mass ratio of 40:11, and reacted at 27°C and 60rpm for 1 hour; tetrabutyl titanate solution is added in a mass ratio of 1:0.6 to silica sol, and reacted at 50°C for 4 hours to obtain titanium dioxide-silica sol;
[0065] Step 2: polytetrahydrofuran and hexamethylene diisocyanate were mixed in a mass ratio of 165:187, nitrogen was used as a protective gas, and the mixture was reacted at 85° C. for 5 hours to obtain a prepolymer; the prepolymer, trimethyl phosphate, dibutyltin dilaurate, BYK141, and BYK347 were mixed in a mass ratio of 352:33:0.3:2:0.4, and the mixture was reacted at 65° C. and 2500 rpm for 30 minutes to obtain a polyurethane coating;
[0066] Step 3: adjusting the pH of the titanium dioxide-silica sol to 8 with triethanolamine, mixing the polyurethane coating and the titanium dioxide-silica sol at a mass ratio of 92:8, reacting at 2500 rpm for 15 minutes, and standing for 15 minutes to obtain a transparent protective coating;
[0067] Step 4: Methyl methacrylate and benzoyl peroxide were mixed in a mass ratio of 100:2.4, reacted at 96°C for 5 hours, adjusted the vacuum degree to 0.098 MPa, continued to react for 2 hours, cooled to 48°C, poured into a mold, cured at 48°C for 12 hours, cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate;
[0068] Step 5: immerse the polymethyl methacrylate substrate in anhydrous ethanol, perform ultrasonic cleaning at 50°C and 50kHz for 15 minutes, take out the polymethyl methacrylate substrate, dry it at 75°C for 8 minutes, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate with a pressure of 0.4MPa, a spraying distance of 20cm, a coating thickness of 500μm, dry it at 40°C for 12h, and cure it at room temperature for 3 days to obtain an anti-aging and yellowing acrylic sheet.
[0069] Detection experiment:
[0070] According to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, acrylic samples required for the experiment were prepared.
[0071] Coating hardness test: According to "Determination of film hardness by pencil method for paint and varnish" (GB / T 6739-2006), the pencil hardness determination method is used to characterize the hardness of the coating. According to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, 7 samples of 200mm×50mm×10mm are prepared, and the samples are fixed on a horizontal table. Hold the pencils of different hardness that have been sharpened in advance, starting from the hardest one, make it at a 45° angle with the coating, push forward with force at a speed of 1mm / s, and continuously scratch five marks with a width of about 3mm, observe the scratches on the coating, and find a pencil that does not scratch the coating with all five marks. The hardness of this pencil is the pencil hardness of the measured coating. The pencil hardness can be divided into 9H, 8H, 7H, 6H, 5H, 4H, 3H, 2H, H, F, HB, 2B, 3B, 4B, 5B, and 6B from large to small, among which 9H is the hardest and 6B is the softest.
[0072] Coating adhesion test: Adhesion was measured by the circle method according to the "Determination of Adhesion of Paint Films" (GB / T 1270-1979). Seven samples of 100 mm × 50 mm × 10 mm were prepared according to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4. The samples were mounted on the workbench of the testing machine and pressed with a pressing plate. The hand wheel was shaken to start the test. The integrity of the transparent PU coating within the range of the circular rolling line scratch was evaluated and divided into 7 levels, of which level 1 was the best and level 7 was the worst.
[0073] UV aging test: Tested according to "Plastic Yellow Index Test Method" (HG / T 3862-2006) and "Plastic Laboratory Light Source Exposure Test Method Part 3: Fluorescent UV Lamp" (GB / T 16422.3-2006). Prepare 7 samples of 100mm×50mm×10mm size according to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4. After measuring the yellow index of each sample, fix the sample on the fixture and irradiate the sample on one side. During the test, the temperature of the aging box is 50℃, the wavelength of the ultraviolet light is 340nm, the light power is 40W, the distance between the sample and the source is 50mm, the time is 7 days, and the yellow index of the sample is measured again after 7 days.
[0074] Damp heat aging test: Tested according to "Plastic Yellow Index Test Method" (HG / T 3862-2006). According to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, 7 samples of 100mm×50mm×10mm were prepared. After measuring the yellow index of each sample, a high / low temperature damp heat test chamber was used to perform a damp heat test on the prepared samples. The experimental process is: the temperature is raised from 30°C to 60°C within 2 hours, and the relative humidity is maintained at 95%, and maintained under this condition for 6 hours, and then cooled to 30°C within 8 hours, and the relative humidity is 95%, and maintained under this condition for 8 hours. This process is 1 cycle, and a total of 10 cycles are required. After 10 cycles, the yellow index of the sample is measured again.
[0075] Impact toughness test: The test was conducted in accordance with the "Resin Casting Impact Test Method" (GB / T 2571-1995). Specifically, a simply supported beam impact pendulum testing machine was used to test, and 7 samples of 120 mm × 15 mm × 10 mm were prepared according to the methods of Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4, respectively. The samples were fixed on the support, and the pendulum was used to impact the center of the sample. The pendulum impact speed was 2.9 m / s, and the impact strength of the sample was measured.
[0076] The results are as follows:
[0077]
[0078]
[0079] Conclusion: It can be seen from the experiment that the performance of Example 1 is better than that of Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4. Compared with Example 1, Comparative Example 1 does not use titanium dioxide-silicon dioxide sol, and the yellow index change value of the sample after ultraviolet treatment and the yellow index change value of the sample after wet heat treatment are greatly increased in the experiment, and the hardness of the coating is reduced; Comparative Example 2 uses titanium dioxide sol alone, and the yellow index change value of the sample after ultraviolet treatment and the yellow index change value of the sample after wet heat treatment are also increased in the experiment, but the increase is not as large as that of Comparative Example 1; Comparative Example 3 does not use polyurethane base coating, and the coating hardness and coating adhesion are greatly decreased in the experiment, and the yellow index change value after wet heat treatment is increased; Comparative Example 4 does not add polypropylene adipate, and does not form an interpenetrating network structure with polymethyl methacrylate, and the tensile strength is decreased. In summary, the acrylic of the present invention has good aging resistance, moisture and heat resistance, and toughness.
[0080] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A method for preparing an anti-aging and yellowing acrylic sheet, characterized in that: The preparation method is: Step 1: TEOS, glacial acetic acid, ethanol, and deionized water are mixed to obtain silica sol after reaction; tetrabutyl titanate, acetylacetone, and ethanol are mixed to obtain tetrabutyl titanate solution; silica sol and KH560 are mixed, tetrabutyl titanate solution is added after reaction, and the reaction is continued to obtain titanium dioxide-silica sol; Step 2: Mix polytetrahydrofuran and hexamethylene diisocyanate, protect with nitrogen, and obtain a prepolymer after reaction; mix the prepolymer, trimethyl phosphate, dibutyltin dilaurate, silicone defoamer, and silicone surfactant, and obtain a polyurethane base coating after reaction; Step 3: adjusting the pH of the titanium dioxide-silica sol to 8-9 with triethanolamine, mixing the polyurethane base coating and the titanium dioxide-silica sol, reacting at 2300-2700 rpm for 14-16 minutes, and standing for 14-16 minutes to obtain a transparent protective coating; Step 4: Adipic acid, 1,2-propylene glycol, and tetrabutyl titanate are mixed, protected with nitrogen, the vacuum degree is adjusted after the reaction, the reaction is continued, and polypropylene adipate is obtained after cooling. Polypropylene adipate, methyl methacrylate, and benzoyl peroxide are mixed, the vacuum degree is adjusted after the reaction, the reaction is continued, and the mixture is poured into a mold for curing after cooling. After curing, the mixture is cooled to room temperature, and demolded to obtain a polymethyl methacrylate substrate; Step 5: Clean the polymethyl methacrylate substrate with anhydrous ethanol, spray the transparent protective coating on the cleaned polymethyl methacrylate substrate, dry at 38-42° C. for 10-14 hours, and cure at room temperature for 2-4 days to obtain an anti-aging yellowing acrylic plate.
2. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 1, characterized in that: The preparation of titanium dioxide-silicon dioxide sol is specifically as follows: Tethyl orthosilicate, glacial acetic acid, ethanol and deionized water are mixed in a mass ratio of (41-43):(0.17-0.19):(108-112):(14-16), and reacted at 45-55° C. for 8-10 hours to obtain silica sol. Tetrabutyl titanate, acetylacetone and ethanol are mixed in a mass ratio of (16-18):(5-6):(8-12) to obtain tetrabutyl titanate solution. Silica sol and γ-glycidyloxypropyltrimethoxysilane are mixed in a mass ratio of (38-42):(10-12), and reacted at 25-30° C. and 50-70 rpm for 0.5-1.5 hours. Tetrabutyl titanate solution in a mass ratio of 1:(0.5-0.7) to silica sol is added, and reacted at 45-55° C. for 3-5 hours to obtain titanium dioxide-silica sol.
3. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 1, characterized in that: The preparation of polyurethane base coating is specifically as follows: Polytetrahydrofuran and hexamethylene diisocyanate are mixed in a mass ratio of (164-166): (186-188), and nitrogen is used as a protective gas. The mixture is reacted at 80-90° C. for 4-6 hours to obtain a prepolymer. The prepolymer, trimethyl phosphate, dibutyltin dilaurate, an organosilicon defoamer, and an organosilicon surfactant are mixed, and the mixture is reacted at 60-70° C. and 2300-2700 rpm for 20-40 minutes to obtain a polyurethane base coating.
4. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 1, characterized in that: The mass ratio of the polyurethane base coating to the titanium dioxide-silicon dioxide sol is (91-93):(7-9).
5. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 1, characterized in that: The preparation of the polymethyl methacrylate substrate is specifically as follows: Adipic acid, 1,2-propylene glycol and tetrabutyl titanate are mixed in a mass ratio of (165-168):(75-77):(0.06-0.08), nitrogen is used as a protective gas, the mixture is reacted at 200-220°C for 5-7h, the vacuum degree is adjusted to 0.096-0.098MPa, the reaction is continued for 1-3h, and the mixture is cooled to obtain polypropylene adipate. Polypropylene adipate, methyl methacrylate and benzoyl peroxide are mixed, the mixture is reacted at 94-98°C for 4-6h, the vacuum degree is adjusted to 0.097-0.099MPa, the reaction is continued for 1-3h, the mixture is cooled to 46-50°C, the mixture is poured into a mold, and the mixture is cured at 46-50°C for 10-14h, the mixture is cooled to room temperature, and the mold is demolded to obtain a polymethyl methacrylate substrate.
6. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 5, characterized in that: The mass ratio of polypropylene adipate, methyl methacrylate and benzoyl peroxide is (10.0-10.4):(99-101):(2.3-2.5).
7. The method for preparing an anti-aging and yellowing acrylic sheet according to claim 1, characterized in that: The specific steps for cleaning the polymethyl methacrylate substrate with anhydrous ethanol are as follows: The polymethyl methacrylate substrate is immersed in anhydrous ethanol, and ultrasonically cleaned at 45-55° C. and 40-60 kHz for 10-20 minutes. The polymethyl methacrylate substrate is taken out and dried at 70-80° C. for 5-10 minutes.